A method for preparing nitrogen-doped graphene-supported iron single-atom catalyst

By preparing nitrogen-doped graphene-supported iron single-atom catalysts, the problem of poor ORR performance of existing catalytic materials is solved, and efficient application in energy devices such as fuel cells is achieved.

CN116031415BActive Publication Date: 2024-11-29CHANGZHOU INST OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211621782.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2024-11-29
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

The poor performance of existing catalytic materials in quad-electron oxygen reduction reaction (ORR) limits the high-performance applications of energy devices such as fuel cells.

Method used

A catalyst with two-dimensional nanosheet structure and porous characteristics is prepared by using the preparation method of nitrogen-doped graphene-supported iron single-atom catalyst, through mixing and stirring, hydrothermal heat, centrifugal drying and high-temperature calcination.

Benefits of technology

It exhibits good ORR catalytic activity in alkaline electrolytes, with a half-wave potential reaching 0.91V, a current density of 5.5mA·cm-2, and is low in cost and easy to synthesize, with good application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116031415B_ABST
    Figure CN116031415B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a nitrogen-doped graphene-supported iron single-atom catalyst, comprising the following steps of selecting carbon nitride, tannic acid, an iron source, 4-diethylamino-salicylaldehyde, an ethanol solution and deionized water; carbon nitride is dispersed in deionized water by ultrasonic wave; an iron source is added to the deionized water containing tannic acid; 4-diethylamino-salicylaldehyde is added to the ethanol solution; solution one, solution two and solution three are mixed and stirred to obtain a uniformly dispersed solution; the uniformly dispersed solution is hydrothermally treated by a hydrothermal kettle; the hydrothermal solution is centrifugally dried to obtain a Fe / C3N4@TA-salicylaldehyde precursor; and a nitrogen-doped graphene-supported iron single-atom catalyst is obtained after high-temperature calcination of the Fe / C3N4@TA-salicylaldehyde precursor in a nitrogen atmosphere. The present invention shows excellent ORR activity by preparing a nitrogen-doped graphene-supported iron single-atom catalyst by modifying C3N4 with tannic acid, and has good oxygen reduction catalytic effect and good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanomaterials, and in particular to a method for preparing a nitrogen-doped graphene-supported iron single-atom catalyst. Background Art

[0002] The growing global energy demand and environmental issues require more advanced energy conversion and storage devices and technologies. Renewable energy conversion and storage systems have been widely explored to alleviate the energy crisis and environmental issues. Fuel cells and metal-air batteries are considered promising candidates due to their high theoretical energy density, high energy efficiency and zero carbon emissions. However, designing high-performance electrocatalysts to accelerate the sluggish kinetics of the four-electron oxygen reduction reaction (ORR) remains one of the key challenges for the large-scale commercialization of these technologies.

[0003] In recent decades, carbon-based materials have attracted widespread attention due to their good electrocatalytic activity, low price, stable performance and environmental friendliness. However, the electrocatalytic activity of carbon-based materials is much lower than that of precious metal-based materials, which limits their use in actual energy devices. Based on this, a lot of research work has been invested in improving the electrocatalytic activity of carbon-based materials. Among them, doping heteroatoms in the carbon skeleton can effectively change the electron distribution, increase the electrochemical active sites, and thus increase the electrocatalytic activity of carbon-based materials; in addition, the electrocatalytic activity can also be improved by rationally controlling the morphology and crystal characteristics of carbon-based materials and increasing the electron and material transfer channels.

[0004] Cathode oxygen reduction (ORR) is a slow kinetic process. In the currently commercial PEMFC, the cathode oxygen reduction catalyst is Pt / C or PtRu / C. Platinum reserves are scarce and expensive. According to surveys, the cost of platinum accounts for about 56% of the entire fuel cell device. In addition, platinum-based catalysts have poor stability. Platinum nanoparticles will dissolve and partially agglomerate in a corrosive environment of high temperature and high humidity, resulting in a reduction in active sites and specific surface area, and a decrease in oxygen reduction activity; at the same time, contact with carbon monoxide (CO) will poison the platinum-based catalyst. Studies have shown that even a small amount of CO (10-20ppm) will cause a significant decrease in the activity of platinum-based catalysts, resulting in poor ORR performance of the catalytic material. These problems have hindered the large-scale application of proton exchange membrane fuel cells. Summary of the invention

[0005] In order to solve the technical problem of poor ORR performance of existing catalytic materials, the present invention provides a method for preparing a nitrogen-doped graphene-supported iron single-atom catalyst.

[0006] The present invention is achieved through the following technical solutions:

[0007] A method for preparing a nitrogen-doped graphene-supported iron single-atom catalyst comprises the following steps:

[0008] S1, select carbon nitride as nitrogen source, tannic acid as carbon source, ferric acetylacetonate or ferric phthalocyanine as iron source, 4-diethylamino-salicylaldehyde, ethanol solution and deionized water;

[0009] S2, dispersing carbon nitride in deionized water by ultrasonic wave to obtain a uniformly dispersed solution 1; adding an iron source to the deionized water containing tannic acid, mixing and stirring to obtain a uniform solution 2; adding 4-diethylamino-salicylaldehyde to the ethanol solution, mixing and stirring to obtain a uniform solution 3;

[0010] S3, mixing solution 1, solution 2 and solution 3 and stirring to obtain a uniformly dispersed solution;

[0011] S4, subjecting the uniformly dispersed solution in S2 to hydrothermal treatment in a hydrothermal reactor;

[0012] S5, centrifugally drying the uniformly dispersed solution after hydrothermal treatment to obtain Fe / C3N4@TA-salicylaldehyde precursor;

[0013] S6. The Fe / C3N4@TA-salicylaldehyde precursor is calcined at high temperature in a nitrogen atmosphere to obtain a nitrogen-doped graphene-supported iron single atom catalyst.

[0014] Furthermore, the amounts of tannic acid, carbon nitride, iron source, 4-diethylamino-salicylic aldehyde, deionized water, and ethanol in S1 are as follows: tannic acid 0.8-0.9 g; carbon nitride 480-500 mg; iron source 19-21 mg; 4-diethylamino-salicylic aldehyde 0.5-0.7 g; deionized water 58-60 mL; ethanol 24-26 mL.

[0015] Furthermore, the amounts of tannic acid, carbon nitride, iron source, 4-diethylamino-salicylic aldehyde, deionized water, and ethanol in S1 are as follows: 0.8506 g tannic acid; 500 mg carbon nitride; 20 mg iron source; 0.6 g 4-diethylamino-salicylic aldehyde; 60 mL deionized water; and 25 mL ethanol.

[0016] Furthermore, the amounts of tannic acid, carbon nitride, iron source, 4-diethylamino-salicylic aldehyde, deionized water, and ethanol in S1 are as follows: 0.8 g tannic acid; 480 mg carbon nitride; 19 mg iron source; 0.5 g 4-diethylamino-salicylic aldehyde; 58 mL deionized water; and 24 mL ethanol.

[0017] Furthermore, the amounts of tannic acid, carbon nitride, iron source, 4-diethylamino-salicylic aldehyde, deionized water, and ethanol in S1 are as follows: 0.9 g tannic acid; 490 mg carbon nitride; 21 mg iron source; 0.7 g 4-diethylamino-salicylic aldehyde; 59 mL deionized water; and 26 mL ethanol.

[0018] Furthermore, the ultrasonic dispersion time in S2 is 60 minutes, the temperature is room temperature, and the mixing time is 60 minutes, the temperature is room temperature.

[0019] Furthermore, the hydrothermal temperature in S4 is 120°C and the time is 10 h.

[0020] Furthermore, the temperature of centrifugal drying in S5 is 60°C.

[0021] Furthermore, the high temperature calcination temperature in S6 is 900°C and the time is 2h.

[0022] The advantages and positive effects of the present invention are: in the method of the present invention, the nitrogen-doped graphene-supported iron single-atom catalyst (Fe / NG) is first obtained by mixing, stirring, hydrothermal, centrifugal drying, and then calcining, and the obtained material has a two-dimensional nanosheet structure, has obvious porous characteristics, and is conducive to electrolyte diffusion. No template assistance is required in the preparation process, no toxic gas is released, the raw materials are easily available, the cost is low, and it is easy to synthesize.

[0023] When used as an electrocatalyst for ORR in an alkaline electrolyte (0.1 M potassium hydroxide), the catalyst prepared by the product of the present invention has good catalytic activity. When the limiting current density is 5.5 mA·cm-2, the half-wave potential of the ORR reaction is 0.91 V. The present invention prepares a nitrogen-doped graphene-supported iron single-atom catalyst by modifying C3N4 with tannic acid, which exhibits excellent ORR activity and has good oxygen reduction catalytic effect and good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is a TEM image of the nitrogen-doped graphene-supported iron single-atom catalyst (Fe / NG) prepared in Example 1 of the present invention;

[0025] Figure 2 (a) is a polarization curve diagram of Fe / NG obtained after calcination of the Fe / C3N4@TA-salicylaldehyde precursor prepared in Example 1 and Fe / C3N4@TA (Comparative Example 1), Fe / C3N4@salicylaldehyde (Comparative Example 2) and Fe / C3N4 (Comparative Example 3) prepared in Comparative Examples 1-3;

[0026] Figure 2(b) is a half-wave potential column comparison chart of Fe / NG obtained after calcining the Fe / C3N4@TA-salicylaldehyde precursor prepared in Example 1 and Fe / C3N4@TA (Comparative Example 1), Fe / C3N4@salicylaldehyde (Comparative Example 2) and Fe / C3N4 (Comparative Example 3) prepared in Comparative Examples 1-3. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention are within the scope of protection of the present invention.

[0028] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.

[0029] The experimental methods in the following examples without specifying specific conditions are usually measured according to national standards; if there is no corresponding national standard, it is carried out according to the general international standards or the standard requirements proposed by relevant enterprises. Unless otherwise specified, all parts are by weight and all percentages are by weight.

[0030] Embodiment 1

[0031] A method for preparing a nitrogen-doped graphene-supported iron single-atom catalyst comprises the following steps:

[0032] Step 1. Select carbon nitride (C3N4) as the nitrogen source, tannic acid as the carbon source, ferric acetylacetonate as the iron source, 4-diethylamino-salicylaldehyde, ethanol solution and deionized water, wherein the amounts of tannic acid, carbon nitride, ferric acetylacetonate, 4-diethylamino-salicylaldehyde, deionized water and ethanol are as follows: 0.8506 g tannic acid; 500 mg carbon nitride; 20 mg ferric acetylacetonate; 0.6 g 4-diethylamino-salicylaldehyde; 60 mL deionized water; 25 mL ethanol.

[0033] Step 2: Add 500 mg of carbon nitride to 40 mL of deionized water and disperse it by ultrasound at room temperature for 60 minutes to obtain a uniformly dispersed solution 1; add 20 mg of ferric acetylacetonate to 40 mL of deionized water containing 0.8506 g of tannic acid, mix and stir for 60 minutes at room temperature (25° C.) to obtain a uniform solution 2; add 0.6 g of 4-diethylamino-salicylaldehyde to 25 mL of ethanol solution, mix and stir for 60 minutes at room temperature to obtain a uniform solution 3;

[0034] Step 3, mixing solution 1, solution 2 and solution 3 and stirring to obtain a uniformly dispersed solution;

[0035] Step 4: subjecting the uniformly dispersed solution in step 3 to hydrothermal treatment in a hydrothermal kettle, wherein the hydrothermal temperature is 120° C. and the time is 10 h;

[0036] Step 5: centrifuge the uniformly dispersed solution after hydrothermal treatment twice for centrifugal drying, take the precipitate and put it into an oven for drying at 60°C to obtain Fe / C3N4@TA-salicylaldehyde precursor;

[0037] Step 6: calcining the Fe / C3N4@TA-salicylaldehyde precursor at high temperature in a nitrogen atmosphere to obtain a nitrogen-doped graphene-supported iron single atom catalyst, wherein the high temperature calcination temperature is 900° C. and the time is 2 h.

[0038] Figure 1 This is a TEM image of the nitrogen-doped graphene-supported iron single-atom catalyst (Fe / NG) prepared in Example 1. It can be seen from the image that the material is a two-dimensional nanosheet structure and there are no obvious metal nanoparticles.

[0039] Embodiment 2

[0040] A method for preparing a nitrogen-doped graphene-supported iron single-atom catalyst comprises the following steps:

[0041] Step 1, select carbon nitride as the nitrogen source, tannic acid as the carbon source, iron phthalocyanine as the iron source, 4-diethylamino-salicylaldehyde, ethanol solution and deionized water, wherein the amounts of tannic acid, carbon nitride, iron phthalocyanine, 4-diethylamino-salicylaldehyde, deionized water and ethanol are as follows: 0.8 g tannic acid; 480 mg carbon nitride; 19 mg iron phthalocyanine; 0.5 g 4-diethylamino-salicylaldehyde; 58 mL deionized water; 24 mL ethanol.

[0042] Step 2: Add 480 mg of carbon nitride to 18 mL of deionized water and disperse it by ultrasound at room temperature for 60 min to obtain a uniformly dispersed solution 1; add 19 mg of iron phthalocyanine to 40 mL of deionized water containing 0.8 g of tannic acid, mix and stir for 60 min at room temperature (25° C.) to obtain a uniform solution 2; add 0.5 g of 4-diethylamino-salicylic aldehyde to 24 mL of ethanol solution, mix and stir for 60 min at room temperature to obtain a uniform solution 3;

[0043] Step 3, mixing solution 1, solution 2 and solution 3 and stirring to obtain a uniformly dispersed solution;

[0044] Step 4: subjecting the uniformly dispersed solution in step 3 to hydrothermal treatment in a hydrothermal kettle, wherein the hydrothermal temperature is 120° C. and the time is 10 h;

[0045] Step 5: centrifuge the uniformly dispersed solution after hydrothermal treatment twice for centrifugal drying, take the precipitate and put it into an oven for drying at 60°C to obtain Fe / C3N4@TA-salicylaldehyde precursor;

[0046] Step 6: calcining the Fe / C3N4@TA-salicylaldehyde precursor at high temperature in a nitrogen atmosphere to obtain a nitrogen-doped graphene-supported iron single atom catalyst, wherein the high temperature calcination temperature is 900° C. and the time is 2 h.

[0047] Embodiment 3

[0048] A method for preparing a nitrogen-doped graphene-supported iron single-atom catalyst comprises the following steps:

[0049] Step 1. Select carbon nitride as the nitrogen source, tannic acid as the carbon source, ferric acetylacetonate as the iron source, 4-diethylamino-salicylaldehyde, ethanol solution and deionized water, wherein the amounts of tannic acid, carbon nitride, ferric acetylacetonate, 4-diethylamino-salicylaldehyde, deionized water and ethanol are as follows: the amounts of tannic acid, carbon nitride, iron source, 4-diethylamino-salicylaldehyde, deionized water and ethanol are as follows: 0.9 g tannic acid; 490 mg carbon nitride; 21 mg ferric acetylacetonate; 0.7 g 4-diethylamino-salicylaldehyde; 59 mL deionized water; 26 mL ethanol.

[0050] Step 2: Add 490 mg of carbon nitride to 19 mL of deionized water and disperse it by ultrasound at room temperature for 60 min to obtain a uniformly dispersed solution 1; add 21 mg of ferric acetylacetonate to 40 mL of deionized water containing 0.9 g of tannic acid, mix and stir for 60 min at room temperature (25° C.) to obtain a uniform solution 2; add 0.7 g of 4-diethylamino-salicylaldehyde to 26 mL of ethanol solution, mix and stir for 60 min at room temperature to obtain a uniform solution 3;

[0051] Step 3, mixing solution 1, solution 2 and solution 3 and stirring to obtain a uniformly dispersed solution;

[0052] Step 4: subjecting the uniformly dispersed solution in step 3 to hydrothermal treatment in a hydrothermal kettle, wherein the hydrothermal temperature is 120° C. and the time is 10 h;

[0053] Step 5: centrifuge the uniformly dispersed solution after hydrothermal treatment twice for centrifugal drying, take the precipitate and put it into an oven for drying at 60°C to obtain Fe / C3N4@TA-salicylaldehyde precursor;

[0054] Step 6: calcining the Fe / C3N4@TA-salicylaldehyde precursor at high temperature in a nitrogen atmosphere to obtain a nitrogen-doped graphene-supported iron single atom catalyst, wherein the high temperature calcination temperature is 900° C. and the time is 2 h.

[0055] Comparative Example 1

[0056] The difference between this comparative example and Example 1 is that no 4-diethylamino-salicylaldehyde and ethanol mixed solution is added, and the specific preparation process is as follows:

[0057] (1) Weigh 500 mg of C3N4 and add it to 40 ml of deionized water. Ultrasonicate the mixture at room temperature for 60 min until a uniformly dispersed solution is obtained;

[0058] Weigh 20 mg of ferric acetylacetonate and 0.8506 g of tannic acid and add them to 20 ml of deionized water, and stir the mixture at room temperature for 60 min until a uniform solution is obtained;

[0059] (2) adding the obtained uniformly mixed solution of ferric acetylacetonate and tannic acid to the C3N4 solution;

[0060] (3) placing the obtained uniformly mixed solution into a hydrothermal kettle and hydrothermally heating it at 120° C. for 10 h;

[0061] (4) centrifuging the liquid after hydrothermal treatment twice, taking the precipitate and drying it in an oven at 60 °C to obtain Fe / C3N4@TA precursor;

[0062] (5) calcining the dried precursor at 900° C. for 2 h under the protection of nitrogen to obtain Fe / NG-1.

[0063] Comparative Example 2

[0064] The difference between this comparative example and Example 1 is that tannic acid is not added, and the specific preparation process is as follows:

[0065] (1) Weigh 500 mg of C3N4 and add it to 40 ml of deionized water. Ultrasonicate the mixture at room temperature for 60 min until a uniformly dispersed solution is obtained;

[0066] Weigh 20 mg of ferric acetylacetonate and add it to 20 ml of deionized water. Stir the mixture for 60 min until a homogeneous solution is obtained.

[0067] Weigh 0.6 g of 4-diethylamino-salicylaldehyde and add it to 25 ml of ethanol solution, and sonicate the mixture at room temperature for 60 min until a uniform solution is obtained;

[0068] (2) adding the obtained ferric acetylacetonate uniformly mixed solution to the C3N4 solution; adding the obtained salicylaldehyde solution to the C3N4 solution;

[0069] (3) placing the obtained uniformly mixed solution into a hydrothermal kettle and hydrothermally heating it at 120° C. for 10 h;

[0070] (4) centrifuging the liquid after hydrothermal treatment twice, taking the precipitate and drying it in an oven at 60°C to obtain Fe / C3N4@salicylaldehyde precursor;

[0071] (5) calcining the dried precursor at 900° C. for 2 h under the protection of nitrogen to obtain Fe / NG-2.

[0072] Comparative Example 3

[0073] The difference between this comparative example and Example 1 is that no tannic acid and salicylaldehyde solution are added, and the specific preparation process is as follows:

[0074] (1) Weigh 500 mg of C3N4 and add it to 40 ml of deionized water. Ultrasonicate the mixture at room temperature for 60 min until a uniformly dispersed solution is obtained;

[0075] Weigh 20 mg of ferric acetylacetonate and add it to 20 ml of deionized water. Stir the mixture for 60 min until a homogeneous solution is obtained.

[0076] (2) adding the obtained uniformly mixed solution of ferric acetylacetonate to the C3N4 solution;

[0077] (3) placing the obtained uniformly mixed solution into a hydrothermal kettle and hydrothermally heating it at 120° C. for 10 h;

[0078] (4) centrifuging the liquid after hydrothermal treatment twice, taking the precipitate and drying it in an oven at 60°C to obtain a Fe@C3N4 precursor;

[0079] (5) calcining the dried precursor at 900° C. for 2 h under the protection of nitrogen to obtain Fe / NG-3.

[0080] The final products of the above Example 1 and Comparative Examples 1-3 were respectively used as catalysts in the oxygen reduction system.

[0081] The electrochemical properties were determined using a conventional three-electrode system: Hg / HgCl2 as the reference electrode, a carbon rod as the counter electrode, and a catalyst-modified glassy carbon electrode as the working electrode.

[0082] Preparation of working electrode: 5 mg of the samples of Example 1 and Comparative Examples 1-3 were mixed with 485 μL of isopropanol and 15 μL of naphthol respectively and ultrasonicated for 1 h to form a uniform mixed solution; 10 μL of the mixed solution was dropped onto the surface of the glassy carbon electrode and naturally air-dried to obtain a glassy carbon electrode modified with a catalyst.

[0083] The electrochemical performance tests were all completed using a Pine electrochemical workstation. The electrochemical performance tests were carried out in 0.1M KOH solution at a fixed scan rate (5mV·s-1).

[0084] The electrochemical performances of Example 1 and Comparative Examples 1-3 are as follows: Figure 2 As shown, Figure 2 (a) is a comparison diagram of polarization curves of oxygen reduction reaction. Figure 2 (b) is a comparison diagram of oxygen reduction half-wave potential. The Fe / NG obtained by calcining the Fe / C3N4@TA-salicylaldehyde precursor of Example 1 of the present invention is used as a catalyst. When the oxygen reduction performance of Fe / NG is tested in a 0.1M KOH solution, when the current density is 5.5mA·cm-2, the half-wave potential of ORR is 0.91V, which is higher than the half-wave potentials of Comparative Examples 1-3. Compared with the relevant literature reported, the material of the present invention also has good oxygen reduction performance, proving that the material of the present invention can be used as an effective catalyst for oxygen reduction.

[0085] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a nitrogen-doped graphene-supported iron single-atom catalyst, characterized in that: The following steps are involved: S1, select carbon nitride as nitrogen source, tannic acid as carbon source, ferric acetylacetonate or ferric phthalocyanine as iron source, 4-diethylamino-salicylaldehyde, ethanol solution and deionized water; S2, dispersing carbon nitride in deionized water by ultrasonic wave to obtain a uniformly dispersed solution 1; adding an iron source to the deionized water containing tannic acid, mixing and stirring to obtain a uniform solution 2; adding 4-diethylamino-salicylaldehyde to the ethanol solution, mixing and stirring to obtain a uniform solution 3; S3, mixing solution 1, solution 2 and solution 3 and stirring to obtain a uniformly dispersed solution; S4, subjecting the uniformly dispersed solution in S2 to hydrothermal treatment in a hydrothermal reactor; S5, centrifuging and drying the uniformly dispersed solution after hydrothermal treatment to obtain Fe / C3N4@TA-salicylaldehyde precursor; S6, calcining the Fe / C3N4@TA-salicylaldehyde precursor at high temperature in a nitrogen atmosphere to obtain a nitrogen-doped graphene-supported iron single atom catalyst; The hydrothermal temperature in S4 is 120° C. and the time is 10 h.

2. The method for preparing the nitrogen-doped graphene-supported iron single-atom catalyst according to claim 1, characterized in that: The amounts of tannic acid, carbon nitride, iron source, 4-diethylamino-salicylaldehyde, deionized water, and ethanol in S1 are as follows: 0.8-0.9 g tannic acid; 480-500 mg carbon nitride; 19-21 mg iron source; 0.5-0.7 g 4-diethylamino-salicylaldehyde; 58-60 mL deionized water; and 24-26 mL ethanol.

3. The method for preparing the nitrogen-doped graphene-supported iron single-atom catalyst according to claim 2, characterized in that: The amounts of tannic acid, carbon nitride, iron source, 4-diethylamino-salicylic aldehyde, deionized water, and ethanol in S1 are as follows: 0.8506 g tannic acid; 500 mg carbon nitride; 20 mg iron source; 0.6 g 4-diethylamino-salicylic aldehyde; 60 mL deionized water; and 25 mL ethanol.

4. The method for preparing the nitrogen-doped graphene-supported iron single-atom catalyst according to claim 2, characterized in that: The amounts of tannic acid, carbon nitride, iron source, 4-diethylamino-salicylaldehyde, deionized water, and ethanol in S1 are as follows: 0.8 g tannic acid; 480 mg carbon nitride; 19 mg iron source; 0.5 g 4-diethylamino-salicylaldehyde; 58 mL deionized water; and 24 mL ethanol.

5. The method for preparing the nitrogen-doped graphene-supported iron single-atom catalyst according to claim 2, characterized in that: The amounts of tannic acid, carbon nitride, iron source, 4-diethylamino-salicylaldehyde, deionized water, and ethanol in S1 are as follows: 0.9 g tannic acid; 490 mg carbon nitride; 21 mg iron source; 0.7 g 4-diethylamino-salicylaldehyde; 59 mL deionized water; and 26 mL ethanol.

6. The method for preparing the nitrogen-doped graphene-supported iron single-atom catalyst according to claim 1, characterized in that: The ultrasonic dispersion time in S2 is 60 minutes, the temperature is room temperature, and the mixing time is 60 minutes, the temperature is room temperature.

7. The method for preparing the nitrogen-doped graphene-supported iron single-atom catalyst according to claim 1, characterized in that: The drying temperature in S5 is 60°C.

8. The method for preparing the nitrogen-doped graphene-supported iron single-atom catalyst according to claim 1, characterized in that: The temperature of high temperature calcination in S6 is 900℃ and the time is 2h.

Citation Information

Cited By

  • Oxygen reduction reaction catalyst with axial nitrogen coordination iron monatomic structure and low-temperature preparation method thereof

    CN121687984A