A method for synthesizing perfluoropolyether by gas phase method

The gas phase synthesis of perfluoropolyether using gaseous raw materials addresses the challenges of reaction control and safety in existing methods, enabling efficient and continuous production of perfluoropolyether with high selectivity and diverse molecular weights.

CN115975167BActive Publication Date: 2024-12-03四川道弘新材料股份有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211638708.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-19
Publication Date
2024-12-03
Estimated Expiration
2042-12-19

AI Technical Summary

Technical Problem

Existing methods for synthesizing perfluoropolyether face challenges such as difficult reaction control, high safety risk, low productivity, high cost, and inability to produce continuously due to the use of liquid raw materials and uncontrollable temperature and pressure.

Method used

A gas phase method involving the mixing of perfluoroolefin, chlorotrifluoroethylene, and oxygen, with controlled reaction conditions including ultraviolet light and continuous operation, allowing for the synthesis of perfluoropolyether with high selectivity and safety.

Benefits of technology

The method achieves efficient, controllable, and safe production of perfluoropolyether with reduced by-products, enabling continuous operation and diverse molecular weight products, thus improving productivity and reducing equipment costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115975167B_ABST
    Figure CN115975167B_ABST
Patent Text Reader

Abstract

The present invention provides a method for synthesizing perfluoropolyether by a gas phase method, and relates to the field of chemical industry. The method for synthesizing perfluoropolyether by a gas phase method of the present invention comprises the following steps: (1) mixing perfluoroolefin, chlorotrifluoroethylene and oxygen in a gas phase; (2) performing a photooxidation reaction to obtain. The present invention solves the problems of the existing process for preparing perfluoropolyether, such as complex process, difficult reaction control, great danger, high safety risk, low productivity, high cost, and difficulty in repairing and maintaining the device, and realizes the continuous operation of the device. The method uses hexafluoropropylene or tetrafluoroethylene as raw materials, irradiates with ultraviolet light together with oxygen, and obtains polyether with slightly different structure by oxidative polymerization. After deoxygenation, hydrolysis, washing, distillation, post-treatment, preparation and other processes, a uniform and stable perfluoropolyether surfactant is obtained. The present invention has the advantages of high efficiency, continuity and safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical industry, and in particular to a method for synthesizing perfluoropolyether by a gas phase method. Background Art

[0002] Perfluoropolyether (PFPE for short) is a high molecular polymer that is a colorless, odorless, transparent liquid at room temperature and is only soluble in perfluorinated organic solvents. PFPE has the characteristics of heat resistance, oxidation resistance, radiation resistance, corrosion resistance, low volatility, non-combustion, and good comprehensive properties such as compatibility with plastics, elastomers, and metal materials, making it an extremely reliable lubricant in harsh environments and widely used in chemical, electronic, electrical, mechanical, magnetic media, nuclear industry, aerospace and other fields.

[0003] At present, there are two main methods for preparing perfluoropolyethers: the direct photooxidation of perfluoroolefins and the anionic polymerization of perfluoroepoxides. In the process of obtaining perfluoropolyethers by the anionic polymerization of perfluoroepoxides, hexafluoropropylene oxide is generally used as the starting material. For example: Chinese patent application with publication number CN103030800 describes a method for preparing high molecular weight perfluoropolyethers, that is, polymerizing hexafluoropropylene oxide in the presence of a fluorinated solvent and a metal fluoride catalyst. Chinese patent application with publication number CN103788363 describes the polymerization of hexafluoropropylene oxide in an aprotic solvent using a phase transfer agent and anhydrous alkali metal fluoride as a catalyst. The above patents all use hexafluoropropylene oxide as a raw material, but due to the high cost of hexafluoropropylene oxide, this method is not a very economical method for preparing perfluoropolyethers.

[0004] The direct photo-oxidation method of perfluoroolefins is a more reasonable technology for synthesizing perfluoropolyethers by copolymerizing hexafluoropropylene or tetrafluoroethylene with oxygen, and its application is more extensive. The direct photo-oxidation method of perfluoroolefins uses hexafluoropropylene or tetrafluoroethylene as raw materials, and irradiates them with ultraviolet light at low temperature together with oxygen to obtain polyethers with slightly different structures through oxidative polymerization. Its production process is mainly as follows: tetrafluoroethylene or hexafluoropropylene → photo-oxidative polymerization → crude ether distillation → alkali washing or fluorination refining → fractionation → post-treatment → preparation → PFPE. The patent application with publication number US3704214 describes the process of obtaining perfluoropolyethers from hexafluoropropylene and oxygen, liquid phase, temperature -100 to 80°C, pressure 0.1 to 40 bar, and ultraviolet radiation. The patent application with publication number US5149842 describes the process of obtaining perfluoroalkyl derivatives from fluoroolefins and oxygen, under the conditions of: liquid phase, temperature not higher than 50°C, containing one or more FX groups, where X=F, Cl, O, or ultraviolet radiation as initiator. The preparation process described in the patent application with publication number CN103073410A is as follows: fluorinated olefin monomers, oxygen and molecular weight regulators are subjected to ultraviolet light-induced photochemical reaction at a temperature of -40 to -80°C to generate fluoroether acyl chloride and fluoroether acyl fluoride, which are hydrolyzed under ultraviolet light to generate fluoroether carboxylic acid, which is then washed and purified to obtain the fluoroether carboxylic acid product. The preparation method described in the patent application with publication number CN107501538A is as follows: in the synthesis stage, hexafluoropropylene liquid is concentrated in a reactor, oxygen and initiator are introduced, and low-temperature oxidative polymerization is carried out at -75 to -40°C. The patent application with publication number CN114031762A discloses a preparation process of perfluoropolyether, which specifically places liquid hexafluoropropylene and trifluorochloroethylene in a photochemical reactor, introduces oxygen for photooxidation reaction, and maintains the pressure in the photochemical reactor at 0-0.05MPa, the wavelength of ultraviolet light at 200-400nm, the power of the light source at 200-600w, the temperature at -30--70°C, the reaction time at 4-10h, and after the reaction, the crude product is deoxygenated, distilled, hydrolyzed, washed, and neutralized to obtain the finished product. Judging from the numerous patent methods mentioned above, the direct photo-oxidation preparation process of perfluoroolefins disclosed in the prior art basically has the following defects: (i) The reaction is carried out at low temperature, and the reaction device has very high requirements for the refrigeration system, resulting in high costs; (ii) The raw materials are added to the reactor in liquid form, which is prone to violent reactions; the temperature and pressure of the reaction are poorly controllable, posing a threat to the safety of the process and posing a high risk; (iii) In the reaction system, the temperature increases as the reaction proceeds, resulting in low selectivity of the target product, a large number of by-products, and great difficulty in subsequent treatment of the by-products; (iv) The raw materials are added to the reactor in liquid form at one time, and the reaction materials are released after the reaction is completed. This is an intermittent reaction, and the entire process is time-consuming and is a low-productivity process.

[0005] Therefore, it is necessary to study a safe, efficient and low-cost method for synthesizing perfluoropolyether. Summary of the invention

[0006] The object of the present invention is to provide a method for synthesizing perfluoropolyether by a gas phase process, so as to solve the problems in the existing preparation process of perfluoropolyether, such as difficult reaction control, high safety risk, single variety, low productivity, high cost and inability to produce continuously.

[0007] The above-mentioned object of the present invention is achieved by the following technical solutions:

[0008] The present invention provides a method for synthesizing perfluoropolyether by a gas phase method, which comprises the following steps:

[0009] (1) Perfluoroolefin, chlorotrifluoroethylene and oxygen are mixed in gas phase;

[0010] (2) Carry out photo-oxidation reaction to obtain.

[0011] Furthermore, in step (1), the perfluoroolefin is hexafluoropropylene or tetrafluoroethylene.

[0012] Further, in step (1), the molar ratio of the perfluoroolefin, chlorotrifluoroethylene and oxygen is determined by the target molecular weight of the perfluoropolyether;

[0013] Preferably, the target molecular weight of the perfluoropolyether is 450-800.

[0014] Furthermore, in step (1), the molar ratio of the perfluoroolefin, chlorotrifluoroethylene and oxygen is (1-20):1:(1-10).

[0015] Furthermore, in step (1), the molar ratio of the perfluoroolefin, chlorotrifluoroethylene and oxygen is (6-15):1:(3-7);

[0016] Preferably, in step (1), the molar ratio of the perfluoroolefin, chlorotrifluoroethylene and oxygen is 6:1:7.

[0017] Furthermore, in step (2), the reaction temperature of the photooxidation reaction is -15 to 40°C;

[0018] And / or, in step (2), the reaction pressure of the photooxidation reaction is 0 to 0.05 MPa;

[0019] And / or, in step (2), ultraviolet light is used during the photooxidation reaction.

[0020] The reaction product of the photooxidation reaction of the present invention is in liquid phase, and the reaction system is a volume reduction reaction, so the progress of the reaction is controlled by controlling the reaction pressure.

[0021] Furthermore, in step (2), the reaction temperature of the photooxidation reaction is -15 to 15°C;

[0022] And / or, in step (2), the wavelength of the ultraviolet light is 200 to 500 nm, and the intensity is 10 to 30 Kw;

[0023] Preferably, in step (2), the wavelength of the ultraviolet light is 350 nm and the intensity is 15 Kw.

[0024] Furthermore, in step (2), the photooxidation reaction is a continuous photooxidation reaction carried out in a photooxidation reactor.

[0025] Furthermore, in the photo-oxidation reactor, unreacted perfluoroolefin, chlorotrifluoroethylene and oxygen can be circulated into the photo-oxidation reactor for continuous reaction.

[0026] Furthermore, in step (2), after the photo-oxidation reaction, the product is purified by the purification method of: the reaction solution is subjected to deoxygenation, hydrolysis, water washing, distillation, post-treatment and blending to obtain perfluoropolyether.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The reaction efficiency is high and the reaction is controllable. Since the gas phase method is used to synthesize perfluoropolyether, the mass transfer and heat transfer efficiency is high, and the temperature and pressure of the polymerization reaction are stably controlled, thus achieving efficient, controllable and safe production.

[0029] (2) The selectivity of the target product is high, the by-products are reduced, and the unreacted materials can be recycled into the reaction system to continue the reaction, reducing the consumption of raw materials.

[0030] (3) The raw materials of this synthesis method are in gaseous state. By regulating the gas flow rate and continuously passing it into the reactor, continuous production can be achieved, greatly improving productivity.

[0031] (4) This synthesis method does not require a high cooling capacity of the refrigeration system, greatly reducing equipment costs.

[0032] (5) The amount of each raw material gas added during the reaction can be controlled to synthesize perfluoropolyethers of various molecular weights, thereby making the reaction varieties more diverse.

[0033] In summary, the present invention provides a gas phase synthesis method of perfluoropolyether, which uses gaseous raw materials, has strong controllability and good safety in the reaction process; at the same time, the synthesis method of the present invention has simple process operation, mild reaction conditions, high mass transfer and heat transfer efficiency of gas raw materials, high selectivity of target products, few by-products, and can also achieve continuous production, so the synthesis method of the present invention has high production efficiency. In addition, by regulating the amount of raw materials added during the reaction, various molecular weight perfluoropolyethers can be synthesized to increase product varieties. It can be seen that the synthesis method of the present invention ensures the safety of equipment and processes, and the method can synthesize various molecular weight perfluoropolyethers and achieve continuous production, greatly improving productivity, changing the current state of single perfluoropolyether product variety, extremely low production capacity, and far from meeting actual needs, and has good application prospects.

[0034] Furthermore, the present invention solves the problems of the existing process for preparing perfluoropolyether, such as complex process, difficult reaction control, great danger, high safety risk, low productivity, high cost, and difficulty in equipment repair and maintenance, and realizes the continuous operation of the device. The method uses hexafluoropropylene or tetrafluoroethylene as raw materials, and irradiates with oxygen under ultraviolet light to obtain polyether with slightly different structures through oxidative polymerization. After the processes of deoxygenation, hydrolysis, washing, distillation, post-treatment, and blending, a uniform and stable perfluoropolyether surfactant is obtained. The present invention has the advantages of high efficiency, continuity, and safety.

[0035] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.

[0036] The above contents of the present invention are further described in detail below through specific implementation methods in the form of embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0038] If not otherwise specified, the technical means used in the specific implementation methods are conventional means well known to those skilled in the art, and the raw materials and equipment used can be obtained from public commercial channels.

[0039] The process flow chart of the present invention is as follows Figure 1 shown.

[0040] Example 1: Synthesis of perfluoropolyether by gas phase method

[0041] A continuous reaction mode is adopted, and a mixed gas with a molar ratio of hexafluoropropylene / chlorotrifluoroethylene / oxygen = 6 / 1 / 7 is continuously introduced into the photo-oxidation reactor; the ultraviolet lamp is turned on, the frequency is adjusted to 350nm, and the intensity is 15Kw; the reaction temperature is controlled at -15°C, the reaction pressure is controlled at 0-0.05Mpa, and the reaction is started. During the reaction process, the material is fed and discharged at the same time. The liquid phase of the photo-oxidation reactor is discharged to the crude product collection tank, and then enters the deoxygenation device to remove the peroxygen, and then according to the conventional method, it undergoes hydrolysis, water washing, distillation, post-treatment, and preparation, and finally obtains qualified perfluoropolyether. The unreacted hexafluoropropylene, chlorotrifluoroethylene, and oxygen in the photo-oxidation reactor are condensed by the condenser and enter the mixer for recycling.

[0042] Example 2: Synthesis of perfluoropolyether by gas phase method

[0043] A continuous reaction mode is adopted, and a mixed gas with a molar ratio of hexafluoropropylene / chlorotrifluoroethylene / oxygen = 9 / 1 / 7 is continuously introduced into the photo-oxidation reactor; the ultraviolet lamp is turned on, the frequency is adjusted to 350nm, and the intensity is 15Kw; the reaction temperature is controlled at -15°C, the reaction pressure is controlled at 0-0.05Mpa, and the reaction is started. During the reaction process, the material is fed and discharged at the same time. The liquid phase of the photo-oxidation reactor is discharged to the crude product collection tank, and then enters the deoxygenation device to remove the peroxygen, and then according to the conventional method, it undergoes hydrolysis, water washing, distillation, post-treatment, and preparation processes to finally obtain qualified perfluoropolyether. The unreacted hexafluoropropylene, chlorotrifluoroethylene, and oxygen in the photo-oxidation reactor are condensed by the condenser and then enter the mixer for recycling.

[0044] Example 3: Synthesis of perfluoropolyether by gas phase method

[0045] A continuous reaction mode is adopted, and a mixed gas with a molar ratio of hexafluoropropylene / chlorotrifluoroethylene / oxygen = 6 / 1 / 5 is continuously introduced into the photo-oxidation reactor; the ultraviolet lamp is turned on, the frequency is adjusted to 350nm, and the intensity is 15Kw; the reaction temperature is controlled at -5°C, the reaction pressure is controlled at 0-0.05Mpa, and the reaction is started. During the reaction process, the material is fed and discharged at the same time. The liquid phase of the photo-oxidation reactor is discharged to the crude product collection tank, and then enters the deoxygenation device to remove the peroxygen, and then according to the conventional method, it undergoes hydrolysis, water washing, distillation, post-treatment, and preparation processes to finally obtain qualified perfluoropolyether. The unreacted hexafluoropropylene, chlorotrifluoroethylene, and oxygen in the photo-oxidation reactor are condensed by the condenser and then enter the mixer for recycling.

[0046] Example 4: Synthesis of perfluoropolyether by gas phase method

[0047] A continuous reaction mode is adopted, and a mixed gas with a molar ratio of hexafluoropropylene / chlorotrifluoroethylene / oxygen = 9 / 1 / 5 is continuously introduced into the photo-oxidation reactor; the ultraviolet lamp is turned on, the frequency is adjusted to 350nm, and the intensity is 15Kw; the reaction temperature is controlled at -5°C, the reaction pressure is controlled at 0-0.05Mpa, and the reaction is started. During the reaction process, the material is fed and discharged at the same time. The liquid phase of the photo-oxidation reactor is discharged to the crude product collection tank, and then enters the deoxygenation device to remove the peroxygen, and then according to the conventional method, it undergoes hydrolysis, water washing, distillation, post-treatment, and preparation processes to finally obtain qualified perfluoropolyether. The unreacted hexafluoropropylene, chlorotrifluoroethylene, and oxygen in the photo-oxidation reactor are condensed by the condenser and then enter the mixer for recycling.

[0048] Example 5: Synthesis of perfluoropolyether by gas phase method

[0049] A continuous reaction mode is adopted, and a mixed gas with a molar ratio of hexafluoropropylene / chlorotrifluoroethylene / oxygen = 9 / 1 / 3 is continuously introduced into the photo-oxidation reactor; the ultraviolet lamp is turned on, the frequency is adjusted to 350nm, and the intensity is 15Kw; the reaction temperature is controlled at 15°C, the reaction pressure is controlled at 0-0.05Mpa, and the reaction is started. During the reaction process, the material is fed and discharged at the same time. The liquid phase of the photo-oxidation reactor is discharged to the crude product collection tank, and then enters the deoxygenation device to remove the peroxygen, and then according to the conventional method, it undergoes hydrolysis, water washing, distillation, post-treatment, and preparation, and finally obtains qualified perfluoropolyether. The unreacted hexafluoropropylene, chlorotrifluoroethylene, and oxygen in the photo-oxidation reactor are condensed by the condenser and enter the mixer for recycling.

[0050] Example 6: Synthesis of perfluoropolyether by gas phase method

[0051] A continuous reaction mode is adopted, and a mixed gas with a molar ratio of hexafluoropropylene / chlorotrifluoroethylene / oxygen = 15 / 1 / 3 is continuously introduced into the photo-oxidation reactor; the ultraviolet lamp is turned on, the frequency is adjusted to 350nm, and the intensity is 15Kw; the reaction temperature is controlled at 15°C, the reaction pressure is controlled at 0-0.05Mpa, and the reaction is started. During the reaction process, the material is fed and discharged at the same time. The liquid phase of the photo-oxidation reactor is discharged to the crude product collection tank, and then enters the deoxygenation device to remove the peroxygen, and then according to the conventional method, it undergoes hydrolysis, water washing, distillation, post-treatment, and preparation processes to finally obtain qualified perfluoropolyether. The unreacted hexafluoropropylene, chlorotrifluoroethylene, and oxygen in the photo-oxidation reactor are condensed by the condenser and then enter the mixer for recycling.

[0052] The implementation conditions and results of Examples 1-6 are shown in Table 1.

[0053] Table 1. Implementation conditions and results of Examples 1-6

[0054]

[0055]

[0056] In summary, the present invention provides a gas phase synthesis method of perfluoropolyether, which uses gaseous raw materials, has strong controllability and good safety in the reaction process; at the same time, the synthesis method of the present invention has simple process operation, mild reaction conditions, high mass transfer and heat transfer efficiency of gas raw materials, high selectivity of target products, few by-products, and can also achieve continuous production, so the synthesis method of the present invention has high production efficiency. In addition, by regulating the amount of raw materials added during the reaction, various molecular weight perfluoropolyethers can be synthesized to increase product varieties. It can be seen that the synthesis method of the present invention ensures the safety of equipment and processes, and the method can synthesize various molecular weight perfluoropolyethers and achieve continuous production, greatly improving productivity, changing the current state of single perfluoropolyether product variety, extremely low production capacity, and far from meeting actual needs, and has good application prospects.

Claims

1. A method for synthesizing perfluoropolyether by a gas phase method, characterized in that: It includes the following steps: (1) a perfluoroolefin, chlorotrifluoroethylene and oxygen are mixed in gas phase; the perfluoroolefin is hexafluoropropylene or tetrafluoroethylene; the molar ratio of the perfluoroolefin, chlorotrifluoroethylene and oxygen is (6-15):1:(3-7); (2) performing a photo-oxidation reaction to obtain the product; the reaction temperature of the photo-oxidation reaction is -15 to 15°C; The reaction pressure of the photo-oxidation reaction is 0-0.05 MPa; ultraviolet light is used in the photo-oxidation reaction; the wavelength of the ultraviolet light is 350 nm and the intensity is 15 Kw.

2. The method according to claim 1, characterized in that: The molecular weight of the perfluoropolyether is 450-800.

3. The method according to claim 1, characterized in that: In step (1), the molar ratio of the perfluoroolefin, chlorotrifluoroethylene and oxygen is 6:1:

7.

4. The method according to claim 1, characterized in that: In step (2), the photooxidation reaction is a continuous photooxidation reaction carried out in a photooxidation reactor.

5. The method according to claim 4, characterized in that: In the photo-oxidation reactor, unreacted perfluoroolefin, chlorotrifluoroethylene and oxygen can be circulated into the photo-oxidation reactor for continuous reaction.

6. The method according to claim 1, characterized in that: In step (2), after the photo-oxidation reaction, the product is purified by the purification method of: the reaction liquid is subjected to deoxygenation, hydrolysis, water washing, distillation, post-treatment and blending to obtain perfluoropolyether.

Citation Information

Cited By

  • A continuous flow synthesis device and method for perfluoropolyether oxides

    CN122974251A