A process for producing low-shrinkage wool tops
Through semi-merceration treatment and twisting stretching process, combined with puffing agent and resin treatment, the problem of high shrinkage in wool strip production is solved, the production of low shrinkage wool strips is achieved, and the anti-shrinkage performance and economic value of the ready-made garments are improved. , and reduce environmental pollution.
Patent Information
- Application Number
- CN202310237504.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-03-14
AI Technical Summary
The existing wool strip production process leads to a high shrinkage rate, which leads to easy felt shrinkage after washing. The chemical treatment method pollutes the environment, making it difficult to achieve the production of low shrinkage wool strips.
Using semi-merceration and twisting stretching technology, the overlap and traction of the scales are controlled by peeling and changing the angle of the wool scales, combining puffing agent and resin treatment, reducing the shrinkage of the wool strips, and bubbling and alkaline through multi-stage sinks Water cleaning improves anti-shrink performance.
The low shrinkage rate of wool strips (4% to 5%) is achieved, which improves the anti-shrinkage performance and economic value of the ready-made garments, and reduces environmental pollution.
Abstract
Description
[Technical field]
[0001] The invention relates to the technical field of wool top production, in particular to a wool top production process with low shrinkage. [Background technology]
[0002] Wool is an important raw material for the textile industry. It has the advantages of good elasticity, strong moisture absorption and good warmth retention. Wool is a slender solid cylinder in a curly shape. The fiber structure is divided into three layers, namely the scale layer, the cortex layer and the medulla layer. The scale layer is the surface layer of wool. Its growth has a certain direction, from the hair root to the hair tip. Each scale is connected to the cortex layer at one end of the hair root and is stretched outward at the other end, covering and connecting one piece after another. The coverage density of scales on wool varies greatly depending on the wool variety. The finer the wool, the more scales there are, the longer the overlapping part is, and the scales are mostly ring-shaped. The thicker the wool, the fewer scales there are, the shorter the overlapping length is, and the scales are mostly corrugated and fish-scale-shaped, overlapping and covering each other. Because the scale layer is stretched out and protruded, if the friction between the fibers is increased, they will restrain each other to produce a felting effect, and the cohesion will be strengthened under hot and humid conditions. This characteristic of wool makes it easy for the finished clothes to be felted and shrunk after washing, resulting in a reduction in the size of the clothes (commonly known as clothes shrinkage). The shrinkage rate of normal wool strips produced by the production process in the prior art is about 20%, and the shrinkage rate of shrink-proof wool strips produced by the production process in the prior art is 7% to 8%. Therefore, how to improve the production process in the prior art to produce a low-shrinkage wool strip (i.e., a shrinkage rate of 4% to 5%) has become a difficult problem that technicians in this field have always wanted to overcome.
[0003] Please refer to Chinese Patent Publication No. CN1239525A, which discloses a method for continuously processing wool, which mainly uses chemical treatment to treat the wool net to improve the shrinkage resistance of the wool. The defect of this chemical treatment method is that a large amount of wastewater needs to be discharged after the chemical treatment, which greatly pollutes the environment.
[0004] Therefore, it is necessary to provide a low-shrinkage wool top production process that solves the above-mentioned technical problems. [Summary of the invention]
[0005] In order to solve the above problems, the purpose of the present invention is to provide a process for producing low-shrinkage wool tops with good shrinkage resistance.
[0006] To achieve the above object, the technical scheme adopted by the present invention is: a low shrinkage wool top production process, comprising the following steps: A, raw wool and wool mixing: select wool with uniform length, the average length of wool is about 65-80mm; B, wool washing: the wool is pre-opened, then the wool is cleaned, washed and dried; C, top making: use a wool machine to open and sew the wool, the amount of wool oil used is controlled to 0.6% of the wool mass, the amount of antistatic agent used is controlled to 1.2% of the wool mass, and then the wool is stewed for more than 12 hours; D, wool combing: use a wool type cotton combing machine for production, the sew speed is controlled at 80-100 meters / minute, and the sew weight is controlled at 20 grams / meter; E, pin combing 1: select an imported GN6 pin combing machine for merging, the sew speed is 45- 55 m / min, feed 6 combs to form slivers, the drafting multiple is set to 6 times, and the weight of the sliver is controlled at 20 g / m; F, gilling 2: select imported gilling machine GN6 for merging, the sliver speed is 45-55 m / min, feed 6 combs 1 to form slivers, the drafting multiple is set to 8 times, and the weight of the sliver is controlled at 15 g / m; G, combing: use a wool-type combing machine, feed 20 combs 2 to form slivers, the hair loss rate is controlled at 8%-9%, the cylinder speed is 150 clamps / min, the gauge is controlled at 35-40mm, the hair feeding amount is controlled at 6mm / time, and the weight of the sliver is controlled at 20 g / m; H, gilling 3: select imported gilling machine GN6 for merging, the sliver speed is 45-55 m / min, feed 6 combs After the strips are formed, the drafting multiples are set to 6 times, and the strip weight is controlled at 20 grams / meter; I. Pin combing 4: Select the imported pin combing machine GN6 for merging, the strip speed is 45-55 meters / minute, and 6 pin combs 3 are fed to form strips, the drafting multiples are set to 6 times, and the strip weight is controlled at 20 grams / meter; J. Soaking: The strips formed after the pin combing 4 are soaked in a five-level water tank, the water temperature in the five-level water tank is 40 degrees, the soaking time of the first level water tank is 6 minutes, the soaking time of the second level water tank is 6 minutes, the soaking time of the third level water tank is 6 minutes, the soaking time of the fourth level water tank is 5 minutes, and the soaking time of the fifth level water tank is 5 minutes; K. Water pressing: The soaked wool strips are pressed by rotating the upper and lower water tank rollers; L. Semi-silk Polishing: Put the wool strips after water pressing into the reaction water tank for semi-mercerization treatment, remove the scales, and then wash and filter with alkaline water; M, twisting and stretching: twist and squeeze the wool strips after washing and filtering, and add 1.5% of the wool strips by weight of the bulking agent, use a drawing machine to stretch it 1.2 times to open the wool scales and change the angle, and then untwist it; N, semi-mercerization: The wool strips after stretching and untwisting are semi-mercerized again, so that the scales at the root of the wool after stretching can be removed; O, washing: wash and filter with alkaline water again; P, softening treatment: add 1% of the wool strips by weight of the resin to the surface of the wool strips washed and filtered with alkaline water for softening treatment; Q, drying and shaping: dry and shape the softened wool strips to obtain low shrinkage wool strips.
[0007] Compared with the prior art, the present invention has the following beneficial effects: the present invention can peel off about half of the scales in the wool strips through semi-mercerization treatment, and through twisting, stretching and adding a bulking agent, not only can the wool scales be fully opened and the angles changed, but the scales can also be softened. Therefore, when the semi-mercerization treatment is performed again, the roots of the scales left over from the first semi-mercerization treatment can be removed. Through this process improvement, low-shrinkage wool strips (i.e., the shrinkage rate is 4% to 5%) can be produced. After the low-shrinkage wool strips are finally made into finished garments, the shrinkage resistance is greatly improved, thereby increasing the economic value. [Specific implementation method]
[0008] The following is a further detailed description of the low shrinkage wool strip production process of the present invention through specific embodiments.
[0009] A process for producing low-shrinkage wool tops, comprising the following steps: A. mixing raw wool and wool: selecting wool of uniform length, wherein the average length of the wool is about 65-80 mm; B. washing wool: pre-opening the wool, then washing and drying the wool; C. making wool tops: using a wool-combing machine to open and commingle the wool, controlling the amount of wool-combing oil to be 0.6% of the wool mass, controlling the amount of antistatic agent to be 1.2% of the wool mass, and then stewing the wool for more than 12 hours; D. combing wool: using a wool-type cotton combing machine for production, controlling the sliver output speed to be 80-100 m / min, and controlling the sliver output weight to be 20 g / m; E. pin combing 1: selecting an imported GN6 pin combing machine for merging, the sliver output speed to be 45-55 m / min, feeding 6 combed wools to form slivers, and drawing times The number of times is set to 6 times, and the weight of the sliver is controlled at 20 g / m; F, gilling 2: imported gilling machine GN6 is selected for merging, the sliver speed is 45-55 m / min, 6 gilling 1 are fed to form slivers, the drafting multiples are set to 8 times, and the weight of the sliver is controlled at 15 g / m; G, combing: a wool-type combing machine is used, 20 gilling 2 are fed to form slivers, the hair loss rate is controlled at 8%-9%, the cylinder speed is 150 clamps / min, the gauge is controlled at 35-40mm, the hair feeding amount is controlled at 6mm / time, and the weight of the sliver is controlled at 20 g / m; H, gilling 3: imported gilling machine GN6 is selected for merging, the sliver speed is 45-55 m / min, 6 gilling 1 are fed to form slivers, the drafting multiples are set to 6 times, and the weight of the sliver is controlled at 15 g / m. The weight of the wool strips is controlled at 20 g / m; I. Pin combing 4: imported pin combing machine GN6 is selected for merging, the sliver output speed is 45-55 m / min, 6 pin combs 3 are fed to form slivers, the drafting multiples are set to 6 times, and the sliver output weight is controlled at 20 g / m; J. Soaking: the slivers formed after pin combing 4 are soaked through a five-level water tank, the water temperature in the five-level water tank is 40 degrees, the soaking time of the first-level water tank is 6 minutes, the soaking time of the second-level water tank is 6 minutes, the soaking time of the third-level water tank is 6 minutes, the soaking time of the fourth-level water tank is 5 minutes, and the soaking time of the fifth-level water tank is 5 minutes; K. Water pressing: the soaked wool strips are pressed by rotating the upper and lower water tank rollers; L. Semi-mercerizing: the wool strips after water pressing are placed in a reaction water tank for semi-mercerizing treatment, The wool is descaled and then washed and filtered with alkaline water to remove the acid residue after chlorine treatment; M, twisting and stretching: the washed and filtered wool strips are twisted and squeezed, and 1.5% of the wool strip mass is added with a swelling agent to soften the scales. The wool strips are stretched 1.2 times with a drawing machine to open the wool scales and change the angle, and then untwisted; N, semi-mercerized: the stretched and untwisted wool strips are semi-mercerized again, so that the scales at the root of the stretched wool can be removed; O, washing: the alkaline water is washed and filtered again; P, softening treatment: the surface of the wool strips washed and filtered with alkaline water is softened with 1% of the wool strip mass of resin; Q, drying and shaping: the softened wool strips are dried and shaped to obtain low shrinkage wool strips.
[0010] In summary, the present invention can peel off about half of the scales in the wool strips through semi-mercerization treatment, and through twisting, stretching and adding a bulking agent, not only can the wool scales be fully opened and the angles changed, but the scales can also be softened. Therefore, when the semi-mercerization treatment is performed again, the roots of the scales left after the first semi-mercerization treatment can be removed (about 95% of the roots of the scales can be removed). Through this process improvement, low-shrinkage wool strips (i.e., the shrinkage rate is 4% to 5%) can be produced. After the low-shrinkage wool strips are finally made into finished garments, the anti-shrinkage performance is greatly improved, thereby increasing the economic value.
[0011] The above-mentioned embodiments are only illustrative of the principles and effects of the invention, as well as some embodiments of its application, and are not intended to limit the invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept of the invention, and all of these belong to the protection scope of the invention.
Claims
1. A process for producing low shrinkage wool tops, characterized in that: The steps include: A. Raw wool and wool blending: Choose wool of uniform length, with an average length of 65~80mm; B. Wool washing: The wool is pre-loosened, then cleaned, washed and dried; C. Top making: Use wool-making machine to loosen the wool, the amount of wool-making oil used is controlled at 0.6% of the wool mass, the amount of antistatic agent used is controlled at 1.2% of the wool mass, and then stew the wool for more than 12 hours; D. Combing: Use wool-type carding machine to produce, the sliver speed is controlled at 80-100 m / min, and the sliver weight is controlled at 20 g / m; E. Gilling 1: Imported GN6 gilling machine is selected for merging, the sliver output speed is 45-55 m / min, 6 combed hairs are fed into slivers, the drafting multiples are set to 6 times, and the sliver weight is controlled at 20 g / m; F. Pin comb 2: Imported pin comb machine GN6 is selected for merging, the sliver delivery speed is 45-55 m / min, 6 pin combs 1 are fed into the slivers, the drafting multiples are set to 8 times, and the sliver weight is controlled at 15 g / m; G. Combing: Use wool type combing machine, feed 20 needles to form slivers, the hair removal rate is controlled at 8%-9%, the cylinder speed is 150 times / min, the gauge is controlled at 35-40mm, the hair feeding amount is controlled at 6mm / time, and the weight of the sliver is controlled at 20g / m; H. Gilling 3: Imported gilling machine GN6 is selected for merging, the sliver delivery speed is 45-55 m / min, 6 slivers are fed into the sliver after combing, the drafting multiples are set to 6 times, and the sliver weight is controlled at 20 g / m; I. Pin comb 4: Imported pin comb machine GN6 is selected for merging, the sliver delivery speed is 45-55 m / min, 6 pin combs 3 are fed into slivers, the drafting multiples are set to 6 times, and the sliver weight is controlled at 20 g / m; J. Soaking: Soak the strips after combing 4 times in a five-level water tank. The water temperature in the five-level water tank is 40 degrees. The soaking time in the first-level water tank is 6 minutes, the soaking time in the second-level water tank is 6 minutes, the soaking time in the third-level water tank is 6 minutes, the soaking time in the fourth-level water tank is 5 minutes, and the soaking time in the fifth-level water tank is 5 minutes. K. Water pressing: The soaked wool strips are passed through the upper and lower water tanks with rotating rollers to press water; L. Semi-mercerization: Put the wool strips after water pressing into the reaction water tank for semi-mercerization treatment, descaling treatment, and then alkaline water washing and filtration; M. Twisting and stretching: twist and squeeze the cleaned and filtered wool strips, add 1.5% bulking agent by weight of the wool strips, stretch them 1.2 times with a drafting machine to open the wool scales and change the angle, and then untwist them; N. Semi-mercerized: The wool strips after stretching and untwisting are semi-mercerized again, so that the scales at the root of the stretched wool can be removed; O. Cleaning: Clean and filter with alkaline water again; P. Softening treatment: Add 1% of the mass of the wool strip to the surface of the wool strip washed and filtered with alkaline water for softening treatment; Q. Drying and shaping: Dry and shape the softened wool strips to obtain low shrinkage wool strips.
Citation Information
Cited By
Wool top pretreatment equipment for cotton spinning
CN120174559A