A pyrolysis gasoline hydrogenation catalyst and preparation method thereof
By using alumina carriers to support molecular sieves and Group VIB and Group VIII metals in pyrolysis gasoline hydrogenation catalysts, the problems of easy deactivation and high cost of existing catalysts are solved, and efficient and low-cost olefin hydrogenation is achieved.
Patent Information
- Application Number
- CN202111278933.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-31
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-10-31
AI Technical Summary
When existing pyrolysis gasoline hydrogenation catalysts remove olefin compounds that are prone to coking, high nickel catalysts are prone to deactivation, precious metal catalysts are costly, and it is difficult to control dispersion and acid content, leading to efficiency and cost problems.
Alumina is used as a carrier to load molecular sieves and Group VIB metals (such as molybdenum, tungsten) and Group VIII metals (such as nickel, cobalt). Through hydrothermal treatment and reduction treatment, the molecular sieve is loaded on the outer surface of the catalyst to improve the dispersion and dispersion of active metals. Acid content, a catalyst with high hydrogenation saturation activity and low price can be prepared.
It improves the hydrogenation activity of the catalyst and the utilization rate of the molecular sieve, reduces the cost, and enhances the stability of the catalyst through the molecular sieve loading technology, avoids the aggregation of active metals, and achieves efficient olefin hydrogenation.
Smart Images

Figure 909237DEST_PATH_IMAGE002 
Figure DEST_PATH_IMAGE001
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil hydrogenation, and in particular to a pyrolysis gasoline hydrogenation catalyst and a preparation method thereof. Background Art
[0002] With the saturation of the refined oil market and the shortage of ethylene raw materials, more and more oil refineries have begun to build or expand ethylene cracking units. Pyrolysis gasoline is the largest by-product of ethylene cracking products, mainly composed of C5-C9 compounds, with a total aromatic content of up to 72%-78%, and contains olefins, diolefins and other compounds that are easy to coke. Pyrolysis gasoline usually uses a two-stage hydrogenation method to remove impurities. The first stage hydrogenation is mainly used to remove olefins and other compounds that are easy to coke, and the second stage hydrogenation is mainly used to remove impurity compounds such as sulfides.
[0003] CN201410193225.3 discloses a method for hydrofining pyrolysis gasoline. The method comprises the following steps: catalyzing and hydrogenating the pyrolysis gasoline raw material in the presence of a nickel-based catalyst having relatively uniformly dispersed active components, wherein the nickel-based catalyst comprises a composite carrier composed of an aluminum oxide-titanium oxide composite and ZSM-5 and nickel oxide supported on the composite carrier, and the content of nickel oxide in the nickel-based catalyst is 12%-20% based on the weight of the catalyst; and hydrofining the pyrolysis gasoline is performed by controlling the reaction conditions during the reaction process to obtain a downstream refined raw material with a low diene value and a low bromine value.
[0004] CN201310585233.8 discloses a pyrolysis gasoline hydrogenation catalyst and its preparation method. The catalyst is mainly composed of an alumina carrier, an active component palladium, and a catalytic promoter metal component of titanium, cerium, lanthanum, and yttrium. The catalytic promoter metal component is introduced from a soluble metal salt and coated on the carrier surface by a hydrothermal synthesis method to form a coating layer, and then the active component palladium is loaded on the coating layer. The mass of the coating layer accounts for 1% to 20% of the mass of the carrier, and the content of the active component palladium is 0.15% to 0.45% of the total mass of the carrier after coating.
[0005] In order to remove olefinic coking compounds in pyrolysis gasoline, high nickel or precious metal catalysts are mainly used. However, high nickel catalysts are prone to aggregation and deactivation, while precious metal catalysts are expensive. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention starts from the olefin hydrogenation reaction mechanism and prepares a pyrolysis gasoline hydrogenation catalyst by means of improving the dispersion of active metals and increasing the acid content. The catalyst has high hydrogenation saturation activity and is low in price.
[0007] In order to achieve the above technical objectives, the technical solution of the present invention is as follows:
[0008] The technical purpose of the first aspect of the present invention is to provide a cracking gasoline hydrogenation catalyst, which uses alumina as a carrier, on which a molecular sieve and an active component are loaded, the active component being a VIB group metal and a VIII group metal. Based on the total weight of the catalyst, the molecular sieve accounts for 1-14%, preferably 2-10%, and more preferably 3-7%; the VIB group metal accounts for 2-15%, preferably 3-8%, and the VIII group metal accounts for 10-30%, preferably 15-25%; the molecular sieve is loaded on the outer surface of the catalyst.
[0009] Furthermore, the molecular sieve loaded on the outer surface of the catalyst is the molecular sieve loaded on the metal of Group VIB, and / or the molecular sieve loaded on the metal of Group VIII, and / or the molecular sieve loaded on alumina.
[0010] Furthermore, the molecular sieve is at least one selected from Y-type molecular sieve, ZSM-5 molecular sieve, β-type molecular sieve and MCM-41 molecular sieve.
[0011] Furthermore, the Group VIB metal is metal molybdenum and / or metal tungsten, and the Group VIII metal is metal nickel and / or metal cobalt.
[0012] The technical purpose of the second aspect of the present invention is to provide a method for preparing the above-mentioned pyrolysis gasoline hydrogenation catalyst, comprising the following steps:
[0013] (1) impregnating an alumina carrier with an impregnation solution containing a Group VIB metal, and obtaining a catalyst precursor A through drying and calcining;
[0014] (2) The catalyst precursor A is impregnated with an impregnation solution containing a Group VIII metal salt and an organic additive, and then dried and calcined to obtain a catalyst precursor B.
[0015] (3) The catalyst precursor B is mixed with the molecular sieve precursor and subjected to hydrothermal treatment, followed by drying, calcination and reduction treatment to obtain the pyrolysis gasoline hydrogenation catalyst.
[0016] Furthermore, the impregnation solution of the VIB group metal in step (1) is a phosphate or ammonium salt solution of the VIB group metal, and its preparation method is well known to those skilled in the art, and is carried out by equal volume impregnation or supersaturated impregnation. The VIB group metal is preferably Mo and / or W.
[0017] Furthermore, the drying conditions of step (1) are: drying temperature 90-200°C, drying time 3-6 hours. The roasting conditions are: roasting temperature 300-500°C, roasting time 3-6 hours.
[0018] Furthermore, the impregnation solution containing the Group VIII metal in step (2) is a nitrate, acetate or sulfate solution of the Group VIII metal, etc., and an equal volume impregnation method can be adopted. The Group VIII metal is Ni and / or Co.
[0019] Furthermore, the organic auxiliary agent in step (2) is an alcohol or organic acid containing hydroxyl and / or carboxyl groups, wherein the number of carbon atoms is 3-10. Specifically, it is at least one selected from ethylene glycol, glycerol, butanediol, pentanediol, acetic acid, citric acid, malonic acid, succinic acid and glutaric acid.
[0020] Furthermore, the drying conditions of step (2) are: drying temperature 90-200°C, drying time 3-6 hours. The roasting conditions are: roasting temperature 300-500°C, roasting time 3-6 hours.
[0021] Furthermore, the molecular sieve precursor in step (3) is a gel formed by mixing a silicon source and / or an aluminum source, a precipitant, a template and water, and its preparation method is well known to those skilled in the art, and adopts a precipitation or sol-gel method. The silicon source is generally one or more of sodium silicate, tetraethyl orthosilicate, silica sol and chromatography silica gel; the aluminum source is generally one or more of sodium aluminate, aluminum hydroxide and pseudo-boehmite; the precipitant is selected from at least one of sodium hydroxide, ammonia water and potassium hydroxide; the template is selected from one or more of hexadecyltrimethylammonium bromide, ethylenediamine, n-butylamine, tetrapropylammonium bromide, ethanol, tetraethylammonium hydroxide, tetraethylammonium bromide, triethylamine, di-n-propylamine, diisopropylamine and methylcellulose.
[0022] Furthermore, the hydrothermal treatment conditions in step (3) are: temperature of 90-200° C., preferably 120-200° C.; pressure of 0.1-2.0 MPa; pH of 7.5-9.0; and time of 5-48 hours.
[0023] Furthermore, the drying conditions of step (3) are: drying temperature 90-200°C, drying time 3-6 hours. The roasting conditions are: roasting temperature 300-500°C, roasting time 3-6 hours.
[0024] Furthermore, the reduction treatment conditions in step (3) are as follows: in a hydrogen atmosphere, the reduction temperature is 200-500° C., the reduction pressure is 2.0-4.0 MPa, and the reduction time is 3-10 hours.
[0025] The technical purpose of the third aspect of the present invention is to provide the application of the pyrolysis gasoline hydrogenation catalyst, which is used in the olefin hydrogenation treatment process of pyrolysis gasoline.
[0026] Compared with the prior art, the catalyst of the present invention has the following advantages:
[0027] (1) The molecular sieve is added to the pyrolysis gasoline hydrogenation catalyst of the present invention, and the molecular sieve is loaded on the outer surface of the catalyst instead of being kneaded with the carrier. On the one hand, it is beneficial to increase the contact surface between the molecular sieve and the active metal, and at the same time, it is beneficial to load the molecular sieve on the active site of the active metal, so as to give full play to the ability of the molecular sieve to provide H protons and improve the hydrogenation activity of the catalyst; on the other hand, it increases the utilization rate of the molecular sieve, thereby reducing the amount of the molecular sieve used and reducing the cost of the catalyst.
[0028] (2) The present invention obtains a cracked gasoline olefin hydrogenation catalyst by first loading a VIB group metal onto a carrier, then loading a VIII group metal, and then loading a molecular sieve, and then performing a reduction treatment; wherein the VIB group metal loaded onto the carrier can modify the high active sites on the carrier surface, weaken the interaction between the carrier and the VIII group metal, and improve the dispersion of the VIII group metal; meanwhile, the VIB group metal interacts with the VIII group metal, and can hinder the aggregation of the VIII group metal.
[0029] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0030] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.
[0031] The catalyst composition provided by the present invention can be characterized by combining inductively coupled plasma ICP and XPS energy spectrum. First, the total content of Group VIB metals and the total content of Group VIII metals in the catalyst are characterized by ICP, and then the content of metal elements with different valence states in the catalyst is quantitatively characterized by XPS energy spectrometer.
[0032] Example 1
[0033] (1) The ammonium heptamolybdate solution was impregnated into the alumina support, followed by drying at 110°C for 3 hours and calcining at 550°C for 3 hours to obtain catalyst precursor A.
[0034] (2) Impregnating the nickel nitrate and glycerol solution into the catalyst precursor A prepared in step (1), and then drying at 110°C for 3 hours and calcining at 350°C for 3 hours to obtain catalyst precursor B.
[0035] (3) Sodium hydroxide, silica sol, sodium aluminate and ethylenediamine are added to deionized water, wherein the molar ratio of each component is n(SiO2):n(Al2O3):n(Na2O):n(ethylenediamine):n(H2O)=13:1:5.5:3.5:180, and stirred to form a uniform sol, i.e., a precursor of Y molecular sieve, and then mixed with the catalyst precursor B prepared in step (2), and then hydrothermally treated at 150°C, 1.0 MPa, pH=8.0 for 10 h; then filtered, washed three times with deionized water, and then dried at 120°C for 3 h, calcined at 450°C for 3 h, and then reduced with H2 at 400°C, 2.0 MPa for 3 h to obtain catalyst C-1.
[0036] The weight percentages of the components in catalyst C-1 are: MoO3 is 4.3%, NiO is 15.1%, Y molecular sieve is 4.1%, and the rest is alumina carrier.
[0037] Example 2
[0038] (1) The ammonium heptamolybdate solution was impregnated into the alumina support, followed by drying at 110°C for 3 hours and calcining at 450°C for 3 hours to obtain catalyst precursor A.
[0039] (2) Impregnating nickel nitrate and ethylene glycol solution into the catalyst precursor A prepared in step (1), and then drying at 110°C for 3 hours and calcining at 250°C for 3 hours to obtain catalyst precursor B.
[0040] (3) Sodium hydroxide, silica sol, sodium aluminate and ethylenediamine are added to deionized water, wherein the molar ratio of each component is n(SiO2):n(Al2O3):n(Na2O):n(n-butylamine):n(H2O)=21:1:6:7:200, and stirred to form a uniform sol, i.e., a precursor of the ZSM-5 molecular sieve, which is then mixed with the catalyst precursor B prepared in step (2), and then hydrothermally treated at 150°C, 1.0 MPa, and pH=8.0 for 10 h; then filtered, washed three times with deionized water, dried at 120°C for 3 h, calcined at 550°C for 3 h, and then reduced with H2 at 400°C and 2.0 MPa for 3 h to obtain catalyst C-2.
[0041] The weight percentages of the components in catalyst C-2 are: MoO3 is 4.6%, NiO is 16.8%, ZSM-5 molecular sieve is 4.8%, and the rest is alumina carrier.
[0042] Example 3
[0043] (1) The ammonium heptamolybdate solution was impregnated into the alumina support, followed by drying at 110°C for 3 hours and calcining at 450°C for 3 hours to obtain catalyst precursor A.
[0044] (2) Impregnating nickel nitrate and ethylene glycol solution into the catalyst precursor A prepared in step (1), and then drying at 110°C for 3 hours and calcining at 450°C for 3 hours to obtain catalyst precursor B.
[0045] (3) Sodium aluminate and sodium hydroxide were dissolved in deionized water, and then tetraethylammonium bromide was added. The mixture was stirred vigorously, and silica sol was slowly added dropwise. The mixture was aged for 3 h, wherein the molar ratio of each component was n(SiO2):n(Al2O3):n(Na2O):n(tetraethylammonium bromide):n(H2O)=26:1:6:5.5:280, to form a precursor of a β-type molecular sieve. The precursor was then mixed with the catalyst precursor B prepared in step (2), and then hydrothermally treated at 150°C, 1.0 MPa, and pH=8.0 for 10 h. The catalyst was then filtered, washed three times with deionized water, dried at 120°C for 3 h, calcined at 550°C for 3 h in a nitrogen atmosphere, and then reduced with H2 at 400°C and 2.0 MPa for 3 h to obtain catalyst C-3.
[0046] The weight percentages of the components in catalyst C-3 are: 3.1% MoO3, 17.8% NiO, 5.0% β-type molecular sieve, and the rest is alumina carrier.
[0047] Example 4
[0048] (1) The ammonium heptamolybdate solution was impregnated into the alumina support, followed by drying at 150°C for 3 hours and calcining at 500°C for 3 hours to obtain catalyst precursor A.
[0049] (2) Impregnating the nickel nitrate and glycerol solution into the catalyst precursor A prepared in step (1), and then drying at 90°C for 3 hours and calcining at 250°C for 3 hours to obtain the catalyst precursor B.
[0050] (3) Hexadecyltrimethylammonium bromide and sodium hydroxide are mixed and then added to deionized water. After stirring, ethyl orthosilicate is added dropwise to the mixed solution. After stirring for 30 minutes, the molar ratio of each component is n(SiO2):n(Na2O):n(hexadecyltrimethylammonium bromide):n(H2O)=13:2.5:3.5:250 to form an MCM-41 molecular sieve precursor, which is then mixed with the catalyst precursor B prepared in step (2), and then hydrothermally treated at 150°C, 1.0 MPa, and pH=8.0 for 10 hours; then filtered, washed three times with deionized water, dried at 120°C for 3 hours, calcined at 500°C for 3 hours in a nitrogen atmosphere, and then reduced with H2 at 400°C and 2.0 MPa for 3 hours to obtain catalyst C-4.
[0051] The weight percentages of the components in catalyst C-4 are: 3.7% MoO3, 13.2% NiO, 3.4% MCM-41 molecular sieve, and the rest is alumina carrier.
[0052] Example 5
[0053] (1) The ammonium heptamolybdate solution was impregnated into the alumina support, followed by drying at 120°C for 3 hours and calcining at 450°C for 3 hours to obtain catalyst precursor A.
[0054] (2) The cobalt nitrate and citric acid solution is impregnated into the catalyst precursor A prepared in step (1), and then dried at 80°C for 3 hours and calcined at 350°C for 3 hours to obtain the catalyst precursor B.
[0055] (3) Sodium hydroxide, silica sol, sodium aluminate and ethylenediamine are added to deionized water, wherein the molar ratio of each component is n(SiO2):n(Al2O3):n(Na2O):n(ethylenediamine):n(H2O)=13:1:5.5:3.5:180, and stirred to form a uniform sol, i.e., a precursor of Y molecular sieve, and then mixed with the catalyst precursor B prepared in step (2), and then hydrothermally treated at 150°C, 1.0 MPa, and pH=8.0 for 10 h; then filtered, washed three times with deionized water, dried at 120°C for 3 h, calcined at 550°C for 3 h in a nitrogen atmosphere, and then reduced with H2 at 400°C and 2.0 MPa for 3 h to obtain catalyst C-5.
[0056] The weight percentages of the components in catalyst C-5 are: MoO3 is 7.8%, CoO is 13.9%, Y-type molecular sieve is 4.8%, and the rest is alumina carrier.
[0057] Example 6
[0058] (1) The ammonium metatungstate solution was impregnated into the alumina carrier, and then dried at 110°C for 3 hours and calcined at 520°C for 3 hours to obtain catalyst precursor A.
[0059] (2) Impregnating nickel nitrate and ethylene glycol solution into the catalyst precursor A prepared in step (1), then drying at 90°C for 3 hours and calcining at 200°C for 3 hours to obtain catalyst precursor B.
[0060] (3) Sodium hydroxide, silica sol, sodium aluminate and ethylenediamine are added to deionized water, wherein the molar ratio of each component is n(SiO2):n(Al2O3):n(Na2O):n(n-butylamine):n(H2O)=21:1:6:7:200, and stirred to form a uniform sol, i.e., a precursor of the ZSM-5 molecular sieve, which is then mixed with the catalyst precursor B prepared in step (2), and then hydrothermally treated at 150°C, 1.0 MPa, and pH=8.0 for 10 h; then filtered, washed three times with deionized water, dried at 120°C for 3 h, calcined at 550°C for 3 h in a nitrogen atmosphere, and then reduced with H2 at 400°C and 2.0 MPa for 3 h to obtain catalyst C-6.
[0061] The weight percentages of the components in catalyst C-6 are: WO3 is 7.8%, NiO is 15.2%, ZSM-5 molecular sieve is 4.8%, and the rest is alumina carrier.
[0062] Example 7
[0063] (1) The ammonium metatungstate solution was impregnated into the alumina carrier, and then dried at 120°C for 3 hours and calcined at 450°C for 3 hours to obtain catalyst precursor A.
[0064] (2) Impregnating the cobalt nitrate and glycerol solution into the catalyst precursor A prepared in step (1), and then drying at 100°C for 3 hours and calcining at 350°C for 3 hours to obtain the catalyst precursor B.
[0065] (3) Sodium hydroxide, silica sol, sodium aluminate and ethylenediamine are added to deionized water, wherein the molar ratio of each component is n(SiO2):n(Al2O3):n(Na2O):n(ethylenediamine):n(H2O)=13:1:5.5:3.5:180, and stirred to form a uniform sol, i.e., a precursor of Y molecular sieve, and then mixed with the catalyst precursor B prepared in step (2), and then hydrothermally treated at 150°C, 1.0 MPa, pH=8.0 for 10 h; then filtered, washed three times with deionized water, dried at 120°C for 3 h, calcined at 520°C for 3 h in a nitrogen atmosphere, and then reduced with H2 at 400°C, 2.0 MPa for 3 h to obtain catalyst C-7.
[0066] The weight percentages of the components in catalyst C-7 are: WO3 is 7.9%, CoO is 16.2%, Y-type molecular sieve is 4.8%, and the rest is alumina carrier.
[0067] Comparative Example 1
[0068] (1) Mix Y-type molecular sieve with alumina powder, nitric acid, starch and deionized water, wherein the mass ratio of Y-type molecular sieve: alumina powder: nitric acid: starch: deionized water is 4.8:95.2:4:3:60, and then knead and extrude into strips, and then dry at 80°C for 10 hours and calcine at 650°C for 3 hours to obtain a modified alumina carrier.
[0069] (2) The ammonium heptamolybdate solution was impregnated into the modified alumina support in step (1), followed by drying at 120°C for 3 hours and calcining at 450°C for 3 hours to obtain catalyst precursor A.
[0070] (3) The nickel nitrate solution was impregnated into the catalyst precursor A prepared in step (2), followed by drying at 90°C for 3 hours, calcining at 250°C for 3 hours, and then reducing with H2 at 400°C and 2.0 MPa for 3 hours to obtain catalyst DC-1.
[0071] The weight percentages of the components in the catalyst DC-1 are: 7.7% MoO3, 4.2% nickel oxide, 4.6% Y molecular sieve, and the rest is aluminum oxide.
[0072] Comparative Example 2
[0073] (1) Mix Y-type molecular sieve with alumina powder, nitric acid, starch and deionized water, wherein the mass ratio of Y-type molecular sieve: alumina powder: nitric acid: starch: deionized water is 8:92:4:3:60, and then knead and extrude into strips, and then dry at 80°C for 10 hours and calcine at 650°C for 3 hours to obtain a modified alumina carrier.
[0074] (2) A mixed solution of phosphomolybdic acid and nickel nitrate was impregnated into the modified alumina carrier prepared in step (1), followed by drying at 120°C for 3 hours, calcining at 450°C for 3 hours, and then reducing with H2 at 400°C and 2.0 MPa for 3 hours to obtain catalyst DC-2.
[0075] The weight percentages of the components in the catalyst DC-2 are: MoO3 is 8.1%, NiO is 4.8%, the Y molecular sieve content is 4.8%, and the rest is alumina.
[0076] The proportion of zero-valent Group VIII metals in the total Group VIII metals was analyzed for the C-1 to C-7 catalysts prepared in the above examples and the DC-1 to DC-2 catalysts prepared in the comparative examples. The analysis results are shown in Table 1.
[0077] Table 1.
[0078]
[0079] Example 8
[0080] This example illustrates the activity of the catalyst provided by the present invention for hydrogenation of olefins in pyrolysis gasoline.
[0081] The raw oil used for evaluation is coking naphtha provided by a refinery of Sinopec, and its main properties are as follows: diolefin content is 15wt%, olefin content is 25wt%. A 200mL fixed bed hydrogenation device was used to evaluate the olefin hydrogenation activity of catalysts C-1 to C-7 and comparative examples DC-1 to DC-2. The evaluation reaction conditions are: operating pressure 3.0MPa, reaction temperature 90℃, hydrogen / oil volume ratio 100:1, volume space velocity 2.0h -1 The evaluation results are shown in Table 2.
[0082] Table 2.
[0083]
[0084] As can be seen from Table 2, the pyrolysis gasoline hydrogenation catalyst of the present invention has a very high olefin hydrogenation saturation activity.
Claims
1. A pyrolysis gasoline hydrogenation catalyst, characterized in that: The catalyst uses alumina as a carrier, on which molecular sieves and active components are loaded. The active components are metals of Group VIB and metals of Group VIII. Based on the total weight of the catalyst, the molecular sieve accounts for 1-14%, the metals of Group VIB account for 2-15%, and the metals of Group VIII account for 10-30%. The molecular sieve is loaded on the outer surface of the catalyst; The pyrolysis gasoline hydrogenation catalyst is prepared by the following method: (1) impregnating an alumina carrier with an impregnation solution containing a Group VIB metal, and obtaining a catalyst precursor A through drying and calcination; (2) impregnating a catalyst precursor A with an impregnation solution containing a Group VIII metal salt and an organic additive, and then drying and calcining to obtain a catalyst precursor B; (3) The catalyst precursor B is mixed with the molecular sieve precursor and subjected to hydrothermal treatment, followed by drying, calcination and reduction treatment to obtain the pyrolysis gasoline hydrogenation catalyst.
2. The catalyst according to claim 1, characterized in that Based on the total weight of the catalyst, the molecular sieve accounts for 2-10%, the Group VIB metal accounts for 3-8%, and the Group VIII metal accounts for 15-25%.
3. The catalyst according to claim 2, characterized in that Based on the total weight of the catalyst, the molecular sieve accounts for 3-7%.
4. The catalyst according to claim 1, characterized in that The molecular sieve loaded on the outer surface of the catalyst is loaded on the metal of Group VIB, and / or the molecular sieve is loaded on the metal of Group VIII, and / or the molecular sieve is loaded on alumina.
5. The catalyst according to claim 1, characterized in that The molecular sieve is at least one selected from Y-type molecular sieve, ZSM-5 molecular sieve, β-type molecular sieve and MCM-41 molecular sieve.
6. The catalyst according to claim 1, characterized in that The VIB group metal is metal molybdenum and / or metal tungsten, and the VIII group metal is metal nickel and / or metal cobalt.
7. The method for preparing the pyrolysis gasoline hydrogenation catalyst according to claim 1, comprising the following steps: (1) impregnating an alumina carrier with an impregnation solution containing a Group VIB metal, and obtaining a catalyst precursor A through drying and calcination; (2) impregnating a catalyst precursor A with an impregnation solution containing a Group VIII metal salt and an organic additive, and then drying and calcining to obtain a catalyst precursor B; (3) The catalyst precursor B is mixed with the molecular sieve precursor and subjected to hydrothermal treatment, followed by drying, calcination and reduction treatment to obtain the pyrolysis gasoline hydrogenation catalyst.
8. The preparation method according to claim 7, characterized in that: The impregnation solution of the Group VIB metal in step (1) is a phosphate or ammonium salt solution of the Group VIB metal, and the Group VIB metal is Mo and / or W.
9. The preparation method according to claim 7, characterized in that: The drying conditions of step (1) are: drying temperature 90-200°C, drying time 3-6 hours; the roasting conditions are: roasting temperature 300-500°C, roasting time 3-6 hours.
10. The preparation method according to claim 7, characterized in that: The impregnation solution containing the Group VIII metal in step (2) is a nitrate, acetate or sulfate solution of the Group VIII metal, and the Group VIII metal is Ni and / or Co.
11. The preparation method according to claim 7, characterized in that: The organic auxiliary agent in step (2) is at least one selected from ethylene glycol, propylene glycol, butylene glycol, pentanediol, acetic acid, citric acid, malonic acid, succinic acid and glutaric acid.
12. The preparation method according to claim 7, characterized in that: The molecular sieve precursor described in step (3) is obtained by mixing a silicon source and / or an aluminum source, a precipitant, a template and water and then adopting a precipitation or sol-gel method.
13. The preparation method according to claim 7, characterized in that: The hydrothermal treatment conditions in step (3) are: temperature of 90-200° C., pressure of 0.1-2.0 MPa, pH of 7.5-9.0, and time of 5-48 hours.
14. The preparation method according to claim 13, characterized in that: The temperature of the hydrothermal treatment in step (3) is 120-200°C.
15. Use of the pyrolysis gasoline hydrogenation catalyst according to claim 1 in an olefin hydrogenation treatment process of pyrolysis gasoline.