Suspended polyhydroxy calcium phosphate defluoridation adsorbent and preparation method and application thereof

Through suspended polymerized calcium hydroxyphosphate and polyvinyl alcohol granulation technology, a fluorine removal adsorbent with high efficiency fluorine removal performance and low cost was prepared, which solved the problems of unstable fluorine removal effect and high cost in the existing technology, and achieved safety , environmentally friendly industrial wastewater treatment.

CN115920830BActive Publication Date: 2024-11-15JIANGSU HELPER FUNCTIONAL MATERIALS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211632950.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-19
Publication Date
2024-11-15
Estimated Expiration
2042-12-19

AI Technical Summary

Technical Problem

The prior art has unstable fluorine removal effect, high cost, insufficient material safety and reusability when treating fluorine-containing industrial wastewater, and traditional adsorbents such as activated alumina have potential hazards and high processing costs.

Method used

Use suspended polymerized hydroxy calcium phosphate fluoride removal adsorbent, and granulated with polyvinyl alcohol as a modified binder to form a granular material with a large specific surface area and specific adsorption capacity, for fluorine removal treatment of fluorine-containing wastewater .

Benefits of technology

It realizes efficient, low-cost and safe fluoride ion removal, has good reusability and industrial application prospects, simplifies the preparation process and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115920830B_ABST
    Figure CN115920830B_ABST
Patent Text Reader

Abstract

The invention discloses a suspended poly hydroxy calcium phosphate defluorination adsorbent and a preparation method and application thereof. Hydroxy calcium phosphate is first prepared, and then the calcium hydroxy phosphate is mixed with a certain amount of dissolved polyvinyl alcohol, reacted, and then stirred evenly. The uniform slurry is squeezed out with a syringe, soaked in water for 1 to 1.5 hours, and vacuum dried to obtain the suspended poly hydroxy calcium phosphate defluorination adsorbent. The invention is based on calcium hydroxy phosphate and uses polyvinyl alcohol as a modified binder for granulation. The prepared defluorination adsorbent has the advantages of being green and environmentally friendly, having a large specific surface area, strong selectivity, and good reusability. The preparation method is simple and the reaction conditions are controllable. The defluorination adsorbent can be widely used in the defluorination treatment of fluorine-containing wastewater, can efficiently remove the fluorine element in the wastewater, and has a good practical application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functional materials, and in particular relates to a suspended polyhydroxy calcium phosphate defluoridation adsorbent and a preparation method and application thereof. Background Art

[0002] Fluorine is a trace element that is widely present in water, soil and the atmosphere. A moderate amount of fluorine is beneficial to the development of human teeth and bones, while an excessive or insufficient amount will harm human health, such as dental caries, dental fluorosis and skeletal fluorosis. The "Sanitary Standard for Drinking Water" (GB5479-2006) stipulates that the upper limit of fluoride ion concentration in drinking water is 1.0 mg / L. In recent years, with the rapid development of industries such as coal mines, the discharge of fluorine-containing industrial wastewater has also been increasing, and industrial wastewater such as fluorine-containing mine water has become the main source of fluorine pollution. Therefore, fluorine-containing wastewater must be strictly and effectively treated.

[0003] At present, the main purification methods for fluoride-containing industrial wastewater include coagulation, reverse osmosis, adsorption, etc. Coagulation utilizes the hydrolysis, flocculation, and adsorption properties of soluble aluminum salts. It is simple and easy to operate, but the defluorination effect is often unstable. Reverse osmosis can remove almost all ions, including trace elements that are beneficial to the human body, but the cost is high and its application is limited. Adsorption is most suitable for purifying groundwater, but the traditional activated alumina has a small adsorption capacity, and soluble aluminum ions have potential hazards; bone carbon is rich in hydroxy calcium phosphate and has a good purification and defluorination effect, but the processing cost is high and the fluoride absorption capacity is small. Patent (CN104399430A) discloses a method for preparing a composite defluorination material for defluorination in electrolytic zinc sulfate solution. However, from the perspective of industrial practicality, it is still inconvenient to directly add finely ground mineral powder to the solution, because it needs to be settled or filtered after stirring, which increases the cost and process. Patents CN102259946A, CN102357357A and CN104324684A can all achieve good defluorination effects, but use raw materials containing elements such as Ti, Zr, and Ce, resulting in high costs for these defluorination materials and only suitable conditions. For example, patent CN1966407A discloses a method for defluorination of acidic zinc electrolyte using aluminum salts and phosphates, but this method causes a considerable loss of valuable element zinc in the electrolyte, so they must be granulated to achieve industrial production. Therefore, the development of effective, safe and cheap granular defluorination materials is of great significance for the treatment of fluorine-containing industrial wastewater.

[0004] Hydroxycalcium phosphate (HAP) has a high adsorption capacity for fluoride ions, and its main components, calcium and phosphorus, are components of the human body and are safe to use. However, HAP is directly used as an adsorbent because of its fine particle size, which makes it difficult to quickly filter and ensure complete removal, resulting in inconvenience in use and the risk of nanoparticle hazard. Therefore, how to comprehensively improve the above-mentioned problems existing in the prior art and obtain a green, environmentally friendly, large specific surface area, specific adsorption capacity, low cost, and good reusability defluorination adsorbent is of great significance for improving the specific removal of fluoride content in industrial wastewater. Summary of the invention

[0005] In view of the above-mentioned technical problems, the present invention provides a suspended polyhydroxy calcium phosphate defluorination adsorbent and a preparation method and application thereof. The present invention first prepares calcium hydroxy phosphate and then uses polyvinyl alcohol as a modified binder for granulation. The defluorination adsorbent has the characteristics of being green and environmentally friendly, having a large specific surface area, having specific adsorption capacity, low cost, good reusability, and being industrially producible. The preparation method is simple and the reaction conditions are controllable, and the defluorination adsorbent can be applied to the defluorination treatment of fluoride-containing wastewater.

[0006] The technical solution of the present invention is:

[0007] The present invention relates to a method for preparing a suspended polyhydroxy calcium phosphate defluoridation adsorbent, comprising the following steps:

[0008] S1. preparing calcium hydroxyphosphate;

[0009] S2. Mix hydroxy calcium phosphate with a certain amount of dissolved polyvinyl alcohol to react, then stir evenly, squeeze out the uniform slurry with a syringe, soak it in water for 1 to 1.5 hours, and vacuum dry it to obtain a suspended polymerized calcium hydroxy phosphate defluoridation adsorbent.

[0010] Preferably, the preparation method of calcium hydroxyphosphate comprises the following steps:

[0011] S11, mixing the calcium salt and sulfate solutions, and dissolving them by ultrasonication to obtain a CaSO4·2H2O solution;

[0012] S12, CaSO4·2H2O solution and PO4 3- The materials are mixed, subjected to hydrothermal reaction, then cooled, and the product is centrifuged, washed, dried, and stored for later use.

[0013] Preferably, in step S11, the calcium salt is CaCl2, and the sulfate is Na2SO4; the frequency of the ultrasonic dissolution is 30 kHz, and the time of the ultrasonic dissolution is 4 to 8 minutes;

[0014] After ultrasonic dissolution, stirring and aging are continued to obtain a suspension, which is then filtered, washed, and dispersed in water again to obtain a CaSO4·2H2O solution.

[0015] Preferably, the process of step S12 is: 3- The solution of the substance is added to the CaSO4·2H2O solution and stirred. The mixed solution after stirring is subjected to a hydrothermal reaction and then cooled. The product is centrifuged, washed and dried.

[0016] Preferably, in step S12, PO4 3- The substance is KH2PO4, and the molar ratio of calcium ion to phosphate is 1 to 3:1;

[0017] The stirring speed is 300-600 r / min, and the stirring time is 3-60 min;

[0018] The temperature of the hydrothermal reaction is 80°C and the reaction time is 10-15h;

[0019] The drying temperature is 60-80° C., and the drying time is 8-12 hours.

[0020] Preferably, the process of step S2 is: firstly, mixing calcium hydroxyphosphate with deionized water, ultrasonically dispersing to obtain a calcium hydroxyphosphate mixed solution, then adding polyvinyl alcohol to the calcium hydroxyphosphate mixed solution under stirring conditions to react, then stirring evenly, squeezing out the uniform slurry with a syringe, soaking it in water for 1.5 hours, chopping it into desired particle size, and vacuum drying it.

[0021] Preferably, in step S2, the mass ratio of calcium hydroxyphosphate to deionized water is 1:0.5, and the mass ratio of calcium hydroxyphosphate to polyvinyl alcohol is 1:4;

[0022] The frequency of ultrasonic dispersion is 30kHz, and the time of ultrasonic dispersion is 5 to 10 minutes;

[0023] The reaction was carried out under stirring conditions, the stirring speed was 900-1200 r / min, and the reaction time was 10-15 h;

[0024] The temperature of vacuum drying is 60-80°C and the time is 8-12 hours.

[0025] The present invention also relates to a suspended polymerized calcium hydroxyphosphate defluorination adsorbent, which comprises calcium hydroxyphosphate and a binder, wherein the binder is polyvinyl alcohol. The defluorination adsorbent has a layered structure, and the surface of the layered structure has thorn-like particles. The layered structure is assembled from calcium hydroxyphosphate sheets, and the particles are stacked from polyvinyl alcohol.

[0026] Preferably, the particle size of the calcium hydroxyphosphate is 3 to 6 μm, and the particle size of the defluorination adsorbent is 500 to 1000 μm.

[0027] The present invention also relates to the use of the above-mentioned suspended polyhydroxy calcium phosphate defluorination adsorbent in the defluorination treatment of fluoride-containing wastewater. When in use, the defluorination adsorbent is mixed with the fluoride-containing wastewater, and oscillation adsorption is performed under normal temperature and pressure conditions to achieve adsorption and desorption equilibrium, thereby completing the removal of the fluoride-containing wastewater. Furthermore, the amount of the defluorination adsorbent used in each liter of fluoride-containing wastewater is 2 to 6 g, the pH of the fluoride-containing wastewater is 5 to 6, and the F - The initial concentration is 150-160ppm.

[0028] The beneficial effects of the present invention are:

[0029] (1) The present invention uses granulation technology to modify polyvinyl alcohol on the hydroxy calcium phosphate structure. The defluorination adsorbent has the advantages of large specific surface area, excellent adsorption performance, high removal selectivity, good reusability, etc., and is a new adsorption material with good use value and application prospects; the preparation method of the defluorination adsorbent has the advantages of being green and environmentally friendly, simple preparation process, controllable reaction conditions, low cost, etc., and is suitable for large-scale preparation and conducive to industrial application;

[0030] (2) The fluorine removal adsorbent prepared by the present invention has hydroxyl groups attached to its surface and there are gaps between the sheets, which is conducive to the adsorption of reaction intermediates so that the removal reaction can be carried out more thoroughly;

[0031] (3) The defluorination adsorbent of the present invention can be applied to the defluorination treatment of fluoride-containing wastewater. The defluorination adsorbent is mixed with the fluoride-containing wastewater and can quickly and effectively adsorb the fluoride ions in the wastewater through oscillation adsorption, thereby achieving the purpose of removing fluoride ions from the water body. The defluorination adsorbent has the characteristics of simple application method, high removal efficiency, good reusability, etc., and has a good practical application prospect. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:

[0033] Figure 1 1 is the XRD spectrum of the hydroxy calcium phosphate composite in Example 1. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0035] The raw materials and instruments used in the following examples are all commercially available. In the following examples, unless otherwise specified, the data obtained are the average values ​​of more than three repeated experiments.

[0036] Example 1

[0037] A method for preparing a suspended polyhydroxy calcium phosphate defluoridation adsorbent comprises the following steps:

[0038] (1) Synthetic Calcium Hydroxyphosphate

[0039] (1.1) CaCl2 solution (0.5 L 0.25 M) and Na2SO4 solution (0.5 L 0.25 M) were ultrasonically dissolved at a frequency of 30 kHz for 6 min to fully dissolve into a uniform system. After the ultrasonication, stirring and aging were continued for 1 h. The suspension was then filtered, washed three times with deionized water, and dispersed again in 100 mL of deionized water to obtain a CaSO4·2H2O solution.

[0040] (1.2) 1 L of 0.125 M KH2PO4 solution was added dropwise to the CaSO4·2H2O solution in (1.1), and the mixture was stirred magnetically at a speed of 500 r / min for 40 min. The mixed solution obtained by stirring was transferred to a reactor, heated to 80°C for hydrothermal reaction for 12 h. After the reaction was completed, it was naturally cooled to room temperature. The hydrothermal reaction product was centrifuged, washed, and vacuum dried at 70°C for 10 h to obtain calcium hydroxyphosphate.

[0041] (2) Synthetic defluorination adsorbent

[0042] (2.1) 30 g of 1 mol of calcium hydroxyphosphate prepared in step (1) was mixed with 15 g of deionized water, and ultrasonically dispersed at a frequency of 30 kHz for 5 min to uniformly disperse the calcium hydroxyphosphate in the water to obtain a calcium hydroxyphosphate mixed solution;

[0043] (2.2) Under the condition of magnetic stirring at a speed of 1000 r / min, 120 g of polyvinyl alcohol was added to the hydroxy calcium phosphate mixture obtained in step (2.1) to react for 15 hours, stirred evenly, and the uniform slurry was squeezed out with a syringe, soaked in water for 1.5 hours, and then cut into pieces to the desired particle size, and vacuum dried at 60°C for 10 hours to obtain a granular suspended polymerized hydroxy calcium phosphate defluorination adsorbent, named material A, with an average particle size of 500 μm.

[0044] The XRD pattern of calcium hydroxyphosphate in this example is as follows: Figure 1 As shown in the figure, it can be seen that: compared with the standard Ca5(PO4)3(OH) diffraction card (73-1731) at 2θ=27.5°, 32°, 41° and 47° respectively, its structure is the same as Ca5(PO4)3(OH), proving that the target sample has been successfully synthesized.

[0045] Embodiment 2:

[0046] The preparation method of the defluorination adsorbent of this embodiment is basically the same as the preparation method of the granular suspended polyhydroxy calcium phosphate defluorination adsorbent in Example 1, with the only difference being that the molar ratio of calcium ion to phosphate in Example 2 is 3:1. Specifically, the preparation method of Example 2 uses CaCl2 solution (1L 1.5M), Na2SO4 solution (1L 1.5M) and 1L 0.5M KH2PO4 solution.

[0047] The defluorination adsorbent prepared in Example 2 is named Material B.

[0048] Comparative Examples 1-3

[0049] The preparation method of the granular suspended polyhydroxy calcium phosphate defluoridation adsorbent is basically the same as that in Example 1, the only difference is that the modified binder in Comparative Examples 1-3 is replaced by diatomaceous earth, silica sol, and polyvinylidene fluoride of the same mass in sequence.

[0050] Weigh 0.03 g of each of the defluorination adsorbents prepared in Example 1 and Comparative Examples 1-3 and add them to 100 mL of F - In industrial fluorine-containing wastewater with a concentration of 158ppm, mix evenly, react for 5 hours, and measure the concentration after reaching adsorption and desorption equilibrium. When reused, the adsorbent is desorbed with 20% sodium carbonate for 3 hours, then washed with water for 1 hour, dried in an oven at 80℃ overnight, and stored for use. The subsequent use conditions of the adsorbent are the same as the first use conditions.

[0051] The removal effect is shown in Table 1 below. The calculation formula for the removal rate is: Removal rate = (raw water concentration - effluent concentration) / raw water concentration * 100%.

[0052] Table 1

[0053] Use modifiers First Removal of Fluoride-Containing Wastewater Secondary removal of fluoride-containing wastewater Example 1 Polyvinyl alcohol 93.9% 91.0% Comparative Example 1 diatomite <92% <83% Comparative Example 2 Silica Sol <84% <82% Comparative Example 3 Polyvinylidene fluoride <82% <81%

[0054] As can be seen from the results of Table 1, the removal rate of the defluorination adsorbent of Example 1 is significantly higher than that of the other three, indicating that calcium hydroxyphosphate modified polyvinyl alcohol has higher adsorption activity. If diatomite is used as a modifier, since the energy band position of diatomite is almost not staggered with calcium hydroxyphosphate, the adsorption efficiency of fluorine is not very high. The preparation process of polyvinylidene fluoride is relatively troublesome. Due to the large specific surface area of ​​quantum dots, the number of surface phase atoms increases, and these surface phase atoms have high activity and are extremely unstable. The nanoparticles produced by the polyvinyl alcohol modified calcium hydroxyphosphate adsorbent during the removal process will not only produce a plasma resonance effect, but also can be used as a capture center for electrons and holes, so that the adsorption activity of the material is further improved. It can be seen that compared to other modifiers (such as diatomite, silica sol, polyvinylidene fluoride), the granular suspended polymerized calcium hydroxyphosphate defluorination adsorbent of the present invention with "polyvinyl alcohol" as a modifier has better performance.

[0055] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.

Claims

1. Application of a suspended polyhydroxy calcium phosphate defluoridation adsorbent in defluoridation treatment of fluoride-containing wastewater, characterized in that: The defluorination adsorbent comprises calcium hydroxyphosphate and a binder, wherein the binder is polyvinyl alcohol, the defluorination adsorbent has a layered structure, and the surface of the layered structure has thorn-like particles, the layered structure is assembled from calcium hydroxyphosphate sheets, and the particles are stacked from polyvinyl alcohol; The preparation method of the suspended polyhydroxy calcium phosphate defluoridation adsorbent comprises the following steps: S1. preparing calcium hydroxyphosphate; S2, mixing calcium hydroxyphosphate with a certain amount of dissolved polyvinyl alcohol, reacting, and then stirring evenly, squeezing out the uniform slurry with a syringe, soaking it in water for 1 to 1.5 hours, and vacuum drying to obtain a suspended poly-calcium hydroxyphosphate defluoridation adsorbent; The S1 step includes the following steps: S11, mixing the calcium salt and sulfate solutions, and dissolving them by ultrasonication to obtain a CaSO4·2H2O solution; S12, CaSO4·2H2O solution and PO4 3- The materials are mixed, subjected to hydrothermal reaction, then cooled, and the product is centrifuged, washed, dried, and stored for later use.

2. The use according to claim 1, characterized in that: In step S11, the calcium salt is CaCl2, and the sulfate is Na2SO4; the frequency of the ultrasonic dissolution is 30 kHz, and the time of the ultrasonic dissolution is 4 to 8 min; After ultrasonic dissolution, stirring and aging are continued to obtain a suspension, which is then filtered, washed, and dispersed in water again to obtain a CaSO4·2H2O solution.

3. The use according to claim 1, characterized in that: The process of step S12 is: 3- The solution of the substance is added to the CaSO4·2H2O solution and stirred. The mixed solution after stirring is subjected to a hydrothermal reaction and then cooled. The product is centrifuged, washed and dried.

4. The use according to claim 3, characterized in that: In step S12, PO4 3- The substance is KH2PO4, and the molar ratio of calcium ion to phosphate is 1~3:1; The stirring speed is 300-600 r / min, and the stirring time is 3-60 min; The temperature of the hydrothermal reaction is 80°C and the reaction time is 10 to 15 hours; The drying temperature is 60-80° C., and the drying time is 8-12 h.

5. The use according to claim 1, characterized in that: The process of step S2 is: firstly, calcium hydroxyphosphate is mixed with deionized water, ultrasonically dispersed to obtain a calcium hydroxyphosphate mixed solution, and then polyvinyl alcohol is added to the calcium hydroxyphosphate mixed solution under stirring conditions to react, and then stirred evenly, the uniform slurry is squeezed out with a syringe, soaked in water for 1 to 1.5 hours, shredded to the desired particle size, and vacuum dried.

6. The use according to claim 5, characterized in that: In step S2, the mass ratio of calcium hydroxyphosphate to deionized water is 1:0.5, and the mass ratio of calcium hydroxyphosphate to polyvinyl alcohol is 1:4; The frequency of ultrasonic dispersion was 30 kHz, and the time of ultrasonic dispersion was 5 to 10 min; The reaction was carried out under stirring conditions, the stirring speed was 900-1200 r / min, and the reaction time was 10-15h; The temperature of vacuum drying is 60-80 ℃ and the time is 8-12 h.

7. The use according to claim 1, characterized in that: The particle size of the calcium hydroxyphosphate is 3-6 μm, and the particle size of the defluorination adsorbent is 500-1000 μm.

Citation Information

Cited By

  • A fluoride ion adsorbent and its preparation method and application

    CN118416870B