Composite seamless steel pipe for oil pipeline and manufacturing method thereof

By using ultra-low carbon Fe-Ni-Cr-Mo-W corrosion-resistant alloy and ceramic lining repair layer, combined with epoxy resin-based composite coating, the corrosion problem of seamless steel pipes in oil pipelines in corrosive environments is solved, and the corrosion problem of seamless steel pipes in oil pipelines is achieved. High strength and corrosion resistance, extending service life.

CN116025774BActive Publication Date: 2024-11-08JIANGYIN WUFENG STEEL PIPE GENERAL FACTORY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211261325.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-14
Publication Date
2024-11-08
Estimated Expiration
2042-10-14

AI Technical Summary

Technical Problem

The existing seamless steel pipes for oil pipelines are prone to corrosion in corrosive environments such as high CO2, H2S, CL-, strong acids or strong alkalis, resulting in stress corrosion and cracking. The existing anti-corrosion measures such as asphalt layer or ceramic linings falling off or mechanical Problem of insufficient performance.

Method used

Using ultra-low carbon Fe-Ni-Cr-Mo-W corrosion-resistant alloy billet, combined with ceramic lining repair layer and epoxy resin-based composite coating, the metal transition layer and ceramic lining layer are formed through aluminum thermal reaction, and repair is used. The glaze fills the cracks in the ceramic layer to form a composite steel pipe with a four-layer structure.

Benefits of technology

It achieves high strength, corrosion resistance and long life of steel pipes. The combination strength of the ceramic lining repair layer and the epoxy resin coating is high, which can effectively resist corrosive substances and environmental media in crude oil and extend its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a composite seamless steel pipe for oil pipeline, which comprises a ceramic lining repair layer, a metal transition layer, a steel pipe layer and an epoxy resin-based composite coating from the inside to the outside. Manufacturing method: S1. Select a steel billet; S2. Heat the steel billet to perforate, continuously roll and size, and heat and quench it again to obtain a seamless steel pipe; S3. Fill the steel pipe with a compound thermite, make it rotate centrifugally, ignite the compound thermite, and after the thermite reaction is completed, a metal transition layer and a ceramic lining layer can be formed on the inner wall of the steel pipe from the outside to the inside; heat the repair glaze, spray it on the inner wall of the steel pipe, cover it on the ceramic layer, slowly rotate the steel pipe to make the molten glaze level and penetrate into the cracks of the ceramic layer, glaze is fired and heat-insulated, and cooled to form a glaze; S4. Spray epoxy resin-based composite material powder on the outer wall of the steel pipe, heat and heat-insulate the powder to melt and cross-link, adhere to the outer wall, cool and solidify to form a film to obtain an epoxy resin-based composite coating. The composite seamless steel pipe is hard inside and tough outside, has good mechanical properties, is corrosion-resistant, and has a long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] Seamless steel pipes can transport oil and natural gas, and can also be used as pipelines for transporting solid materials such as coal. They are widely used in mining, metallurgy, chemical industry, petroleum, coal and other industries.

[0002] Oil and gas fields are mostly distributed in remote areas such as polar regions, ice sheets, deserts, and oceans. During the production process, oil pipelines are often exposed to high CO2, H2S, and CL - In a highly corrosive medium environment such as strong acid or strong alkali, the outer wall of ordinary seamless steel pipes is extremely corrosive. Sulfides, chlorides, organic acids, carbon dioxide and other substances present in crude oil will also seriously corrode pipelines.

[0003] Therefore, the corrosion of seamless steel pipes used in oil pipelines comes from two aspects. One is the corrosion of the outer wall of the steel pipe by the external environment, and the other is the corrosion of the inner wall of the steel pipe by the corrosive substances contained in the crude oil. If the anti-corrosion performance of seamless steel pipes used in oil pipelines is not enough and the anti-corrosion quality does not meet the standards, stress corrosion cracking is prone to occur after long-term use, causing crude oil leakage, causing accidents and polluting the surrounding environment.

[0004] The existing method for solving the corrosion of the outer wall of seamless steel pipes for oil pipelines is to coat an asphalt layer or cement mortar, but the coating layer is thick and easy to fall off.

[0005] The existing technology for solving the inner wall corrosion of seamless steel pipes for oil pipelines includes plastic-lined pipes and ceramic-lined layers. The plastic-lined pipes have good corrosion resistance, but the plastic pipes have low strength, poor mechanical properties, narrow operating temperature range, easy aging and short life. The ceramic-lined layer has good mechanical properties and surface quality, and is often prepared by centrifugal aluminothermic method. During the preparation process, the ceramic layer inevitably cracks due to internal stress and oxide inclusions formed by the different expansion coefficients of the base steel pipe and the ceramic layer, which reduces its corrosion resistance and inner surface quality, seriously affecting the service life of the composite steel pipe and limiting its application.

[0006] Moreover, seamless steel pipes used in oil pipelines are often in high-pressure environments and also need to have good mechanical properties. Summary of the invention

[0007] Based on the above, the present invention provides a composite seamless steel pipe for oil pipeline and a manufacturing method thereof.

[0008] A method for manufacturing a composite seamless steel pipe for an oil pipeline comprises the following steps:

[0009] S1. A solid steel pipe raw material is selected as a steel billet, which includes the following components in weight percentage: C: 0.01-0.02%, Mn: 0.43%-0.51%, W: 1.55-1.74%, Ti: 0.42-0.48%, Ni: 2.4-3.1%, Cr: 7.5%-8.5%, M0: 1.4%-1.8%, CU: 0.12-0.16%, Nb: 0.02-0.04%, V: 0.01-0.02%, Ti: 0.01-0.03%, Ce: 0.02-0.04%, Si: 0.38-0.43%, S<0.002%, P<0.015%, and the balance is Fe and other impurities.

[0010] The carbon content in the above-mentioned steel billet is low, which can improve the corrosion resistance of the seamless steel pipe. The added W and Mn elements can play a role in solid solution strengthening to compensate for the partial strength loss caused by the reduction of C content. During the heat treatment process, a small amount of Ti will precipitate and disperse from the organization and form TiC with C, which greatly improves the yield strength. The presence of Ni element can improve the strength and hardness of the steel pipe after quenching and tempering while maintaining good toughness. The high nickel content also makes it have good resistance to stress corrosion cracking under aqueous corrosion conditions. The high chromium content will precipitate during the quenching and tempering treatment to form a Cr2O3 dense body, which makes it have better resistance to point corrosion. Corrosion and oxidation resistance, especially resistance to CO2 and sulfide corrosion; appropriate Mo content can refine the grains and improve the steel pipe's resistance to sulfide stress corrosion cracking and cyclopentane acid corrosion in antigenic oil; appropriate amounts of Cu, Cr, Mn and Ni can improve the hardenability of the steel; the added V, Ti, Nb microalloying elements can play a role in refining grains and precipitation strengthening during the quenching and tempering process, which can reduce stress concentration, enhance toughness, and reduce the probability of microcracks on the material surface; a small amount of rare earth element Ce can effectively improve the acid corrosion resistance of the steel pipe, which is very cost-effective; and control the content of harmful impurities S and P to improve corrosion resistance.

[0011] S2. The cylindrical solid steel billet described in S1 is uniformly heated to 1230-1265℃ in an annular heating furnace, and is punched on a puncher to form a rough pipe. After dephosphorization with high-pressure water, it is continuously rolled and sizing, and then heated to 960-980℃ again and evenly heated for 30-50min before high-temperature water quenching. During the high-temperature water quenching, the steel pipe is rotated along its own axis, water is axially penetrated through the inner wall of the steel pipe, and the outer wall is sprayed in the form of a water curtain, so that each part of the seamless steel pipe can be evenly cooled to prevent bending; when the temperature drops to 350-380℃, it is changed to water mist cooling to reduce the cooling rate, which can reduce tissue stress and clean the steel pipe; finally, it is changed to air cooling to blow away excess liquid.

[0012] S3. Preparation of ceramic lining repair layer:

[0013] After the bottom of the seamless steel pipe obtained in step S2 is sealed with metal foil, the compound thermite is filled into the seamless steel pipe, and then the steel pipe is clamped on the centrifuge to make the seamless steel pipe centrifugally rotate, and the speed is controlled to be 1500r-1700r / min; the compound thermite is ignited with an energized tungsten wire or an oxyacetylene flame to cause thermite reaction, and the high-speed rotation is maintained for 3-5min. After the thermite reaction is completed, a metal transition layer and a ceramic lining layer can be formed on the inner wall of the steel pipe from the outside to the inside. The high-density molten materials such as Fe, Cr, and Cu produced by the thermite reaction are closely attached to the inner wall of the seamless steel pipe under the action of centrifugation, and at the same time, a thin layer on the surface of the inner wall of the steel pipe is melted, and the metal transition layer is formed after cooling, and the thickness is 1.9-2.5mm; the alumina molten material generated by the reaction is attached to the metal transition layer under the action of centrifugation due to its relatively small density, and a ceramic lining layer is formed on its surface after cooling, and the thickness is 1.6-2.1mm.

[0014] Heat the repair glaze to make it in liquid molten state. After the thermite reaction is completed and before the seamless steel pipe is completely cooled, hot spray the molten repair glaze on the inner wall of the steel pipe to cover the ceramic layer. Slowly rotate the steel pipe to make the molten glaze level and penetrate into the cracks of the ceramic layer. Keep the steel pipe rotating slowly and glaze-fire at 620-640℃ for 80-110min. At this temperature, the steel pipe can be tempered and kept warm at the same time to eliminate the internal stress generated by the phase change during quenching of the steel pipe and optimize the quenching structure. The stress of the ceramic layer and the metal transition layer can also be fully released during the insulation process, so that potential cracks are also released, and the repair glaze immediately penetrates into the cracks for repair. After the insulation is completed, it is cooled with the furnace. After it comes out of the furnace at a certain temperature, compressed gas is introduced into the steel pipe to maintain a certain pressure in the pipe. The introduction of compressed gas at a certain pressure can maintain the surface quality of the inner wall and prevent the incompletely solidified glaze layer from deforming. Finally, it is cooled to room temperature to form a glaze and form a ceramic lining repair layer together with the ceramic layer. The thickness of the ceramic lining repair layer after repair is 2-2.8mm.

[0015] S4. Preparation of epoxy resin-based composite coating: The seamless steel pipe with a ceramic lining repair layer obtained in step S3 is sandblasted and cleaned on its outer wall, and then preheated in an induction heating furnace. The epoxy resin-based composite material powder is then sprayed on the outer wall of the steel pipe by electrostatic spraying, and heated and preserved in an insulation furnace to melt and cross-link the epoxy resin-based composite material powder and bond to the outer wall of the steel pipe. After cooling and curing to form a film, an epoxy resin-based composite coating is obtained. The thickness of the epoxy resin-based composite coating is controlled to be 400-700um by controlling the spraying amount.

[0016] Preferably, the repair glaze comprises the following ingredients: boron oxide, calcium borate, sodium tripolyphosphate, sodium borate, silicon oxide and molybdenum trioxide.

[0017] Furthermore, the weight ratio of the components of the repair glaze is boron oxide: calcium borate: sodium tripolyphosphate: sodium borate: silicon oxide: molybdenum trioxide = 22-24: 6.7-7.4: 1-1.4: 5.6-6.8: 17-19: 7.6-8.8.

[0018] Boron oxide and calcium borate can be used as solvents when heated and melted. Introducing boron into the glaze layer with boride having a lower melting point can reduce the glaze firing temperature and expansion coefficient, improve the glaze layer and increase its wear resistance. Sodium tripolyphosphate can act as a dispersant in the eutectic, improving the flow and wettability of the eutectic and the stability of the components in each part. Boron oxide, calcium borate and sodium tripolyphosphate have low melting points themselves, and the eutectic system formed by them cooperates with sodium borate to act as a solvent by completely melting. Components with higher melting points, such as silicon oxide, can be dispersed and dissolved in the solvent to form a eutectic, which can have a lower temperature point during glaze firing. Molybdenum trioxide can be used as a nucleating agent during low-temperature glaze firing, which can densify the network structure of the glaze, increase the mechanical strength, and has good bonding with the metal surface. In addition to bonding with the ceramic layer, it can also penetrate into the cracks of the ceramic layer and bond with the metal transition layer.

[0019] Preferably, in step S3: the heating and melting temperature of the repair glaze is 800-830°C, the rotation speed of the steel pipe after hot spraying the repair glaze is 20-30r / min, after the glaze firing and insulation is completed, the temperature when it is cooled out of the furnace is 390-410°C, and the pressure in the pipe maintained by introducing compressed gas is 4-6MPa.

[0020] Preferably, the epoxy resin-based composite material powder comprises the following components in weight percentage: 36%-40% bisphenol A epoxy resin, 12%-16% thermoplastic acrylic resin, 9%-14% dicyandiamide, 20%-25% calcium silicate, 7%-10% mica powder, 2%-4% polyurea, 3%-5% polybutyl acrylate, and 0.5%-1% benzoin.

[0021] The epoxy resin-based composite material powder is obtained by mixing the above components in a mixer, then melting and extruding them in an extruder, and finally crushing and grinding them.

[0022] Epoxy resin is used as the matrix, and thermoplastic acrylic resin is used as the second phase to be blended with the epoxy resin matrix. It can cross-link with the epoxy resin to form a network structure, thereby improving film-forming properties, increasing film toughness, and increasing weather resistance. Calcium silicate and mica powder are both fillers, and inorganic salt wear-resistant powder calcium silicate is used as a film-forming filler, which can increase the wear resistance of the coating, reduce the shrinkage of the coating during curing, and enhance the adhesion of the coating. Polyurea has a high viscosity, and a small amount of polyurea can increase the cross-linking density of the dual resin system when it is melted, increase the density of the coating, and improve corrosion resistance. Dicyandiamide is a curing agent, polybutyl acrylate is a leveling agent, and benzoin is a defoaming agent.

[0023] Preferably, in step S4: the steel pipe is preheated to 150-170°C, the heating and insulation temperature is 220-227°C, and the insulation time is 15-30min.

[0024] Preferably, the composite thermite comprises the following powders in parts by weight: 274-288 parts of Fe2O3, 100-110 parts of Al, 5-15 parts of CrO3, 9-14 parts of CuO, 19-33 parts of glass powder, 5-12 parts of cryolite, 15-24 parts of lithium feldspar and 19-33 parts of corundum, and is obtained by grinding and mixing the above powders for 4-7 hours and drying them at 170-190°C.

[0025] Adding an appropriate amount of glass powder to the composite thermite can generate a glass phase of Fe·Al2O3·4SiO2 in the thermite reaction, which can isolate the Fe·Al2O3 phase that is susceptible to corrosion and improve corrosion resistance; the diamond sand powder has a high melting point and hardness, and can be distributed in the ceramic layer to reduce the porosity of the ceramic layer, improve its density, and greatly improve its corrosion resistance and wear resistance; CrO3 and CuO can act as combustion aids when reacting with Al to release a large amount of heat and increase the reaction conversion rate, thereby increasing the residence time of the melt in the liquid phase, allowing the gas to be fully discharged and reducing the porosity; cryolite can act as an emulsifier and a solvent to effectively reduce the melting point of alumina, and lithium feldspar is a low melting point phase that can effectively reduce the viscosity of the melt.

[0026] Preferably, in step S2: "heating to 960-980°C and soaking for 30-50min" before quenching is carried out in a heating furnace, and quicklime is used to adjust the atmosphere in the furnace. During soaking, the rough pipe is also filled with pig iron powder, which can reduce oxidation and burning, ensure dimensional stability, and especially prevent excessive oxide scale from being generated on the inner wall; 8%-12% sodium hydroxide is added to the water for high-temperature water quenching, and the explosion generated when sodium hydroxide crystals are precipitated is used to destroy the steam film formed during water quenching, so as to improve the cooling effect and enhance the quenching effect; fine sand is also mixed in the water when the inner wall is axially penetrated, and the fine sand can also break the steam film; the sodium hydroxide in the water can remove oil, and the explosion of sodium hydroxide at high temperature can also break the oxide scale inevitably generated on the outer wall and inner wall of the rough pipe, and the fine sand can knock down the broken oxide scale on the inner wall of the steel pipe under the action of water flow and steel pipe rotation, which is convenient for the subsequent preparation of the lining layer.

[0027] Preferably, in step S2: during high-temperature water quenching, the rotation speed of the steel pipe along its own axis is 75-85r / min, and the spraying volume of the outer wall water curtain is 2850-2950m 3 / h, the axial water penetration of the inner wall is 3200-3450m 3 / h, and control the water temperature at 20-35℃.

[0028] A composite seamless steel pipe for oil pipeline is made according to the above method, and comprises, from the inner layer to the outer layer, a ceramic lining repair layer, a metal transition layer, a steel pipe layer and an epoxy resin-based composite coating.

[0029] Through the above technical solution, the present invention at least includes the following beneficial effects:

[0030] 1. The seamless steel pipe for oil pipeline prepared by the method of the present invention includes four structural layers, which are hard inside and tough outside, have good mechanical properties, are corrosion-resistant, and have a long service life. The seamless steel pipe made by using the ultra-low carbon Fe-Ni-Cr-Mo-W corrosion-resistant alloy as the steel billet of the present invention has good corrosion resistance and high strength performance; the ceramic lining repair layer prepared by the method of the present invention has a smooth and dense surface, is wear-resistant, and has high hardness, which can improve and ensure the transportation efficiency of crude oil, and has strong chemical inertness, can resist the corrosion of sulfides, chlorides, organic acids, carbon dioxide and other substances in crude oil, and has a long service life when transporting crude oil; the epoxy resin composite coating prepared by the method of the present invention has a high bonding strength with the outer wall of the steel pipe, is not easy to fall off, has a high coating density, can block water and air, and prevent environmental corrosive media from contacting the outer wall of the seamless steel pipe, and has excellent antistatic performance, toughness, wear resistance, erosion resistance, weather resistance, acid and alkali corrosion resistance, and environmental medium corrosion resistance.

[0031] 2. The generation of iron oxide scale on the inner wall of the rough pipe can be reduced by the preferred heat-saturation method before quenching. The generation of iron oxide scale on the inner wall of the rough pipe can be reduced by the preferred water-quenching method. The oil can be removed and the oxide scale inevitably generated on the inner wall of the rough pipe can be removed at the same time. Under the combined effect of the heat-saturation method and the water-quenching method, the inner wall of the rough pipe has a clean surface. After water mist cleaning and air-cooling and drying, the inner lining layer can be directly prepared, which can save the steps of alkali washing and acid washing of the inner wall before preparing the inner lining layer, can reduce the production process and reduce energy consumption.

[0032] 3. The repair glaze provided by the present invention is an ultra-low temperature glass glaze that can be fired quickly. It has a lower glaze firing temperature than other low temperature glass glazes, and the glaze firing and insulation temperature range of the repair glaze overlaps with the tempering and insulation temperature range of the steel pipe. The steel pipe can be tempered while the ceramic lining repair layer is prepared by glazing and insulation at 620-640°C, which can shorten the production process and reduce energy consumption. The ceramic lining repair layer repaired by the repair glaze has no cracks and pores and good surface quality. The repair glaze itself also has excellent corrosion resistance. After filling the cracks of the ceramic lining layer, its corrosion resistance is greatly improved, and the repair glaze that penetrates into the cracks can combine with the metal transition layer, enhance the bonding force between the ceramic lining layer and the metal transition layer, and improve its compressive shear strength. DETAILED DESCRIPTION

[0033] The present invention will now be further described in detail with reference to Examples 1-3 and Comparative Examples 1-4.

[0034] Example 1

[0035] A method for manufacturing a composite seamless steel pipe for an oil pipeline comprises the following steps:

[0036] S1. A solid steel pipe raw material is selected as a steel billet, which includes the following components in weight percentage: C: 0.01%, Mn: 0.48%, W: 1.71%, Ti: 0.45%, Ni: 2.6%, Cr: 8.3%, Mo: 1.7%, Cu: 0.13%, Nb: 0.04%, V: 0.02%, Ti: 0.02%, Ce: 0.03%, Si: 0.4%, S: 0.001%, P: 0.01%, and the balance is Fe and other impurities.

[0037] S2. The cylindrical solid steel billet described in S1 is uniformly heated to 1247°C in an annular heating furnace, and is perforated on a puncher to form a rough pipe. After high-pressure water dephosphorization, it is continuously rolled and sized, and then heated to 974°C in a heating furnace again and soaked for 40 minutes. Quicklime is used to adjust the furnace atmosphere in the heating furnace. During soaking, the rough pipe is also filled with pig iron powder, which can reduce oxidation and burning, ensure dimensional stability, and especially prevent excessive oxide scale from forming on the inner wall; after soaking and taking out of the furnace, high-temperature water quenching is performed, and 10% sodium hydroxide is added to the water for high-temperature water quenching. The explosion generated when sodium hydroxide crystallizes is used to destroy the steam film formed during water quenching, so as to improve the cooling effect and enhance the quenching effect; during the high-temperature water quenching, the steel pipe rotates along its own axis at a rotation speed of 80r / min, and water penetrates axially through the inner wall of the steel pipe, with a water penetration of 3380m 3 / h, the outer wall is sprayed in the form of a water curtain, and the spray volume is 2910m 3 / h, and control the water temperature at 28℃, so that every part of the seamless steel pipe can be evenly cooled to prevent bending; fine sand is also mixed in the water when the inner wall is axially penetrated, and the fine sand can also break the steam film; the sodium hydroxide in the water can remove oil, and the explosion of sodium hydroxide at high temperature can also break the oxide scale that is inevitably produced on the outer and inner walls of the rough pipe. The fine sand can knock down the broken oxide scale on the inner wall of the steel pipe under the action of water flow and steel pipe rotation, which is convenient for the subsequent preparation of the lining layer. When the temperature drops to 367℃, it is changed to water mist cooling to reduce the cooling rate, which can reduce tissue stress and clean the steel pipe; finally, it is changed to air cooling to blow away excess liquid. At this time, the size of the seamless steel pipe is φ242mmx13mm.

[0038] S3. Preparation of ceramic lining repair layer:

[0039] The selected composite thermite includes the following powders in weight proportions: 278 parts of Fe2O3, 105 parts of Al, 12 parts of CrO3, 11 parts of CuO, 26 parts of glass powder, 8 parts of cryolite, 17 parts of lithium feldspar and 26 parts of corundum. The powders are ground and mixed for 7 hours and dried at 190°C.

[0040] After the bottom of the seamless steel pipe obtained in step S2 is sealed with metal foil, the compound thermite is filled into the seamless steel pipe, and then the steel pipe is clamped on the centrifuge to make the seamless steel pipe centrifugal rotate, and the speed is controlled to be 1650r / min. The compound thermite is ignited with an energized tungsten wire or an oxyacetylene flame to cause thermite reaction, and the high-speed rotation is maintained for 5 minutes. After the thermite reaction is completed, a metal transition layer and a ceramic lining layer can be formed on the inner wall of the steel pipe from the outside to the inside. The high-density melts such as Fe, Cr, and Cu produced by the thermite reaction are close to the inner wall of the seamless steel pipe under the action of centrifugation, and at the same time, a thin layer on the surface of the inner wall of the steel pipe is melted, and they are mutually dissolved to form a metallurgical bond. The thickness of the metal transition layer formed after cooling is 2.2mm; the alumina melt generated by the reaction is attached to the metal transition layer under the action of centrifugation due to its relatively small density, and a ceramic lining layer is formed on its surface after cooling, and the thickness is 1.9mm.

[0041] The selected repair glaze includes the following ingredients: boric oxide, calcium borate, sodium tripolyphosphate, sodium borate, silicon oxide and molybdenum trioxide. The weight ratio of each ingredient is boric oxide: calcium borate: sodium tripolyphosphate: sodium borate: silicon oxide: molybdenum trioxide = 23:7.1:1.2:6.1:18:8.1.

[0042] The repair glaze is heated to 822℃ to make it in liquid molten state. After the thermite reaction is completed and before the seamless steel pipe is completely cooled, the molten repair glaze is hot sprayed on the inner wall of the steel pipe to cover the ceramic layer. The steel pipe is slowly rotated to make the molten glaze level and penetrate into the cracks of the ceramic layer. The steel pipe is kept rotating slowly at a speed of 27r / min. The glaze is fired and kept warm at 632℃ for 95min. At this temperature, the steel pipe can be tempered and kept warm at the same time to eliminate the internal stress generated by the phase change during quenching of the steel pipe and optimize the quenching structure. The stress of the ceramic layer and the metal transition layer can also be fully released during the insulation process, so that potential cracks are also released, and the repair glaze then penetrates into the cracks for repair. After the insulation is completed, the pipe is cooled to 405℃ and then taken out of the furnace. Compressed gas is introduced into the steel pipe to maintain the pressure in the pipe at 5.5MPa. The introduction of compressed gas at a certain pressure can maintain the surface quality of the inner wall and prevent the incompletely solidified glaze layer from deforming. Finally, it is cooled to room temperature to form a glaze and form a ceramic lining repair layer together with the ceramic layer. The thickness of the ceramic lining repair layer after repair is 2.5mm.

[0043] S4. Preparation of epoxy resin-based composite coating:

[0044] The selected epoxy resin-based composite material powder includes the following components in weight percentage: 38% bisphenol A epoxy resin, 13% thermoplastic acrylic resin, 11% dicyandiamide, 22% calcium silicate, 8% mica powder, 3% polyurea, 4.2% polybutyl acrylate, and 0.8% benzoin. The epoxy resin-based composite material powder is obtained by mixing the above components in a mixer, then melting and extruding in an extruder, and finally crushing and grinding.

[0045] The seamless steel pipe with a ceramic lining repair layer obtained in step S3 is sandblasted and cleaned on its outer wall, and then preheated to 160°C in an induction heating furnace. The epoxy resin-based composite material powder is then sprayed on the outer wall of the steel pipe by electrostatic spraying, and heated to 224°C in an insulation furnace to melt and cross-link the epoxy resin-based composite material powder and bond it to the outer wall of the steel pipe. After insulation for 25 minutes, it is cooled and solidified to form a film, thereby obtaining an epoxy resin-based composite coating. The thickness of the epoxy resin-based composite coating is controlled to be 500um by controlling the spraying amount.

[0046] The composite seamless steel pipe for oil pipeline prepared according to the method comprises, from the inner layer to the outer layer, a ceramic lining repair layer, a metal transition layer, a steel pipe layer and an epoxy resin-based composite coating.

[0047] Example 2

[0048] A method for manufacturing a composite seamless steel pipe for an oil pipeline comprises the following steps:

[0049] S1. A solid steel pipe raw material is selected as a steel billet, which includes the following components in weight percentage: C: 0.015%, Mn: 0.44%, W: 1.65%, Ti: 0.46%, Ni: 2.8%, Cr: 7.8%, M0: 1.5%, Cu: 0.15%, Nb: 0.03%, V: 0.02%, Ti: 0.03%, Ce: 0.02%, Si: 0.39%, S: 0.0015%, P: 0.012%, and the balance is Fe and other impurities.

[0050] S2. The cylindrical solid steel billet described in S1 is uniformly heated to 1237°C in an annular heating furnace, and is perforated on a puncher to form a rough pipe. After high-pressure water dephosphorization, it is continuously rolled and sized, and then heated to 965°C in a heating furnace again and heated for 35 minutes. Quicklime is used to adjust the furnace atmosphere in the heating furnace. During the heating, the rough pipe is also filled with pig iron powder, which can reduce oxidation and burning, ensure dimensional stability, and especially prevent excessive oxide scale from forming on the inner wall. After being heated and taken out of the furnace, high-temperature water quenching is performed. 9% sodium hydroxide is added to the water for high-temperature water quenching. The explosion generated when sodium hydroxide crystals are precipitated is used to destroy the steam film formed during water quenching, so as to improve the cooling effect and enhance the quenching effect. During the high-temperature water quenching, the steel pipe rotates along its own axis at a rotation speed of 76r / min, and water penetrates axially through the inner wall of the steel pipe, with a water penetration of 3270m 3 / h, the outer wall is sprayed in the form of a water curtain, and the spray volume is 2870m 3 / h, and control the water temperature at 25℃, so that every part of the seamless steel pipe can be evenly cooled to prevent bending; fine sand is also mixed in the water when the inner wall is axially penetrated, and the fine sand can also break the steam film; the sodium hydroxide in the water can remove oil, and the explosion of sodium hydroxide at high temperature can also break the oxide scale that is inevitably produced on the outer and inner walls of the rough pipe. The fine sand can knock down the broken oxide scale on the inner wall of the steel pipe under the action of water flow and steel pipe rotation, which is convenient for the subsequent preparation of the lining layer. When the temperature drops to 355℃, it is changed to water mist cooling to reduce the cooling rate, which can reduce tissue stress and clean the steel pipe; finally, it is changed to air cooling to blow away excess liquid. At this time, the size of the seamless steel pipe is φ242mmx13mm.

[0051] S3. Preparation of ceramic lining repair layer:

[0052] The selected composite thermite includes the following powders in weight proportions: 275 parts of Fe2O3, 110 parts of Al, 8 parts of CrO3, 10 parts of Cuo, 28 parts of glass powder, 6 parts of cryolite, 22 parts of lithium feldspar and 21 parts of corundum. The powders are ground and mixed for 6 hours and dried at 175°C.

[0053] After the bottom of the seamless steel pipe obtained in step S2 is sealed with metal foil, the compound thermite is filled into the seamless steel pipe, and then the steel pipe is clamped on the centrifuge to make the seamless steel pipe centrifugal rotate, and the speed is controlled to be 1550r / min. The compound thermite is ignited with an energized tungsten wire or an oxyacetylene flame to cause thermite reaction, and the high-speed rotation is maintained for 4 minutes. After the thermite reaction is completed, a metal transition layer and a ceramic lining layer can be formed on the inner wall of the steel pipe from the outside to the inside. The high-density melts such as Fe, Cr, and Cu produced by the thermite reaction are close to the inner wall of the seamless steel pipe under the action of centrifugation, and at the same time, a thin layer on the surface of the inner wall of the steel pipe is melted, and they are mutually dissolved to form a metallurgical bond. After cooling, a metal transition layer with a thickness of 2.4mm is formed; the alumina melt generated by the reaction is attached to the metal transition layer under the action of centrifugation due to its relatively small density, and a ceramic lining layer with a thickness of 2mm is formed on its surface after cooling.

[0054] The selected repair glaze includes the following ingredients: boric oxide, calcium borate, sodium tripolyphosphate, sodium borate, silicon oxide and molybdenum trioxide. The weight ratio of each ingredient is boric oxide: calcium borate: sodium tripolyphosphate: sodium borate: silicon oxide: molybdenum trioxide = 24:6.9:1.1:6.6:17:7.7.

[0055] The repair glaze is heated to 827℃ to make it in liquid molten state. After the thermite reaction is completed and before the seamless steel pipe is completely cooled, the molten repair glaze is hot sprayed on the inner wall of the steel pipe to cover the ceramic layer. The steel pipe is slowly rotated to make the molten glaze level and penetrate into the cracks of the ceramic layer. The steel pipe is kept rotating slowly at a speed of 24r / min. The glaze is fired and kept warm at 625℃ for 85min. At this temperature, the steel pipe can be tempered and kept warm at the same time to eliminate the internal stress generated by the phase change during quenching of the steel pipe and optimize the quenching structure. The stress of the ceramic layer and the metal transition layer can also be fully released during the insulation process, so that potential cracks are also released, and the repair glaze then penetrates into the cracks for repair. After the insulation is completed, the pipe is cooled to 395℃ and then taken out of the furnace. Compressed gas is introduced into the steel pipe to maintain the pressure in the pipe at 4.5MPa. The introduction of compressed gas at a certain pressure can maintain the surface quality of the inner wall and prevent the incompletely solidified glaze layer from deforming. Finally, it is cooled to room temperature to form a glaze and form a ceramic lining repair layer together with the ceramic layer. The thickness of the ceramic lining repair layer after repair is 2.4mm.

[0056] S4. Preparation of epoxy resin-based composite coating:

[0057] The selected epoxy resin-based composite material powder includes the following components in weight percentage: 37% bisphenol A epoxy resin, 15% thermoplastic acrylic resin, 10% dicyandiamide, 24% calcium silicate, 7% mica powder, 2% polyurea, 4% polybutyl acrylate, and 1% benzoin. The epoxy resin-based composite material powder is obtained by mixing the above components in a mixer, then melting and extruding in an extruder, and finally crushing and grinding.

[0058] The seamless steel pipe with a ceramic lining repair layer obtained in step S3 is sandblasted and cleaned on its outer wall, and then preheated to 155°C in an induction heating furnace. The epoxy resin-based composite material powder is then sprayed on the outer wall of the steel pipe by electrostatic spraying, and heated to 221°C in an insulation furnace to melt and cross-link the epoxy resin-based composite material powder and bond it to the outer wall of the steel pipe. After insulation for 30 minutes, it is cooled and solidified to form a film, thereby obtaining an epoxy resin-based composite coating. The thickness of the epoxy resin-based composite coating is controlled to be 400um by controlling the spraying amount.

[0059] The composite seamless steel pipe for oil pipeline prepared according to the method comprises, from the inner layer to the outer layer, a ceramic lining repair layer, a metal transition layer, a steel pipe layer and an epoxy resin-based composite coating.

[0060] Example 3

[0061] A method for manufacturing a composite seamless steel pipe for an oil pipeline comprises the following steps:

[0062] S1. A solid steel pipe raw material is selected as a steel billet, which includes the following components in weight percentage: C: 0.02%, Mn: 0.49%, W: 1.57%, Ti: 0.43%, Ni: 2.7%, Cr: 8.1%, M0: 1.6%, Cu: 0.14%, Nb: 0.02%, V: 0.01%, Ti: 0.01%, Ce: 0.04%, Si: 0.41%, S: 0.001%, P: 0.014%, and the balance is Fe and other impurities.

[0063] S2. The cylindrical solid steel billet described in S1 is uniformly heated to 1255°C in a ring furnace heating furnace, and is perforated on a punching machine to form a rough pipe. After high-pressure water dephosphorization, it is continuously rolled and sized, and then heated to 978°C in a heating furnace again and soaked for 45 minutes. Quicklime is used to adjust the furnace atmosphere in the heating furnace. During soaking, the rough pipe is also filled with pig iron powder, which can reduce oxidation and burning, ensure dimensional stability, and especially prevent excessive oxide scale from forming on the inner wall; after soaking and taking out of the furnace, high-temperature water quenching is carried out, and 11% sodium hydroxide is added to the water for high-temperature water quenching. The explosion generated when sodium hydroxide crystals are precipitated is used to destroy the steam film formed during water quenching, so as to improve the cooling effect and enhance the quenching effect; during the high-temperature water quenching, the steel pipe rotates along its own axis at a rotation speed of 84r / min, and water penetrates axially through the inner wall of the steel pipe, with a water penetration of 3410m 3 / h, the outer wall is sprayed in the form of a water curtain, and the spray volume is 2940m 3 / h, and control the water temperature at 32℃, so that every part of the seamless steel pipe can be evenly cooled to prevent bending; fine sand is also mixed in the water when the inner wall is axially penetrated, and the fine sand can also break the steam film; the sodium hydroxide in the water can remove oil, and the explosion of sodium hydroxide at high temperature can also break the oxide scale that is inevitably produced on the outer and inner walls of the rough pipe. The fine sand can knock down the broken oxide scale on the inner wall of the steel pipe under the action of water flow and steel pipe rotation, which is convenient for the subsequent preparation of the lining layer. When the temperature drops to 375℃, it is changed to water mist cooling to reduce the cooling rate, which can reduce tissue stress and clean the steel pipe; finally, it is changed to air cooling to blow away excess liquid. At this time, the size of the seamless steel pipe is φ242mmx13mm.

[0064] S3. Preparation of ceramic lining repair layer:

[0065] The selected composite thermite includes the following powders in weight proportions: 283 parts of Fe2O3, 100 parts of Al, 14 parts of CrO3, 12 parts of Cuo, 20 parts of glass powder, 11 parts of cryolite, 20 parts of lithium feldspar and 30 parts of corundum. The powders are ground and mixed for 5 hours and dried at 180°C.

[0066] After the bottom of the seamless steel pipe obtained in step S2 is sealed with metal foil, the compound thermite is filled into the seamless steel pipe, and then the steel pipe is clamped on the centrifuge to make the seamless steel pipe centrifugal rotate, and the speed is controlled to be 1700r / min. The compound thermite is ignited with an energized tungsten wire or an oxyacetylene flame to cause thermite reaction, and the high-speed rotation is maintained for 3 minutes. After the thermite reaction is completed, a metal transition layer and a ceramic lining layer can be formed on the inner wall of the steel pipe from the outside to the inside. The high-density melts such as Fe, Cr, and Cu produced by the thermite reaction are close to the inner wall of the seamless steel pipe under the action of centrifugation, and at the same time, a thin layer on the surface of the inner wall of the steel pipe is melted, and the metal transition layer is formed after cooling with a thickness of 2mm; the alumina melt generated by the reaction is attached to the metal transition layer under the action of centrifugation due to its relatively small density, and a ceramic lining layer is formed on its surface after cooling, with a thickness of 1.8mm.

[0067] The selected repair glaze includes the following ingredients: boric oxide, calcium borate, sodium tripolyphosphate, sodium borate, silicon oxide and molybdenum trioxide. The weight ratio of each ingredient is boric oxide: calcium borate: sodium tripolyphosphate: sodium borate: silicon oxide: molybdenum trioxide = 22:7.3:1.3:5.8:19:8.5.

[0068] The repair glaze is heated to 810℃ to make it in liquid molten state. After the thermite reaction is completed and before the seamless steel pipe is completely cooled, the molten repair glaze is hot sprayed on the inner wall of the steel pipe to cover the ceramic layer. The steel pipe is slowly rotated to make the molten glaze level and penetrate into the cracks of the ceramic layer. The steel pipe is kept rotating slowly at a speed of 30r / min. The glaze is fired and kept warm at 638℃ for 105min. At this temperature, the steel pipe can be tempered and kept warm at the same time to eliminate the internal stress generated by the phase change during quenching of the steel pipe and optimize the quenching structure. The stress of the ceramic layer and the metal transition layer can also be fully released during the insulation process, so that potential cracks are also released, and the repair glaze then penetrates into the cracks for repair. After the insulation is completed, the pipe is cooled to 400℃ and then taken out of the furnace. Compressed gas is introduced into the steel pipe to maintain the pressure in the pipe at 4MPa. The introduction of compressed gas at a certain pressure can maintain the surface quality of the inner wall and prevent the incompletely solidified glaze layer from deforming. Finally, it is cooled to room temperature to form a glaze and form a ceramic lining repair layer together with the ceramic layer. The thickness of the ceramic lining repair layer after repair is 2.2mm.

[0069] S4. Preparation of epoxy resin-based composite coating:

[0070] The selected epoxy resin-based composite material powder includes the following components in weight percentage: 37% bisphenol A epoxy resin, 12% thermoplastic acrylic resin, 13% dicyandiamide, 21% calcium silicate, 9% mica powder, 4% polyurea, 3.5% polybutyl acrylate, and 0.5% benzoin. The epoxy resin-based composite material powder is obtained by mixing the above components in a mixer, then melting and extruding in an extruder, and finally crushing and grinding.

[0071] The seamless steel pipe with a ceramic lining repair layer obtained in step S3 is sandblasted and cleaned on its outer wall, and then preheated to 170°C in an induction heating furnace. The epoxy resin-based composite material powder is then sprayed on the outer wall of the steel pipe by electrostatic spraying, and heated to 226°C in an insulation furnace to melt and cross-link the epoxy resin-based composite material powder and bond it to the outer wall of the steel pipe. After insulation for 20 minutes, it is cooled and solidified to form a film, thereby obtaining an epoxy resin-based composite coating. The thickness of the epoxy resin-based composite coating is controlled to be 600um by controlling the spraying amount.

[0072] The composite seamless steel pipe for oil pipeline prepared according to the method comprises, from the inner layer to the outer layer, a ceramic lining repair layer, a metal transition layer, a steel pipe layer and an epoxy resin-based composite coating.

[0073] Comparative Example 1

[0074] This comparative example is a single-layer seamless steel pipe prepared according to the method of the present invention, and the corresponding process parameters are the same as those of Example 1. The specific steps are as follows:

[0075] S1. A solid steel pipe raw material is selected as a steel billet, which includes the following components in weight percentage: C: 0.01%, Mn: 0.48%, W: 1.71%, Ti: 0.45%, Ni: 2.6%, Cr: 8.3%, M0: 1.7%, Cu: 0.13%, Nb: 0.04%, V: 0.02%, Ti: 0.02%, Ce: 0.03%, Si: 0.4%, S: 0.001%, P: 0.01%, and the balance is Fe and other impurities.

[0076] S2. The cylindrical solid steel billet described in S1 is uniformly heated to 1247°C in a ring furnace heating furnace, and is perforated on a punching machine to form a rough pipe. After high-pressure water dephosphorization, it is continuously rolled and sized, and then heated to 974°C in a heating furnace again and soaked for 40 minutes. Quicklime is used to adjust the furnace atmosphere in the heating furnace. During soaking, the rough pipe is also filled with pig iron powder, which can reduce oxidation and burning, ensure dimensional stability, and especially prevent excessive oxide scale from forming on the inner wall; after soaking and taking out of the furnace, high-temperature water quenching is carried out, and 10% sodium hydroxide is added to the water for high-temperature water quenching. The explosion generated when sodium hydroxide crystals are precipitated is used to destroy the steam film formed during water quenching, so as to improve the cooling effect and enhance the quenching effect; during the high-temperature water quenching, the steel pipe rotates along its own axis at a rotation speed of 80r / min, and water penetrates axially through the inner wall of the steel pipe, with a water penetration of 3380m 3 / h, the outer wall is sprayed in the form of a water curtain, and the spray volume is 2910m 3 / h, and control the water temperature at 28℃, so that every part of the seamless steel pipe can be evenly cooled to prevent bending; fine sand is also mixed in the water when the inner wall is axially penetrated, and the fine sand can also break the steam film; the sodium hydroxide in the water can remove oil, and the explosion of sodium hydroxide at high temperature can also break the oxide scale that is inevitably produced on the outer and inner walls of the rough pipe, and the fine sand can knock down the broken oxide scale on the inner wall of the steel pipe under the action of water flow and steel pipe rotation. When the temperature drops to 367℃, it is changed to water mist cooling to reduce the cooling rate, which can reduce tissue stress and clean the steel pipe; finally, it is changed to air cooling to blow away excess liquid. At this time, the size of the seamless steel pipe is φ242mmx13mm.

[0077] S3. Tempering and quenching: The steel pipe is rotated slowly at a speed of 27r / min, heated to 632℃ for tempering and heat preservation for 95min to eliminate the internal stress caused by phase change during quenching of the steel pipe and optimize the quenching structure. After the heat preservation is completed, it is cooled to 405℃ in the furnace and then taken out of the furnace, and finally cooled to room temperature to obtain a single-layer seamless steel pipe for oil pipeline.

[0078] Comparative Example 2

[0079] The commercially available corrosion-resistant seamless steel pipes that have been delivered after normalizing + high-temperature tempering treatment are made of 9Cr1Mo steel.

[0080] Comparative Example 3

[0081] The composite seamless steel pipe of this comparative example is prepared according to the method of the present invention with a ceramic inner lining layer, but without repair, and an outer anti-corrosion layer is prepared. The corresponding process parameters are the same as those of Example 1, and the specific steps are as follows:

[0082] S1. A solid steel pipe raw material is selected as a steel billet, which includes the following components in weight percentage: C: 0.01%, Mn: 0.48%, W: 1.71%, Ti: 0.45%, Ni: 2.6%, Cr: 8.3%, M0: 1.7%, Cu: 0.13%, Nb: 0.04%, V: 0.02%, Ti: 0.02%, Ce: 0.03%, Si: 0.4%, S: 0.001%, P: 0.01%, and the balance is Fe and other impurities.

[0083] S2. The cylindrical solid steel billet described in S1 is uniformly heated to 1247°C in a ring furnace heating furnace, and is perforated on a punching machine to form a rough pipe. After high-pressure water dephosphorization, it is continuously rolled and sized, and then heated to 974°C in a heating furnace again and soaked for 40 minutes. Quicklime is used to adjust the furnace atmosphere in the heating furnace. During soaking, the rough pipe is also filled with pig iron powder, which can reduce oxidation and burning, ensure dimensional stability, and especially prevent excessive oxide scale from forming on the inner wall; after soaking and taking out of the furnace, high-temperature water quenching is carried out, and 10% sodium hydroxide is added to the water for high-temperature water quenching. The explosion generated when sodium hydroxide crystals are precipitated is used to destroy the steam film formed during water quenching, so as to improve the cooling effect and enhance the quenching effect; during the high-temperature water quenching, the steel pipe rotates along its own axis at a rotation speed of 80r / min, and water penetrates axially through the inner wall of the steel pipe, with a water penetration of 3380m 3 / h, the outer wall is sprayed in the form of a water curtain, and the spray volume is 2910m 3 / h, and control the water temperature at 28℃, so that every part of the seamless steel pipe can be evenly cooled to prevent bending; fine sand is also mixed in the water when the inner wall is axially penetrated, and the fine sand can also break the steam film; the sodium hydroxide in the water can remove oil, and the explosion of sodium hydroxide at high temperature can also break the oxide scale that is inevitably produced on the outer and inner walls of the rough pipe. The fine sand can knock down the broken oxide scale on the inner wall of the steel pipe under the action of water flow and steel pipe rotation, which is convenient for the subsequent preparation of the lining layer. When the temperature drops to 367℃, it is changed to water mist cooling to reduce the cooling rate, which can reduce tissue stress and clean the steel pipe; finally, it is changed to air cooling to blow away excess liquid. At this time, the size of the seamless steel pipe is φ242mmx13mm.

[0084] S3. Preparation of ceramic lining:

[0085] The selected composite thermite includes the following powders in weight proportions: 278 parts of Fe2O3, 105 parts of Al, 12 parts of CrO3, 11 parts of CuO, 26 parts of glass powder, 8 parts of cryolite, 17 parts of lithium feldspar and 26 parts of corundum. The powders are ground and mixed for 7 hours and dried at 190°C.

[0086] After the bottom of the seamless steel pipe obtained in step S2 is sealed with metal foil, the compound thermite is filled into the seamless steel pipe, and then the steel pipe is clamped on the centrifuge to make the seamless steel pipe centrifugal rotate, and the speed is controlled to be 1650r / min. The compound thermite is ignited with an energized tungsten wire or an oxyacetylene flame to cause thermite reaction, and the high-speed rotation is maintained for 5 minutes. After the thermite reaction is completed, a metal transition layer and a ceramic lining layer can be formed on the inner wall of the steel pipe from the outside to the inside. The high-density molten materials such as Fe, Cr, and Cu produced by the thermite reaction are close to the inner wall of the seamless steel pipe under the action of centrifugation, and the thin layer on the surface of the inner wall of the steel pipe is melted, and the metal transition layer is formed after cooling. The thickness of the metal transition layer is 2.2mm; the alumina molten material generated by the reaction is attached to the metal transition layer under the action of centrifugation due to its relatively small density, and a ceramic lining layer is formed on its surface after cooling, and the thickness is 1.9mm, and cracks are distributed on the obtained ceramic lining layer.

[0087] S4. Tempering and tempering treatment: The steel pipe is rotated slowly at a speed of 27r / min, heated to 632℃ for tempering and heat preservation for 95min to eliminate the internal stress caused by phase transformation during quenching of the steel pipe and optimize the quenching structure. After the heat preservation is completed, it is cooled to 405℃ in the furnace and then taken out of the furnace, and finally cooled to room temperature.

[0088] S5. Preparation of epoxy resin-based composite coating:

[0089] The selected epoxy resin-based composite material powder includes the following components in weight percentage: 38% bisphenol A epoxy resin, 13% thermoplastic acrylic resin, 11% dicyandiamide, 22% calcium silicate, 8% mica powder, 3% polyurea, 4.2% polybutyl acrylate, and 0.8% benzoin. The epoxy resin-based composite material powder is obtained by mixing the above components in a mixer, then melting and extruding in an extruder, and finally crushing and grinding.

[0090] The seamless steel pipe with a ceramic lining repair layer obtained in step S4 is sandblasted and cleaned on its outer wall, and then preheated to 160°C in an induction heating furnace. The epoxy resin-based composite material powder is then sprayed on the outer wall of the steel pipe by electrostatic spraying, and heated to 224°C in a heat-insulating furnace to melt and cross-link the epoxy resin-based composite material powder and bond it to the outer wall of the steel pipe. After heat preservation for 25 minutes, it is cooled and solidified to form a film, thereby obtaining an epoxy resin-based composite coating. The thickness of the epoxy resin-based composite coating is controlled to be 500um by controlling the spraying amount.

[0091] The composite seamless steel pipe for oil pipeline prepared according to the method comprises, from the inner layer to the outer layer, a ceramic lining layer, a metal transition layer, a steel pipe layer and an epoxy resin-based composite coating.

[0092] Comparative Example 4

[0093] This comparative example uses 20# (ANTI-H2S) seamless steel pipe with a specification of φ242mmx13mm, lined with PE plastic pipe, and covered with asphalt coating on the outside. The PE lining pipe is 2.5mm thick, and the allowable operating temperature is -20-80℃. The inner lining layer is made by induction heating and pressurized compounding, and the outer asphalt coating is 3.5mm thick.

[0094] The following performance tests were carried out on the products of the above embodiments and comparative examples.

[0095] A. Corrosion resistance test

[0096] Acid resistance test: Cut a 100mm steel pipe sample, wash and weigh it, and isolate the cross section of the steel pipe sample with paraffin. At room temperature 27°C, completely immerse it in 10% H2SO4 solution. After 5 days, take it out, wash off the corrosive substances, dry it, and weigh it again. Calculate the corrosion rate by the weight loss method.

[0097] Alkali resistance test: Cut a 100mm steel pipe sample, wash and weigh it, and isolate the cross section of the steel pipe sample with paraffin. At room temperature 27°C, completely immerse it in 10% NaOH solution. After 5 days, take it out, wash off the corrosive substances, dry it, and weigh it again. Calculate the corrosion rate by the weight loss method.

[0098] The above results are shown in Table 1, and the results are the average values ​​of multiple samples.

[0099] Table 1:

[0100]

[0101] CO2 and H2S stress corrosion cracking resistance test: refer to the high temperature and high pressure test method and four-point bending test method in GB / T4157-2017 "Laboratory test method for metal resistance to sulfide stress cracking and stress corrosion cracking in hydrogen sulfide environment", and carry out stress corrosion test in a high temperature and high pressure autoclave in a simulated environment containing CO2 and H2S. The solution is Cl - The concentration is 10x10 4 mg / L of brine, adjusted PH=4, test temperature 20℃ and 95℃, CO2 partial pressure 2.5MPa, H2S partial pressure 1.5Mpa, loading stress 50MPa applied to the specimen, maintained for 192h, removed and corrosion products, after washing, observed stress corrosion cracking on the specimen surface and determined and calculated corrosion rate.

[0102] The above results are shown in Table 2, and the results are the average values ​​of multiple samples.

[0103] Table 2:

[0104]

[0105]

[0106] The inner wall of the oil pipeline gradually becomes rough due to corrosion, so that the flow resistance of crude oil gradually increases with the increase of use time. The inner wall of each steel pipe in the embodiment has excellent corrosion resistance and will not become rough due to corrosion after long-term use, which can ensure the transportation efficiency of crude oil. The PE liner pipe softens and deforms at 95°C and is not resistant to high temperatures, while the ceramic liner repair layer has no damage and visible corrosion in a high-temperature corrosive environment. It has good heat resistance and corrosion resistance, acid and alkali corrosion resistance, CO2 and H2S stress corrosion cracking resistance. The epoxy resin-based coating on the outer layer also has excellent corrosion resistance.

[0107] B. Mechanical strength test

[0108] The tensile strength was measured by tensile test according to GB / T228.1-2010 "Metallic materials tensile test Part 1: Room temperature test method";

[0109] Refer to the determination method of GB / T6804-2008 "Determination of radial crushing strength of sintered metal bushings" and press down at a speed of 2mm / min on a compression testing machine to measure the radial crushing load of the product sample and calculate the radial crushing strength;

[0110] A load is applied vertically to the inner layer of the composite steel pipe specimen on a compression shear testing machine until the inner lining is peeled off from the steel pipe. The maximum load at this time is recorded and its compressive shear strength is calculated.

[0111] The above results are shown in Table 3, and the results are the average values ​​of multiple samples.

[0112] Table 3:

[0113]

[0114] The products of each embodiment made according to the scheme provided by this application have good mechanical strength. The compressive shear strength of the composite steel pipe reflects the bonding strength between the inner lining pipe layer and the steel pipe layer. The PE inner lining pipe is made by heating and pressurizing the inner wall of the steel pipe with hot melt adhesive, and its bonding strength is much lower than that of the ceramic inner lining pipe. The ceramic inner lining repair layer after the cracks are repaired by the repair glaze enhances the bonding force between the ceramic inner lining layer and the metal transition layer, and its compressive shear strength is also improved.

[0115] C. Surface quality test

[0116] Inner wall hardness determination: Refer to GB / T4340.1-2009 "Vickers hardness test for metallic materials, Part 1: Test method" to calculate the Vickers hardness through a hardness tester.

[0117] Scour test: Cut a 700mm long steel pipe sample and use mud containing 30% silicon oxide to scour the inner and outer surfaces at the same time. The mud scour pressure is controlled at 0.8MPa and the scour lasts for 12h. After the test, the mass loss rate is measured and calculated.

[0118] The above results are shown in Table 4, and the results are the average values ​​of multiple samples.

[0119] Table 4:

[0120]

[0121] The inner wall of the oil pipeline becomes rough due to fluid scouring, which will gradually increase the flow resistance of crude oil with the increase of use time. The ceramic lining layer with cracks has a large friction resistance and is easily worn in the sediment scouring test. The repaired ceramic lining repair layer in each embodiment is smooth and crack-free, and has excellent anti-scouring and wear resistance. It will not become rough due to fluid scouring after long-term use, and can ensure the transportation efficiency of crude oil. In the scouring test, the mass loss of comparative example 4 is mainly due to the shedding of the asphalt layer. The asphalt layer is thick and easy to peel off. The epoxy resin-based composite coating is thin and has good bonding strength with the outer wall of the steel pipe, and is not easy to peel off.

Claims

1. A method for manufacturing a composite seamless steel pipe for oil pipeline, characterized in that: The following steps are involved: S1. A solid steel pipe raw material is selected as a steel billet, which includes the following components in weight percentage: C: 0.01-0.02%, Mn: 0.43%-0.51%, W: 1.55-1.74%, Ti: 0.42-0.48%, Ni: 2.4-3.1%, Cr: 7.5%-8.5%, Mo: 1.4%-1.8%, Cu: 0.12-0.16%, Nb: 0.02-0.04%, V: 0.01-0.02%, Ti: 0.01-0.03%, Ce: 0.02-0.04%, Si: 0.38-0.43%, S<0.002%, P<0.015%, and the balance is Fe and other impurities; S2. The steel billet described in S1 is uniformly heated to 1230-1265°C, perforated to form a rough pipe, dephosphorized with high-pressure water, continuously rolled and sized, and then heated to 960-980°C again and soaked for 30-50 minutes before high-temperature water quenching. During the high-temperature water quenching, the steel pipe is rotated along its own axis, water is axially penetrated through the inner wall of the steel pipe, and the outer wall is sprayed in the form of a water curtain. When the temperature drops to 350-380°C, it is changed to water mist cooling, and finally to air cooling; S3. Preparation of ceramic lining repair layer: Fill the seamless steel pipe obtained in step S2 with a compound thermite, centrifugally rotate the seamless steel pipe, ignite the compound thermite, and cause a thermite reaction. After the thermite reaction, a metal transition layer and a ceramic lining layer can be formed on the inner wall of the steel pipe from the outside to the inside in sequence; heat the repair glaze to make it in a liquid molten state, and after the thermite reaction is completed and before the seamless steel pipe is completely cooled, hot spray the molten repair glaze on the inner wall of the steel pipe to cover the ceramic lining layer, slowly rotate the steel pipe to make the molten glaze level and penetrate into the cracks of the ceramic layer, keep the steel pipe rotating slowly, glaze firing and heat preservation at 620-640℃ for 80-110min, cool with the furnace after the insulation is completed, and after a certain temperature is taken out of the furnace, introduce compressed gas into the steel pipe to maintain a certain pressure in the pipe, cool to room temperature to form a glaze, and form a ceramic lining repair layer together with the ceramic lining layer; S4. Preparation of epoxy resin-based composite coating: The seamless steel pipe with ceramic lining repair layer obtained in step S3 is sandblasted and cleaned on its outer wall, and then preheated, and then epoxy resin-based composite material powder is sprayed on the outer wall of the steel pipe by electrostatic spraying, and the epoxy resin-based composite material powder is heated and insulated to melt and cross-link, and bonded to the outer wall of the steel pipe, and the epoxy resin-based composite coating is obtained after cooling and curing to form a film; the epoxy resin-based composite material powder includes the following components in weight percentage: 36%-40% bisphenol A epoxy resin, 12%-16% thermoplastic acrylic resin, 9%-14% dicyandiamide, 20%-25% calcium silicate, 7%-10% mica powder, 2%-4% polyurea, 3%-5% polybutyl acrylate, and 0.5%-1% benzoin; In step S2, "heating to 960-980°C and soaking for 30-50 minutes" before quenching is carried out in a heating furnace, and quicklime is used to adjust the atmosphere in the furnace. During soaking, the rough pipe is also filled with pig iron powder; 8%-12% sodium hydroxide is added to the water for high-temperature water quenching, and fine sand is also mixed in the axial water of the inner wall; in step S2, during high-temperature water quenching, the rotation speed of the steel pipe along its own axis is 75-85r / min, and the spraying volume of the outer wall water curtain is 2850-2950m 3 / h, the axial water penetration of the inner wall is 3200-3450m 3 / h, and control the water temperature at 20-35℃; In step S3, the repair glaze includes the following ingredients: boric oxide, calcium borate, sodium tripolyphosphate, sodium borate, silicon oxide and molybdenum trioxide; the weight ratio of the components of the repair glaze is boric oxide: calcium borate: sodium tripolyphosphate: sodium borate: silicon oxide: molybdenum trioxide = 22-24: 6.7-7.4: 1-1.4: 5.6-6.8: 17-19: 7.6-8.8; the heating melting temperature of the repair glaze is 800-830°C, and the rotation of the steel pipe after hot spraying the repair glaze The speed is 20-30r / min. After the glaze firing and heat preservation are completed, the temperature when the furnace is cooled and taken out of the furnace is 390-410°C. The pressure in the tube maintained by the compressed gas is 4-6MPa. The composite thermite includes the following powders in parts by weight: 274-288 parts of Fe2O3, 100-110 parts of Al, 5-15 parts of CrO3, 9-14 parts of CuO, 19-33 parts of glass powder, 5-12 parts of cryolite, 15-24 parts of lithium feldspar and 19-33 parts of corundum. In step S4, the steel pipe is preheated to 150-170°C, the heating and insulation temperature is 220-227°C, and the insulation time is 15-30 minutes.

2. A composite seamless steel pipe for oil pipeline, characterized in that: It is prepared according to the method of claim 1, and comprises, from the inner layer to the outer layer, a ceramic lining repair layer, a metal transition layer, a steel pipe layer and an epoxy resin-based composite coating.