A method for preparing a slow-release carbon source filler

By heating, freezing and thawing treatment of polyvinyl alcohol-sodium alginate solution and starch, combined with calcium chloride aqueous solution, a sustained-release carbon source filler with more stable sustained-release performance is prepared, which solves the problem of poor existing sustained-release performance and cost. It solves high problems and achieves stable carbon source release and cost reduction in sewage treatment.

CN115594300BActive Publication Date: 2024-10-29RES INST FOR ENVIRONMENTAL INNOVATION SUZHOU TSINGHUA

Patent Information

Application Number
CN202211376942.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-04
Publication Date
2024-10-29
Estimated Expiration
2042-11-04

AI Technical Summary

Technical Problem

The slow-release performance of existing slow-release carbon source fillers is not stable enough and the cost is high. In addition, there is a problem of insufficient carbon sources in sewage treatment, which affects denitrification efficiency and cost control.

Method used

A slow-release carbon source filler with more stable slow-release performance was prepared by mixing polyvinyl alcohol-sodium alginate solution with starch, heating, freezing and thawing cycles, and combining it with calcium chloride aqueous solution.

Benefits of technology

It improves the stability and cost-effectiveness of the slow-release carbon source filler, achieves stable release of carbon sources for a long time, reduces the cost of carbon source input in sewage treatment, and enhances denitrification efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003926928080000011
    Figure HDA0003926928080000011
  • Figure HDA0003926928080000012
    Figure HDA0003926928080000012
  • Figure HDA0003926928080000021
    Figure HDA0003926928080000021
Patent Text Reader

Abstract

The present invention relates to a method for preparing a slow-release carbon source filler. The method for preparing a slow-release carbon source filler of the present invention comprises the following steps: (1) mixing a polyvinyl alcohol-sodium alginate solution with starch, heating it to boiling and keeping the boiling state for 0.5h to 1h, and then injecting the material into a mold while hot; (2) when the temperature of the material in the mold naturally drops to 50°C to 60°C, adding a calcium chloride aqueous solution to the mold, and standing to obtain a preliminarily formed filler; (3) freezing the preliminarily formed filler at -25°C to -10°C for 8 to 15 hours, thawing it at 20°C to 25°C for 2 to 5 hours, and after 2 to 5 freeze-thaw cycles, drying the filler thawed for the last time to obtain the slow-release carbon source filler. The slow-release carbon source filler of the present invention has a more stable carbon release performance and lower cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention specifically relates to a method for preparing a slow-release carbon source filler. Background Art

[0002] In recent years, due to the excessive use of pesticides and fertilizers, and the large-scale discharge of nitrogen-containing domestic and industrial wastewater into water bodies, nitrate nitrogen pollution in water bodies has become a prominent problem of water pollution. The removal of nitrates in water bodies is a difficult problem in the field of water pollution control. At present, there are two major methods for removing nitrates from water: physical and chemical methods and biological denitrification methods. The physical and chemical methods mainly include ion exchange and membrane separation. The ion exchange treatment process is relatively mature and the investment is relatively low. Its limitations are mainly manifested in: high salt content in the regeneration liquid, difficult to handle; low selectivity, and sulfate and other substances will produce competitive adsorption for nitrates. The membrane separation method mainly includes reverse osmosis and electrodialysis. The disadvantages are high cost, lack of selectivity for nitrates, and the concentrated waste brine produced needs further treatment. Biological denitrification is the most economical and effective denitrification method. It mainly uses denitrifying bacteria to convert nitrate ions and nitrite ions in water into nitrogen gas under anoxic conditions, thereby reducing the concentration of nitrate nitrogen in water.

[0003] For low carbon-nitrogen ratio sewage, insufficient carbon source is one of the main factors affecting the denitrification efficiency of sewage treatment. At present, there is a common problem of insufficient carbon source in urban sewage in my country, which seriously restricts the denitrification process and denitrification efficiency. External carbon sources include liquid carbon sources and solid carbon sources. Among them, liquid carbon sources include sodium acetate, methanol, etc., which have problems such as high cost, difficulty in controlling the dosage, and easy to cause secondary pollution. Solid carbon sources can also serve as growth carriers for denitrifying bacteria while acting as carbon sources. Among them, cellulose solid carbon sources have relatively low operating costs and can increase the denitrification rate to a certain extent. However, solid carbon sources are greatly affected by temperature during the reaction process, and the release of carbon sources is difficult to control. After long-term operation, the denitrification efficiency decreases and post-treatment is difficult, which has certain limitations in practical applications. As a denitrification carbon source and biological carrier, polymers do not need to add organic matter to meet the growth needs of denitrifying bacteria during the denitrification process. Organic matter is dissolved and released under the action of microorganisms. It solves a series of problems caused by the difficulty in controlling the dosage of liquid carbon sources in the denitrification process and ensures the stability of the living environment of denitrifying bacteria. However, polymer materials have a single chemical composition and often require the addition of trace elements to meet the growth needs of microorganisms. In addition, the price of polymer materials is higher than that of natural materials, which is also the reason why the application of such materials is limited. The slow-release carbon source filler obtained by processing natural materials has a relatively low price, relatively higher carbon source performance, and basically no secondary pollution, and has a good application prospect in the field of sewage treatment. However, the slow-release carbon performance of existing slow-release carbon sources is not stable enough, and the cost needs to be further reduced. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a slow-release carbon source filler with more stable carbon release performance and lower cost.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A method for preparing a slow-release carbon source filler, the method comprising the following steps:

[0007] (1) Mixing the polyvinyl alcohol-sodium alginate solution and starch, heating to boiling and maintaining the boiling state for 0.5 h to 1 h, and then injecting the material into a mold while it is hot;

[0008] (2) When the temperature of the material in the mold naturally drops to 50° C. to 60° C., a calcium chloride aqueous solution is added to the mold and allowed to stand to obtain a preliminarily formed filler;

[0009] (3) Freezing the initially formed filler at -25°C to -10°C for 8 to 15 hours, and thawing at 20°C to 25°C for 2 to 5 hours. After 2 to 5 freeze-thaw cycles, drying the filler thawed for the last time to obtain the slow-release carbon source filler.

[0010] Further preferably, in step (3), the initially formed filler is frozen at -25°C to -10°C for 10 to 12 hours, and thawed at 20°C to 25°C for 3 to 4 hours. After 3 to 4 freeze-thaw cycles, the filler thawed for the last time is dried.

[0011] Preferably, the mass ratio of polyvinyl alcohol, sodium alginate and starch in the slow-release carbon source filler is (3-7):1:(6-14).

[0012] Preferably, in step (2), the concentration of the calcium chloride aqueous solution is 3wt% to 6wt%, and the amount of the calcium chloride aqueous solution used is 3% to 8% of the total mass of the material.

[0013] Further preferably, in step (2), the concentration of the calcium chloride aqueous solution is 4wt% to 5wt%, and the amount of the calcium chloride aqueous solution is 4% to 6% of the total mass of the material.

[0014] Preferably, in step (1), in the polyvinyl alcohol-sodium alginate solution, the concentration of polyvinyl alcohol is 10wt% to 20wt%, for example, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%; the concentration of sodium alginate is 3wt% to 5wt%, for example, 3wt%, 4wt%, 5wt%.

[0015] Preferably, the method for preparing the sustained-release carbon source filler further comprises the step of preparing a polyvinyl alcohol-sodium alginate solution, wherein the step of preparing the polyvinyl alcohol-sodium alginate solution is: uniformly mixing polyvinyl alcohol and sodium alginate with water at 45° C. to 55° C.

[0016] More preferably, polyvinyl alcohol and sodium alginate are added into deionized water, heated in a constant temperature water bath at 45° C. to 55° C., and stirred and mixed for 10 to 15 minutes to obtain a polyvinyl alcohol-sodium alginate solution.

[0017] Preferably, in step (3), the drying temperature is 55°C to 65°C.

[0018] Further preferably, in step (3), the drying temperature is 58°C to 62°C.

[0019] Preferably, the drying time is 3 to 5 hours.

[0020] Preferably, in step (1), the heating temperature is 103°C to 107°C.

[0021] Preferably, in step (1), the starch is one or more of potato starch, sweet potato starch or corn starch.

[0022] Preferably, the particle size of the starch is 80 μm to 100 μm, for example, 80 μm, 85 μm, 90 μm, 95 μm, or 100 μm.

[0023] Preferably, in step (1), the polyvinyl alcohol is 1788 (L) type.

[0024] Preferably, the viscosity of the polyvinyl alcohol is 1 mPa·S to 10 mPa·S, for example, 1 mPa·S, 2 mPa·S, 3 mPa·S, 4 mPa·S, 5 mPa·S, 6 mPa·S, 7 mPa·S, 8 mPa·S, 9 mPa·S, or 10 mPa·S.

[0025] Preferably, the viscosity of the sodium alginate is 5 to 20 mPa·S, for example, 5 mPa·S, 8 mPa·S, 10 mPa·S, 12 mPa·S, 14 mPa·S, 16 mPa·S, 18 mPa·S, or 20 mPa·S.

[0026] The present invention also provides a slow-release carbon source filler prepared by the slow-release carbon source filler preparation method.

[0027] The invention also provides application of the slow-release carbon source filler in sewage treatment.

[0028] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:

[0029] The slow-release carbon source filler preparation method of the present invention uses a small number of raw materials with a wide source and low cost. The prepared slow-release carbon source filler has better slow-release stability and can effectively control the investment cost of sewage treatment in terms of added carbon sources. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a physical picture of the slow-release carbon source filler;

[0031] Figure 2 A schematic diagram of a mold for preparing a slow-release carbon source filler;

[0032] Figure 3 This is a state diagram of the slow-release carbon source filler of Example 1 immersed in water for 6 hours;

[0033] Figure 4 This is a state diagram of the slow-release carbon source filler of Comparative Example 1 immersed in water for 6 hours;

[0034] Figure 5 This is a state diagram of the slow-release carbon source filler of Comparative Example 2 immersed in water for 6 hours;

[0035] Figure 6 This is a state diagram of the slow-release carbon source filler of Comparative Example 3 immersed in water for 6 hours;

[0036] Figure 7 This is a state diagram of the slow-release carbon source filler of Comparative Example 4 immersed in water for 6 hours;

[0037] Figure 8 It is a carbon release trend diagram of the slow-release carbon source filler of the embodiment. DETAILED DESCRIPTION

[0038] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the embodiments of the present invention. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.

[0039] In order to solve the problem of poor slow-release carbon performance of existing slow-release carbon sources, the present invention has conducted a lot of exploration and experimental verification on the component formula and preparation process of the slow-release filler, and has proposed an optimized preparation method of the slow-release carbon source filler. The present invention uses polyvinyl alcohol as the skeleton material of the filler, sodium alginate as the skeleton material cross-linking agent, and uses calcium chloride solution to effectively cooperate with polyvinyl alcohol-sodium alginate solution for low-temperature cross-linking, and combines the freeze-thaw cycle operation to make the starch and polyvinyl alcohol uniformly formed. Through the organic combination of the component formula and preparation method of the slow-release filler, the stability of the skeleton structure of the slow-release carbon source filler is improved, and the slow-release performance of the carbon source is improved. At the same time, the components are simple and the source is wide, the cost of the slow-release carbon source filler is reduced, and the stable skeleton structure is conducive to the attachment and survival of microorganisms. The better slow-release performance can stably release the carbon source for a long time, thereby achieving stable and effective removal of pollutants in sewage.

[0040] The technical solution of the present invention is further described below in conjunction with embodiments and comparative examples.

[0041] In the following examples and comparative examples, all raw materials can be purchased commercially and / or prepared by known means, and unless otherwise specified, all meet the requirements of standard chemical products.

[0042] In the following examples and comparative examples, the polyvinyl alcohol is 1788 (L) type with a viscosity of about 5 mPa·S, and the viscosity of sodium alginate is about 10 mPa·S.

[0043] In the following examples and comparative examples, the particle size of potato starch is 80 μm to 100 μm.

[0044] In the present invention, the COD detection method refers to the national standard HJ 828-2017 Determination of Chemical Oxygen Demand of Water Quality - Dichromate Method.

[0045] Example 1

[0046] This embodiment provides a method for preparing a slow-release carbon source filler, which specifically comprises the following steps:

[0047] S1. Add 20 g of polyvinyl alcohol and 6 g of sodium alginate into 200 ml of deionized water, heat in a water bath at 50° C. for 10 minutes, and stir to mix well to obtain a polyvinyl alcohol-sodium alginate solution;

[0048] S2. Prepare a calcium chloride solution with a mass concentration of 4 wt% using anhydrous calcium chloride and ultrapure water, and set aside;

[0049] S3, add 80g potato starch to the polyvinyl alcohol-sodium alginate solution, stir evenly, heat to 105°C and boil, and keep the boiling state for half an hour;

[0050] S4, inject the material after boiling for half an hour into the mold, and add a calcium chloride solution with a mass concentration of 4wt% after the material is naturally cooled to 50°C, the amount of calcium chloride solution added is 5% of the total mass of the material, and then stand for 12 hours to obtain a preliminarily formed filler;

[0051] S5, freezing the initially formed filler at -25°C for 12 hours, thawing at 25°C (normal temperature) for 4 hours, and performing the freezing and thawing cycle 3 times;

[0052] S6. Dry the filler thawed for the last time at 60° C. for 5 hours and then take it out to obtain a slow-release carbon source filler.

[0053] Example 2

[0054] This embodiment is substantially the same as Embodiment 1, except that 60 g of potato starch is added in step S3.

[0055] Example 3

[0056] This embodiment is substantially the same as the embodiment 1, except that 30 g of polyvinyl alcohol is added in step S1, and 60 g of potato starch is added in step S3.

[0057] Example 4

[0058] This embodiment is substantially the same as Embodiment 1, except that 30 g of polyvinyl alcohol is added in step S1, and 40 g of potato starch is added in step S3.

[0059] Example 5

[0060] This embodiment is substantially the same as the embodiment 1, except that 40 g of polyvinyl alcohol is added in step S1, and 40 g of potato starch is added in step S3.

[0061] Example 6

[0062] This embodiment is basically the same as Embodiment 1, except that the freezing temperature in step S5 is -10°C and the freezing time is 10 hours.

[0063] Example 7

[0064] This embodiment is basically the same as Embodiment 1, except that the number of freeze-thaw cycles in step S5 is 2.

[0065] Comparative Example 1

[0066] This comparative example is basically the same as Example 1, except that, without the freezing and thawing step, the initially formed filler is directly dried at 60° C. for 5 hours and then taken out to obtain a slow-release carbon source filler.

[0067] Comparative Example 2

[0068] This comparative example is basically the same as Example 1, except that only one freezing and thawing operation is performed in step S5.

[0069] Comparative Example 3

[0070] This comparative example is substantially the same as Example 1, except that the concentration of the calcium chloride solution prepared in step S2 is 3% by weight, and the amount of the calcium chloride solution added in step S4 is 3% of the total mass of the material.

[0071] Comparative Example 4

[0072] This comparative example is substantially the same as Example 1, except that 10 g of polyvinyl alcohol is added in step S1, and 100 g of potato starch is added in step S3.

[0073] Performance Testing

[0074] Disintegration experiment of sustained-release carbon source filler

[0075] The examples and comparative examples were placed in water, and the state of the slow-release carbon source filler was observed after 6 hours. The experiment found that the slow-release carbon source filler of each example remained in the initial state without disintegration, while the slow-release carbon source filler of each comparative example disintegrated to varying degrees ( Figures 4 to 7 ), among which the disintegration degree of comparative example 1 is the most obvious ( Figure 4 ). The faster the disintegration, the worse the sustained release effect.

[0076] Static carbon release experiment

[0077] Take about 10g (3 grains) of the slow-release carbon source filler of each embodiment, add them to a conical flask containing about 500 ml of deionized water, seal the mouth of the conical flask with a sterile culture container sealing film, place the conical flask in a constant temperature shaking incubator at 25°C, and the shaking frequency is 80rpm. Take out the conical flask after 24 hours, replace the water in the conical flask with 500 ml of deionized water and put it into the constant temperature shaking incubator again. The replaced water is tested for COD concentration (recorded as the first day), and the above static water replacement step is repeated until the 15th day, that is, the immersion experiment is carried out continuously for 15 days, and the carbon release trend graph is drawn. The carbon release curves of the slow-release carbon source fillers of Examples 1 to 7 are shown in FIG. Figure 8 .

[0078] Depend on Figure 8It can be seen that after the first soaking for one day, the COD concentration in the soaking water of the slow-release carbon source fillers of Examples 1 to 7 was about 190 mg / L, which may be caused by the rapid dissolution of sodium alginate into the water on the surface of the carbon source. Subsequently, the COD concentration in the soaking water gradually decreased. From 8 days to 15 days of soaking, the COD concentration was stable at 40-50 mg / L, indicating that it had good carbon release stability during this period. During the treatment period of 8 to 15 days of soaking, the daily organic carbon release rate of Examples 1 to 7 was calculated respectively, and the organic carbon release rate = [COD concentration increased during the release time (mg / L) × deionized water volume (L)] / [mass of slow-release carbon source filler (g) × soaking time (d)], and the organic carbon release rates of Examples 1 to 7 were 2.84 mg / (g·d), 2.67 mg / (g·d), 2.59 mg / (g·d), 2.35 mg / (g·d), 2.27 mg / (g·d), 2.41 mg / (g·d), and 2.52 mg / (g·d) respectively. The organic carbon release rate of Examples 1 to 7 can be stably controlled at 2 to 3 mg / (g·d).

[0079] According to statistics, the material cost of the slow-release carbon source fillers of Examples 1 to 7 is between 20 and 30 yuan / kg. Considering the carbon release performance and cost of the slow-release carbon source fillers, the slow-release carbon source filler prepared in Example 2 has the highest cost performance and has good and stable carbon release performance.

[0080] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a slow-release carbon source filler, characterized in that: The preparation method of the slow-release carbon source filler comprises the following steps: (1) Mixing the polyvinyl alcohol-sodium alginate solution and starch, heating to boiling and maintaining the boiling state for 0.5 h to 1 h, and then injecting the material into a mold while it is hot; (2) When the temperature of the material in the mold naturally drops to 50° C. to 60° C., a calcium chloride aqueous solution is added to the mold and allowed to stand to obtain a preliminarily formed filler; (3) freezing the initially formed filler at -25°C to -10°C for 8 to 15 hours, thawing at 20°C to 25°C for 2 to 5 hours, performing the freezing and thawing cycle 2 to 5 times, and drying the filler thawed for the last time to obtain the slow-release carbon source filler. The mass ratio of polyvinyl alcohol, sodium alginate and starch in the slow-release carbon source filler is 20:6:

60. In step (1), in the polyvinyl alcohol-sodium alginate solution, the concentration of polyvinyl alcohol is 10wt%, the concentration of sodium alginate is 3wt%, In step (2), the concentration of the calcium chloride aqueous solution is 4wt%, and the amount of the calcium chloride aqueous solution is 5% of the total mass of the material.

2. The method for preparing the slow-release carbon source filler according to claim 1, characterized in that: The method for preparing the slow-release carbon source filler further comprises the step of preparing a polyvinyl alcohol-sodium alginate solution, wherein the step of preparing the polyvinyl alcohol-sodium alginate solution is: uniformly mixing polyvinyl alcohol and sodium alginate with water at 45° C. to 55° C.

3. The method for preparing the slow-release carbon source filler according to claim 1, characterized in that: In step (3), the drying temperature is 55° C. to 65° C.; and / or the drying time is 3 to 5 hours.

4. The method for preparing the slow-release carbon source filler according to claim 1, characterized in that: In step (1), the starch is one or more of potato starch, sweet potato starch or corn starch; And / or, the starch has a particle size of 80 μm to 100 μm.

5. The method for preparing the slow-release carbon source filler according to claim 1, characterized in that: In step (1), the polyvinyl alcohol is 1788 (L) type; and / or the viscosity of the polyvinyl alcohol is 1 mPa·S to 10 mPa·S; and / or the viscosity of the sodium alginate is 5 mPa·S to 20 mPa·S.

6. A slow-release carbon source filler prepared by the method for preparing a slow-release carbon source filler according to any one of claims 1 to 5.

7. Use of the slow-release carbon source filler as claimed in claim 6 in sewage treatment.

Citation Information

Patent Citations

  • Polyvinyl alcohol slow-release carbon source material and preparation method thereof

    CN102583742A

  • Hydrated spherical polyvinyl alcohol gel and its production

    JP1990212523A

Cited By

  • Preparation method of slow-release carbon source and application of slow-release carbon source in treatment of low-carbon-nitrogen-ratio wastewater

    CN120288956A

  • Preparation method of slow-release carbon source and application thereof in treatment of low carbon-nitrogen ratio wastewater

    CN120288956B