A regenerable adsorbent for hydrogen sulfide removal and preparation method thereof

By optimizing the mesoporous channel structure of the composite carrier of activated alumina and ZSM-5 molecular sieve and the combination of alkaline metal salts, the problems of high temperature dependence and complicated preparation of hydrogen sulfide adsorbents in the existing technology have been solved, and efficient and economical vulcanization has been achieved. Hydrogen removal effect and long life adsorbent.

CN114146682BActive Publication Date: 2024-10-01SHANGHAI LVQIANG NEW MATERIALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111503433.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-10
Publication Date
2024-10-01
Estimated Expiration
2041-12-10

AI Technical Summary

Technical Problem

Existing renewable hydrogen sulfide adsorbents are used at high temperatures and have cumbersome preparation processes, resulting in high manufacturing costs and limited adsorption effects.

Method used

A composite carrier of activated alumina and ZSM-5 molecular sieve is used to optimize the mesoporous channel structure to form mesoporous channels of 2 to 20nm and 20 to 50nm, combined with alkaline metal salts as active components to improve the activity and use of the adsorbent. life.

Benefits of technology

It improves the utilization rate of the active components of the adsorbent, extends the single use time, reduces the regeneration frequency, achieves efficient hydrogen sulfide removal accuracy, and the process is economical, environmentally friendly, and suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114146682B_ABST
    Figure CN114146682B_ABST
Patent Text Reader

Abstract

The present invention relates to a regenerable adsorbent for removing hydrogen sulfide and a preparation method thereof, wherein the adsorbent is composed of an active component and a carrier, wherein the active component is an alkaline metal salt, and the carrier is a composite carrier having several mesoporous channel structures and composed of activated alumina and a molecular sieve. Compared with the prior art, the present invention improves the utilization effect of the active component by adjusting the channel structure of the composite carrier in the adsorbent so that it has a mesoporous structure with a pore size distribution of 2 to 20 nm and 20 to 50 nm, thereby extending the single use time of the adsorbent and reducing the regeneration frequency, thereby achieving the purpose of reducing operating energy consumption in industrial applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adsorbent preparation, and relates to a regenerable adsorbent for removing hydrogen sulfide and a preparation method thereof. Background Art

[0002] In the petrochemical industry, the presence of hydrogen sulfide is extremely harmful. It not only causes equipment damage, catalyst poisoning, and product quality degradation, but also poses a great threat to the life safety of operators. Therefore, in order to avoid the harm caused by hydrogen sulfide, it must be removed.

[0003] There are many methods for removing hydrogen sulfide in the industry, which can be summarized into chemical removal and physical removal. For example, US13395834B discloses a method for removing hydrogen sulfide from hydrocarbon streams, using zinc oxide to react with hydrogen sulfide to reduce the hydrogen sulfide content in the raw material to a certain range. US03400389 discloses a method for preparing a molecular sieve adsorbent and examines its removal effect on polar impurities such as H2S.

[0004] In order to meet the needs of industrial continuous production and reduce the discharge of solid waste, renewable hydrogen sulfide adsorbents are receiving more and more attention. CN110882675 discloses a mixed powder obtained by pre-treating pseudo-boehmite, polyethylene glycol and tetraethyl orthosilicate, and then calcining to obtain a renewable hydrogen sulfide gas adsorbent. CN113231037 discloses a solid amine adsorbent for removing trace hydrogen sulfide. It is prepared by using oxidatively modified activated carbon as a carrier, then using a grafting method to immobilize tert-butylaminopropyltrimethoxysilane on the oxidatively modified activated carbon, and finally loading the tertiary amine on the immobilized activated carbon. CN103769043 discloses a gas desulfurization adsorbent, its preparation method and application. The adsorbent uses M41S series mesoporous materials as a carrier, zinc oxide as an active component, and adds a promoter, calcium oxygen acid salt, and VB / VIB group metal oxide. The adsorbent can effectively remove sulfides at high temperatures. CN112295544 discloses a hydrogen sulfide adsorbent having a modified metal organic compound skeleton, a preparation method and an application thereof. The preparation method of the invention comprises heat-treating a mixed solution containing an aluminum source, terephthalic acid, activated carbon and water, and then calcining to obtain a metal organic skeleton adsorbent.

[0005] Although the above-mentioned renewable adsorbent can maintain a certain adsorption effect on H2S, it still has some defects, such as being able to be used only at high temperatures, the adsorbent preparation process is too complicated, and the manufacturing cost is high. Summary of the invention

[0006] The purpose of the present invention is to provide a regenerable adsorbent for hydrogen sulfide removal and a preparation method thereof. By optimizing the pore structure of the composite carrier of activated alumina and ZSM-5 molecular sieve, the composite carrier has several (may be two) mesoporous pore structures, and the pore distribution is more concentrated, thereby improving the utilization rate of the active ingredients in the adsorbent and increasing the single use time of the adsorbent, thereby reducing the regeneration frequency.

[0007] The object of the present invention can be achieved by the following technical solutions:

[0008] One of the technical solutions of the present invention provides a regenerable adsorbent for hydrogen sulfide removal, which consists of two parts: an active component and a carrier, wherein the active component is an alkaline metal salt, and the carrier is a composite carrier having several mesoporous channel structures and composed of activated alumina and molecular sieves.

[0009] Furthermore, the mesoporous channel structure in the composite carrier includes two types, namely, mesopores with a channel diameter of 2 to 20 nm and mesopores with a channel diameter of 20 to 50 nm. Furthermore, the volume ratio of the mesopores with a channel diameter of 2 to 20 nm to the total channel structure in the composite carrier is (0.1 to 0.45):1, preferably, 0.15 to 0.35:1; the volume ratio of the mesopores with a channel diameter of 20 to 50 nm to the total channel structure in the composite carrier is (0.1 to 0.35):1, preferably 0.1 to 0.3:1.

[0010] Furthermore, the activated alumina in the composite carrier is chi-phase alumina, rho-phase alumina, eta-phase alumina or a mixture thereof; preferably, the activated alumina carrier is activated alumina obtained by rapid dehydration of aluminum hydroxide by high-temperature calcination, and more preferably, the secondary aggregated particle size distribution of the activated alumina is 10 to 40 microns.

[0011] Further, the molecular sieve is a ZSM-5 molecular sieve, and the silicon-aluminum ratio of the molecular sieve is 15 to 150. Preferably, the silicon-aluminum ratio of the ZSM-5 molecular sieve used is 20 to 100, and the particle size of the molecular sieve is 2 to 50 microns. It should be noted that the ZSM-5 molecular sieve of the present invention does not need to contain a mesoporous structure. As is familiar to those skilled in the art, a ZSM-5 molecular sieve with a mesoporous structure can be obtained by adding an organic soft template, an activated carbon hard template, or using means such as dissolving aluminum and dissolving silicon during the synthesis of the ZSM-5 molecular sieve. However, obtaining a ZSM-5 molecular sieve with a multi-level pore structure by such a method alone often increases the manufacturing cost, and is therefore not recommended. In the present invention, it is found that the introduced active component has a suitable alkalinity, and only a slight change in the way the active component is added can be used to load the active component on the carrier while utilizing its alkaline characteristics to make the ZSM-5 molecular sieve additionally form a mesoporous structure, and then by refining parameters such as the amount of addition and temperature, the mesoporous distribution can be effectively regulated.

[0012] Furthermore, the active component is an alkaline metal salt, including aluminate, and at least one of carbonate and hydroxide; the metal ion is one of sodium or potassium or a mixture of the two. Preferably, the alkaline metal ion is sodium ion.

[0013] Further, the mass proportion of the active component is 5-22wt%, and the mass proportion of the composite carrier is 78-95wt%. Preferably, the carrier accounts for 85-95%wt, and the active component accounts for 5-15%wt. More preferably, the carrier accounts for 87.5-92%wt, and the active component accounts for 8-12.5%wt. The composite carrier activated alumina and molecular sieve are calculated in a mass ratio of (1-5):1, and preferably the mass ratio of activated alumina to molecular sieve is (2-4):1.

[0014] The second technical solution of the present invention provides a method for preparing a regenerable adsorbent for removing hydrogen sulfide, comprising the following steps:

[0015] (1) weighing activated alumina, molecular sieve and a first solution of alkaline metal salt according to a mass ratio, mixing to form a mixed slurry solution, stirring, drying and crushing to obtain a mixed powder;

[0016] (2) The obtained mixed powder is mixed with a second salt solution, molded, dried, and calcined to obtain the target product.

[0017] Furthermore, in step (1), the total mass proportion of activated alumina and molecular sieve in the mixed slurry solution is 5wt% to 40wt%, preferably 10 to 35%wt, and the mass proportion of the first solution of alkaline metal salt is 60wt% to 95wt%, preferably 65 to 90%wt, wherein the concentration of the first solution of alkaline metal salt is 2.8wt% to 5wt%.

[0018] Furthermore, in step (1), the cation in the first solution of the alkaline metal salt is at least one of sodium ion or potassium ion, and the anion is aluminate ion, or a mixture of aluminate ion and hydroxide ion. Preferably, the metal element is sodium. The aluminate is preferably a freshly prepared solution. An optional implementation method is to react NaOH with Al(OH)3 in a ratio of (1.1 to 1.2):1 to obtain sodium aluminate. A slight excess of alkali is beneficial to maintaining the stability of the sodium aluminate, and the obtained sodium aluminate can be stored for a longer period of time.

[0019] Furthermore, in step (1), the stirring temperature is 60-100°C and the stirring time is 4-15 hours. Preferably, the temperature is controlled at 70-85°C and the time is maintained at 8-12 hours. More preferably, the stirring process is carried out under sealed conditions to avoid pH fluctuations of the slurry solution due to water loss. The drying temperature of the mixed slurry solution is 100-180°C and the time is 0.5-8 hours.

[0020] Furthermore, in step (2), the mass ratio of the mixed powder to the second salt solution is 1.3-2.0:1.

[0021] Furthermore, in step (2), the mass concentration of the second salt solution is 0.5-5%, and the cations contained therein are a mixture of one or two of sodium ions or potassium ions, and the anions contained therein are a mixture of one or more of bicarbonate ions, acetate ions, and oxalate ions. Here, the purpose of selecting acetate or oxalate is to utilize this type of organic salt to release gas during roasting to construct secondary pores, thereby further improving the pore distribution inside the adsorbent, improving the diffusion and mass transfer of gas on the surface of the adsorbent, and then improving the adsorption performance (at the same time, the acetate, oxalate ions, etc. after roasting will decompose into carbonates). Preferably, the second salt solution contains bicarbonate and one of acetate or oxalate, and more preferably bicarbonate and acetate, the mass ratio of the two is 1:1.

[0022] Furthermore, in step (2), the drying temperature is 100-120°C and the drying time is 1-12 hours. The drying method can be oven drying, and the drying space can be assisted by providing negative pressure conditions to accelerate the evaporation of water, and then the obtained cake or block material is crushed and ground to obtain a powder for easy molding; a more preferred drying method is to directly obtain a mixed powder by spray drying; preferably, the particle size range of the mixed powder is 10-40 microns.

[0023] Furthermore, in step (2), the specific process conditions for roasting are: first, maintain the temperature at 200-250°C in the low temperature section for 0.5-1h, maintain the temperature at 400-450°C in the medium temperature section for 0.5-1h, and maintain the temperature at 550-600°C in the high temperature section for 0.5-1h. Preferably, the temperature in the low temperature section is controlled at 230-250°C and maintained for 1h, the temperature in the medium temperature section is controlled at 400-430°C and maintained for 1h, and the temperature in the high temperature section is controlled at 560-580°C and maintained for 0.5h, and the heating rate is controlled at 5-10°C / min.

[0024] Furthermore, the mixed powder can be formed into adsorbents in different shapes such as bars, spheres, hollow bars, honeycombs, etc. By using different molding equipment and adjusting the molding conditions, the adsorbent with suitable particle size can be selected to meet the needs of industrial operation and optimize the pressure drop, mechanical wear and other parameters of the adsorbent during operation.

[0025] The present invention combines activated alumina and ZSM-5 molecular sieve as adsorbent carriers, and then adjusts the pore structures of the molecular sieve and alumina under alkaline conditions to form two mesoporous pore structures. On the one hand, the pore structure of the adsorbent is optimized to improve the utilization rate of the active components, and on the other hand, the diffusion rate of the molecules in the composite carrier is adjusted to reduce the occurrence of side reactions. In addition, since the alkaline components are retained as active species, no secondary washing is required, no waste liquid is generated, and it is more economical and environmentally friendly, and suitable for industrial production.

[0026] On the third aspect, the patent of the present invention provides a regenerable adsorbent for hydrogen sulfide adsorption, and its use conditions are 20-80°C. When used in industry, it is usually combined with the TSA process. The adsorbent is loaded in two adsorption towers or multiple adsorption towers. When one of the adsorption towers fails (the outlet H2S concentration is higher than the process design value), the adsorption tower is switched to regeneration mode; during regeneration, the adsorbent is heated with a carrier gas at 200-300°C, preferably with a carrier gas at 250-280°C to heat the bed, so that the adsorbed hydrogen sulfide is resolved and its adsorption capacity for hydrogen sulfide is restored again.

[0027] Furthermore, the regeneration gas may be selected from nitrogen, hydrogen, and alkane gases.

[0028] Furthermore, the adsorbent provided by the present invention has the advantage of being repeatedly used without attenuation, and the adsorbent obtained by the preparation method has a longer service life. Usually, the adsorbent will be irreversibly deactivated due to carbon deposition and side reactions, resulting in its operating life continuously attenuating. Specifically, the adsorbent provided by the present invention can maintain its adsorption capacity unchanged after repeated regeneration 20 times.

[0029] The present invention improves the utilization rate of active components by optimizing the pore structure of the adsorbent. Compared with existing industrially applied adsorbents, the single-time service life can be increased by more than double. Compared with the prior art, the present invention has the following advantages:

[0030] 1) Compared with the prior art, the adsorbent of the present invention has richer and more concentrated mesoporous channels, which improves the utilization effect of the active components of the adsorbent and increases the single service life of the adsorbent, thereby reducing the regeneration frequency of industrial operation and saving operating energy consumption.

[0031] 2) The regenerable adsorbent obtained by the preparation method has a high removal accuracy of hydrogen sulfide, which can reach 0.1ppm, and can be regenerated repeatedly. After repeating the cycle process for 20 times, the adsorption performance remains unchanged.

[0032] 3) The adsorbent preparation process of the present invention is green, economical, efficient and suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a comparison diagram of pore size distribution between Example 5 and Comparative Example 1;

[0034] Figure 2 It is a comparison chart of the adsorption capacity test of Example 5 and Comparative Example 1. DETAILED DESCRIPTION

[0035] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0036] In the following examples, the commercially available activated alumina powder was purchased from Aluminum Corporation of China; the ZSM-5 molecular sieve was purchased from the NKF-5 series molecular sieve products produced by the Catalyst Plant of Nankai University; the hydrogen sulfide standard gas was customized from Air Liquide, France. Other reagents were purchased from Sinopharm Group.

[0037] In the following examples, the prepared catalyst samples were subjected to desulfurization performance evaluation tests and butadiene side reaction evaluation experiments, as follows:

[0038] Table 1 Adsorbent evaluation conditions

[0039]

[0040]

[0041] The specific evaluation method is as follows: first, add 40.0g of adsorbent into the fixed bed reactor, pass hydrogen to purge the system, and then start the evaluation after the system pressure stabilizes at 1.5MPa. First, switch the gas line, introduce hydrogen sulfide standard gas into the system, set the mass flow meter parameter to 2000ml / min, and start the evaluation. The tail gas is passed into the gas chromatograph, and the tail gas is collected every 3 minutes. When the outlet concentration of hydrogen sulfide is greater than 0.1ppm, the adsorption is considered saturated and the regeneration process begins. First, switch the gas line to hydrogen, purge the system for 10 minutes, and start heating. When the bed temperature reaches 250°C, keep the temperature constant for 4h, and the regeneration is completed. After the system cools down to room temperature, switch the gas line to hydrogen sulfide standard gas and start the second adsorption.

[0042] The butadiene side reaction evaluation experiment is evaluated by the McBain device. The test condition is 30℃. After the system is evacuated, butadiene is introduced to increase the system pressure to about 100 torr and maintained at the test temperature for 48 hours. The degree of polymerization of butadiene in the sample is evaluated by the change in sample mass. The lighter the sample weight gain, the lower the degree of polymerization.

[0043] [Example 1]

[0044] Step 1: weigh 100 g of activated alumina and 100 g of ZSM-5 molecular sieve with a silicon-aluminum ratio of 15, add them into 375 g of 2.8% wt sodium aluminate solution, and maintain at 80° C. for 4 hours under stirring.

[0045] Step 2: Dry the slurry solution obtained in step 1 at 100° C. for 8 hours, and then crush and grind to obtain a modified mixed powder.

[0046] Step 3: Mix 150g of the mixed powder obtained in step 2 with 80g of sodium acetate and sodium bicarbonate with a concentration of 0.5%wt, wherein the mass ratio of sodium acetate to sodium bicarbonate is 1:1, mix and shape to obtain spherical particles, then dry at 100°C, and then calcine at 200°C for 1h, 450°C for 0.5h, and 550°C for 0.5h to obtain a finished adsorbent. Marked as sample S-1.

[0047] [Example 2]

[0048] Step 1: weigh 100 g of activated alumina and 20 g of ZSM-5 molecular sieve with a silicon-aluminum ratio of 150, add them into 360 g of 5% wt sodium aluminate solution, and maintain at 80° C. for 4 hours under stirring.

[0049] Step 2: spray-dry the slurry solution obtained in step 1 at 180° C. for 0.5 h to obtain a modified mixed powder.

[0050] Step 3: 130 g of the mixed powder obtained in step 2 is mixed with 100 g of sodium acetate and sodium bicarbonate with a concentration of 3.0% wt, wherein the mass ratio of sodium acetate to sodium bicarbonate is 1:1, mixed and molded to obtain strip particles, then dried at 100° C., and then calcined at 200° C. for 1 h, 450° C. for 0.5 h, and 550° C. for 0.5 h to obtain a finished adsorbent. Marked as sample S-2.

[0051] [Example 3]

[0052] Step 1: weigh 100 g of activated alumina and 50 g of ZSM-5 molecular sieve with a silicon-aluminum ratio of 20, add them into 1350 g of 5% wt sodium aluminate solution, and maintain at 80° C. for 4 hours under stirring.

[0053] Step 2: Dry the slurry solution obtained in step 1 at 100° C. for 8 hours, and then crush and grind to obtain a modified mixed powder.

[0054] Step 3: 120 g of the mixed powder obtained in step 2 is mixed with 80 g of sodium acetate and sodium bicarbonate with a concentration of 0.5% wt, wherein the mass ratio of sodium acetate to sodium bicarbonate is 1:1, mixed and molded to obtain spherical particles, then dried at 100° C., and then calcined at 200° C. for 1 h, 450° C. for 0.5 h, and 550° C. for 0.5 h to obtain a finished adsorbent. Marked as sample S-3.

[0055] [Example 4]

[0056] Step 1: weigh 100 g of activated alumina and 20 g of ZSM-5 molecular sieve with a silicon-aluminum ratio of 100, add them into 223 g of 2.8% wt sodium aluminate solution, and maintain at 80° C. for 4 hours under stirring.

[0057] Step 2: Dry the slurry solution obtained in step 1 at 100° C. for 8 hours, and then crush and grind to obtain a modified mixed powder.

[0058] Step 3: Mix 120g of the mixed powder obtained in step 2 with 60g of sodium acetate and sodium bicarbonate with a concentration of 3%wt, wherein the mass ratio of sodium acetate to sodium bicarbonate is 1:1, mix and shape to obtain spherical particles, then dry at 100°C, and then calcine at 200°C for 1h, 450°C for 0.5h, and 550°C for 0.5h to obtain a finished adsorbent. Marked as sample S-3.

[0059] [Example 5]

[0060] Step 1: weigh 100 g of activated alumina and 100 g of ZSM-5 molecular sieve with a silicon-aluminum ratio of 75, add them into 466 g of 2.8% wt sodium aluminate solution, and maintain at 80° C. for 4 hours under stirring.

[0061] Step 2: Dry the slurry solution obtained in step 1 at 100° C. for 8 hours, and then crush and grind to obtain a modified mixed powder.

[0062] Step 3: 150 g of the mixed powder obtained in step 2 was mixed with 100 g of sodium acetate with a concentration of 3% wt, and shaped into spherical particles, which were then dried at 100° C., and then calcined at 200° C. for 1 h, 450° C. for 0.5 h, and 550° C. for 0.5 h to obtain a finished adsorbent. This was labeled as sample S-5.

[0063] [Example 6]

[0064] Example 6 is similar to Example 5, except that the concentration of sodium metaaluminate in the first step is 5% wt., which is labeled as sample S-6.

[0065] [Example 7]

[0066] Step 1: weigh 100 g of activated alumina and 60 g of ZSM-5 molecular sieve with a silicon-aluminum ratio of 100, add them into 373 g of a 5% wt mixed solution of sodium aluminate and sodium hydroxide, and maintain at 60° C. for 4 hours under stirring.

[0067] Step 2: Dry the slurry solution obtained in step 1 at 100° C. for 8 hours, and then crush and grind to obtain a modified mixed powder.

[0068] Step 3: 160 g of the mixed powder obtained in step 2 was mixed with 100 g of sodium acetate with a concentration of 3% wt, and shaped into spherical particles, which were then dried at 100° C., and then calcined at 200° C. for 1 h, 450° C. for 0.5 h, and 550° C. for 0.5 h to obtain a finished adsorbent. The finished adsorbent was labeled as sample S-7.

[0069] [Example 8]

[0070] Example 8 is similar to Example 7, except that in step 1, the heating time is 12 h and the heating temperature is 100° C. It is labeled as sample S-8.

[0071] [Example 9]

[0072] Step 1: weigh 100 g of activated alumina and 25 g of ZSM-5 molecular sieve with a silicon-aluminum ratio of 20, add them to 292 g of a 5% wt mixed solution of sodium aluminate and potassium hydroxide, and maintain at 80° C. for 4 hours under stirring.

[0073] Step 2: Dry the slurry solution obtained in step 1 at 100° C. for 8 hours, and then crush and grind to obtain a modified mixed powder.

[0074] Step 3: 120 g of the mixed powder obtained in step 2 was mixed with 90 g of sodium acetate with a concentration of 3% wt, and shaped into spherical particles, which were then dried at 100° C., and then calcined at 200° C. for 0.5 h, 400° C. for 0.5 h, and 550° C. for 0.5 h to obtain a finished adsorbent, which was labeled as sample S-9.

[0075] [Example 10]

[0076] Example 10 is similar to Example 9, except that the calcination conditions in step 3 are changed to 250° C. for 1 h, 450° C. for 1 h, and 600° C. for 1 h. It is labeled as sample S-10.

[0077] [Comparative Example 1]

[0078] The regenerable hydrogen sulfide adsorbent EZ-500, which is currently in industrial application, is selected and marked as comparison 1.

[0079] [Comparative Example 2]

[0080] Similar to Example 5, except that in step 3, the 3% sodium acetate solution is replaced by water.

[0081] Table 1 Performance results of adsorbents in Examples 1 to 10 and Comparative Example 1

[0082]

[0083] Table 2 Evaluation results of adsorbents of Examples 1-10 and Comparative Example 1

[0084]

[0085]

[0086] For relevant performance test results of Example 5 and Comparative 1, see Figure 1 and Figure 2 shown.

[0087] Embodiment 11:

[0088] Compared with Example 1, most of the contents are the same, except that in this example, the total mass of activated alumina and molecular sieve is adjusted in equal proportion so that the total mass of activated alumina and molecular sieve accounts for 5 wt % in the mixed slurry solution.

[0089] Embodiment 12:

[0090] Compared with Example 1, most of the contents are the same, except that in this example, the total mass of activated alumina and molecular sieve is adjusted in equal proportion so that the total mass of activated alumina and molecular sieve accounts for 40 wt % in the mixed slurry solution.

[0091] Embodiment 13:

[0092] Compared with Example 1, most of them are the same, except that in this example, the calcination temperature conditions are adjusted to: 200°C, keep for 1 hour, keep for 1 hour at 400°C, and keep for 1 hour at 550°C.

[0093] Embodiment 14:

[0094] Compared with Example 1, most of them are the same, except that in this example, the calcination temperature conditions are adjusted to: 250°C, keep for 0.5h, keep for 0.5h at 450°C, keep for 0.5h at 600°C.

[0095] In general, the present invention improves the adsorption capacity of the adsorbent for hydrogen sulfide by adjusting the pore structure inside the adsorbent so that it has richer and more optimized composite pores. The introduction of alkaline metal salts into the adsorbent not only serves as an active component but also as a regulator of the carrier pores. It can simultaneously adjust the pore structure of the composite carrier in the adsorbent so that it has a mesoporous structure with pore size distributions of 2 to 20 nm and 20 to 50 nm, respectively. This approach can improve the utilization effect of the active component, extend the single use time of the adsorbent, reduce the regeneration frequency, and thus reduce the operating energy consumption in industrial applications.

[0096] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A regenerable adsorbent for hydrogen sulfide removal, characterized in that: It consists of two parts: an active component and a carrier, wherein the active component is an alkaline metal salt, and the carrier is a composite carrier having several mesoporous channel structures and composed of activated alumina and molecular sieve; The mesoporous channel structure in the composite carrier includes two types, namely, mesopores with a channel diameter of 2 to 20 nm and mesopores with a channel diameter of 20 to 50 nm; The activated alumina in the composite carrier is chi-phase alumina, rho-phase alumina, eta-phase alumina or a mixed phase thereof; The particle size distribution of the activated alumina in the composite carrier is 10 to 40 microns; The molecular sieve is a ZSM-5 molecular sieve, and the silicon-aluminum ratio of the molecular sieve is 15 to 150; The regenerable adsorbent is prepared by the following method: (1) pretreating the mixed carrier: weighing activated alumina, molecular sieve and the first solution of alkaline metal salt according to the mass ratio, mixing to form a mixed slurry solution, stirring, drying and crushing to obtain a mixed powder; (2) Obtaining an adsorbent with specific shape characteristics: mixing the obtained mixed powder with a second salt solution, forming, drying, and calcining to obtain a target product; In step (1), the total mass proportion of activated alumina and molecular sieve in the mixed slurry solution is 5wt% to 40wt%, and the mass proportion of the first solution of alkaline metal salt is 60wt% to 95wt%, wherein the concentration of the first solution of alkaline metal salt is 2.8wt% to 5wt%; The cation in the first solution of the alkaline metal salt is at least one of a sodium ion or a potassium ion, and the anion is a metaaluminate ion, or a mixture of a metaaluminate ion and a hydroxide ion; In step (1), the stirring temperature is 60-100° C., and the stirring time is 4-15 h; the drying temperature is 100-180° C., and the drying time is 0.5-8 h; In step (2), the mass ratio of the mixed powder to the second salt solution is (1.3-2.0):1; The mass concentration of the second salt solution is 0.5-5%, the cations contained therein are one or a mixture of sodium ions or potassium ions, and the anions contained therein are one or a mixture of bicarbonate ions, acetate ions, and oxalate ions; In step (2), the drying temperature is 100-120°C and the time is 1-12h; the specific process conditions of roasting are: at 200-250°C, keep for 0.5-1h, at 400-450°C, keep for 0.5-1h, at 550-600°C, keep for 0.5-1h; In step (2), the formed adsorbent is in the shape of bars, spheres, hollow bars, or honeycombs.

2. A regenerable adsorbent for hydrogen sulfide removal according to claim 1, characterized in that: The volume ratio of mesopores with a pore diameter of 2 to 20 nm to the total pore structure in the composite carrier is (0.1 to 0.45):1; The volume ratio of the mesopores with a pore diameter of 20 to 50 nm to the total pore structure in the composite carrier is (0.1 to 0.35):

1.

3. A regenerable adsorbent for hydrogen sulfide removal according to claim 1, characterized in that: The mass proportion of the active component is 5-22wt%, and the mass proportion of the composite carrier is 78-95wt%.

4. A method for preparing a regenerable adsorbent for hydrogen sulfide removal according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) pretreating the mixed carrier: weighing activated alumina, molecular sieve and the first solution of alkaline metal salt according to the mass ratio, mixing to form a mixed slurry solution, stirring, drying and crushing to obtain a mixed powder; (2) Obtaining an adsorbent with specific shape characteristics: mixing the obtained mixed powder with a second salt solution, forming, drying, and calcining to obtain a target product; In step (1), the total mass proportion of activated alumina and molecular sieve in the mixed slurry solution is 5wt% to 40wt%, and the mass proportion of the first solution of alkaline metal salt is 60wt% to 95wt%, wherein the concentration of the first solution of alkaline metal salt is 2.8wt% to 5wt%; The cation in the first solution of the alkaline metal salt is at least one of a sodium ion or a potassium ion, and the anion is a metaaluminate ion, or a mixture of a metaaluminate ion and a hydroxide ion; In step (1), the stirring temperature is 60-100° C., and the stirring time is 4-15 h; the drying temperature is 100-180° C., and the drying time is 0.5-8 h; In step (2), the mass ratio of the mixed powder to the second salt solution is (1.3-2.0):1; The mass concentration of the second salt solution is 0.5-5%, the cations contained therein are one or a mixture of sodium ions or potassium ions, and the anions contained therein are one or a mixture of bicarbonate ions, acetate ions, and oxalate ions; In step (2), the drying temperature is 100-120°C and the time is 1-12h; the specific process conditions of roasting are: at 200-250°C, keep for 0.5-1h, at 400-450°C, keep for 0.5-1h, at 550-600°C, keep for 0.5-1h; In step (2), the formed adsorbent is in the shape of bars, spheres, hollow bars, or honeycombs.