Environmentally friendly wet-mixed mortar based on waste slurry from a pipe pile factory and preparation method thereof
Through the synergy between the modified pipe pile waste slurry and mortar additives, an efficient wet mixing mortar is prepared, which solves the problems of rapid water loss and poor flexibility of wet mixing mortar, and promotes the recycling and utilization of pipe pile waste slurry , realizes the preparation of high mechanical properties and environmentally friendly moisturizing mortar.
Patent Information
- Application Number
- CN202211732875.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-30
AI Technical Summary
The existing wet-mixed mortar has problems such as fast water loss, poor flexibility, high brittleness, low strength and poor crack resistance during construction. At the same time, the environmental pollution problem of waste slurry in the pipe pile factory needs to be solved urgently.
The environmentally friendly and moisturizing mortar is used based on the waste slurry of pipe pile factory. Through the synergy of modified pipe pile waste slurry, mortar additives and mortar additives, wet-mixed mortar that thickens, water retention and improves mechanical properties is prepared, and porous ceramic particles are used. , nano-sodium aluminosilicate, chlorinated polyvinyl chloride CPVC resin and other materials are modified and combined with quartz sand, natural river sand, gravel powder and fillers to form an efficient wet-mixed mortar.
The plastic maintenance time of wet-mixed mortar is extended, its operability and mechanical properties are improved, the bonding strength between materials is enhanced, the problems of fast water loss, poor flexibility and low strength are solved, and the pipe pile waste slurry is realized. recycle and use.
Smart Images

Figure BDA0004031653870000121 
Figure BDA0004031653870000122 
Figure BDA0004031653870000131
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wet-mixed mortar, and particularly relates to an environmentally friendly wet-mixed mortar based on waste slurry from a pipe pile factory and a preparation method thereof. Background Art
[0002] With the improvement of economic level, the construction industry has also developed, and the requirements for the basic materials used in the construction industry, such as concrete and mortar, have become increasingly higher. Among them, wet-mixed mortar, as a traditional construction material, is produced and stored on site, and then laid on the base material. The construction is relatively simple, but it is also accompanied by many defects, such as rapid water loss, poor flexibility, high brittleness, low strength, and poor crack resistance.
[0003] Concrete pipe piles are widely used in the current construction industry. They can achieve cost savings in the construction process, achieve good construction results, and play an important role. However, a series of waste slurries are produced during the production of pipe piles, which will pollute the environment and become a major problem that needs to be solved urgently. Therefore, in order to better develop and utilize pipe pile waste slurry, it is necessary to study a use scheme of pipe pile waste slurry suitable for wet-mixed mortar preparation, and use pipe pile waste slurry to produce wet-mixed mortar with excellent effects, so as to promote the recycling of waste materials in the construction industry. Summary of the invention
[0004] In view of the above problems, the object of the present invention is to provide an environmentally friendly wet-mix mortar based on waste slurry from a pipe pile factory and a preparation method thereof.
[0005] The technical contents of the present invention are as follows:
[0006] The present invention provides an environmentally friendly wet-mixed mortar based on waste slurry from a pipe pile factory, wherein the environmentally friendly wet-mixed mortar comprises the following components: cement, modified waste slurry from pipe pile factories, quartz sand, natural river sand, crushed stone powder, filler, mortar additive, mortar additive and water;
[0007] Calculated by mass fraction, the cement accounts for 28-40%, the modified pipe pile waste slurry accounts for 15-18%, the quartz sand accounts for 6-12%, the natural river sand accounts for 6-8%, the crushed stone powder accounts for 5-7%, the filler accounts for 5-9%, the mortar auxiliary agent accounts for 2-4%, the mortar additive accounts for 7-10%, and the water is supplemented to 100%.
[0008] The cement includes one or more of silicate cement, fluoroaluminate cement and phosphate cement;
[0009] The filler includes one or more of quartz powder, fly ash, silica fume powder, mica powder, and sintered brick powder;
[0010] The mortar additive includes silicon nitride or silicon carbide.
[0011] The modified pipe pile waste is prepared by using the waste pulp of pipe pile factory, porous ceramsite, nano sodium aluminosilicate and chlorinated polyvinyl chloride (CPVC) resin as raw materials;
[0012] The waste slurry of the pipe pile factory comes from waste materials generated by the production of the pipe pile factory, and mainly contains components such as water, silicate cement and ground sand, with a water content of 30-40%.
[0013] The mortar additives include a water retaining agent, a retarder and a water reducing agent, and the mixing mass ratio thereof is (2-3): (2-4): (1-3);
[0014] The water retaining agent is a mixture of phosphorus slag powder, cellulose ether, chitosan nano whiskers and solid sulfur ash, and the mixing mass ratio is (4-7): (2-3): (1-3): (5-7). The water retaining agent is prepared by magnetically stirring the phosphorus slag powder, solid sulfur ash and chitosan nano whisker aqueous solution, then adding a dilute hydrochloric acid solution of cellulose ether and magnetically stirring to obtain the water retaining agent.
[0015] The retarder is a mixture of sodium rosin acid, glucose and organic phosphonic acid, and the mixing mass ratio is (1-3): (5-7): (3-4). The preparation method is as follows: after the sodium rosin acid and glucose are evenly mixed, the organic phosphonic acid solution is added, and ultrasonic stirring is performed at 30-40° C., and the retarder is obtained by stirring evenly.
[0016] The water reducing agent includes a polycarboxylic acid-based water reducing agent.
[0017] The present invention also provides a method for preparing environmentally friendly wet-mixed mortar based on waste slurry from a pipe pile factory, comprising the following steps:
[0018] 1) Preparation of modified pipe pile waste slurry:
[0019] a) mixing the waste slurry from the pipe pile factory with the porous ceramsite and nano sodium aluminosilicate at a stirring speed of 500 to 600 rpm to obtain a pretreated waste slurry from the pipe pile factory;
[0020] The porous ceramsite accounts for 30-40wt% of the waste slurry, and the nano-sodium aluminosilicate accounts for 10-15wt% of the waste slurry;
[0021] The particle size of the porous ceramsite is 0.5 to 1 cm;
[0022] b) heating the pretreated waste slurry of pipe piles to 60-70° C., adding a silane coupling agent, and then heating to 120-130° C., adding chlorinated polyvinyl chloride (CPVC) resin, stirring at a speed of 100-200 rpm, and stirring to obtain modified waste pipe piles;
[0023] The addition amount of the silane coupling agent is 3-6wt%, and the addition amount of the chlorinated polyvinyl chloride (CPVC) resin is 15-17wt%;
[0024] The silane coupling agent includes one or more of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane and 3-aminopropyltriethoxysilane;
[0025] The waste slurry of the pipe pile factory comes from the waste generated by the production of the pipe pile factory, and mainly contains water, silicate cement and ground sand, etc., with a water content of 30-40%;
[0026] 2) Raw material pretreatment: drying quartz sand, natural river sand, crushed stone powder, filler and mortar additives, and grinding them into uniform particles;
[0027] 3) Preparation of mortar additives: prepare a water retaining agent and a retarder respectively, mix the water retaining agent, the retarder and the water reducing agent according to a mass ratio to obtain a mortar additive, wherein the mixing mass ratio is (2-3): (2-4): (1-3);
[0028] The water retaining agent is a mixture of phosphorus slag powder, cellulose ether, chitosan nano whiskers and solid sulfur ash, and the mixing mass ratio is (4-7): (2-3): (1-3): (5-7). The water retaining agent is prepared by magnetically stirring the phosphorus slag powder, solid sulfur ash and chitosan nano whisker aqueous solution, then adding a dilute hydrochloric acid solution of cellulose ether and magnetically stirring to obtain the water retaining agent.
[0029] The retarder is a mixture of sodium rosin acid, glucose and organic phosphonic acid, and the mixing mass ratio is (1-3): (5-7): (3-4). The preparation method is as follows: after the sodium rosin acid and glucose are evenly mixed, the organic phosphonic acid solution is added, and ultrasonic stirring is performed at 30-40° C., and the retarder is obtained by stirring evenly.
[0030] 4) Preparation of wet-mixed mortar: according to the mass fraction ratio, cement, modified pipe pile waste slurry, mortar auxiliary agent and mortar additive are mixed and stirred evenly, and then quartz sand, natural river sand, crushed stone powder, filler and water are added and stirred evenly to obtain wet-mixed mortar.
[0031] The beneficial effects of the present invention are as follows:
[0032] The environmentally friendly wet-mixed mortar based on waste slurry from a pipe pile factory of the present invention, under the synergistic effect of modified waste slurry from pipe pile factories, mortar additives, mortar auxiliary agents and fillers, enhances the thickening and water-retaining effects of the wet-mixed mortar, thereby helping to maintain the plasticity of the wet-mixed mortar while extending its operability time, reducing the dispersion of the mortar and the inhibitory effect of cement hydration, extending the plasticity retention time of the mortar, and enhancing the operability space of the mortar, so that the prepared wet-mixed mortar can meet construction requirements.
[0033] The method for preparing the environmentally friendly wet-mixed mortar based on waste slurry from a pipe pile factory of the present invention utilizes the waste slurry generated by the pipe pile factory, modifies the waste slurry, and prepares the environmentally friendly wet-mixed mortar by combining fillers, mortar additives and mortar additives. The waste slurry from the pipe pile factory is not only recycled, but also the compatibility of the waste slurry from the pipe pile factory with cement and aggregate is improved by physically modifying the waste slurry. The wet-mixed mortar with improved performance is prepared by adding mortar additives, mortar additives and the like, thereby improving its mechanical properties and solving the problems of rapid water loss, poor flexibility and low strength. The modified waste slurry from the pipe pile factory is used to improve the physical bonding ability of the molecules, which is helpful for bonding cement, sand and gravel as well as mortar additives, fillers and other materials, thereby enhancing the bonding strength between materials, and at the same time, it is helpful for the waste utilization of the waste slurry from the pipe pile factory, and the mechanical properties of the wet-mixed mortar are enhanced, thereby creating utilization value for the waste slurry from the pipe pile factory and expanding its application. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below through specific implementation cases. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of protection of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art are all within the scope of the claims attached to this application.
[0035] Unless otherwise specified, all raw materials and reagents of the present invention are raw materials and reagents from the conventional market.
[0036] Example 1
[0037] Preparation of environmentally friendly wet-mixed mortar based on waste slurry from pipe pile factory
[0038] 1) Preparation of modified pipe pile waste slurry:
[0039] a) mixing the waste slurry from the pipe pile factory with 35 wt% of porous ceramsite and 12 wt% of nano sodium aluminosilicate at a stirring speed of 550 rpm to obtain a pretreated waste slurry from the pipe pile factory;
[0040] The particle size of the porous ceramsite is 0.5 to 1 cm;
[0041] b) heating the pretreated waste slurry of pipe piles to 65° C., adding 5 wt % 3-aminopropyltrimethoxysilane, and then heating to 125° C., adding 16 wt % chlorinated polyvinyl chloride (CPVC) resin, stirring at a speed of 150 rpm, and stirring to obtain modified waste pipe piles;
[0042] The waste slurry of the pipe pile factory comes from the waste generated by the production of the pipe pile factory, and mainly contains water, silicate cement and ground sand, etc., with a water content of 30-40%;
[0043] 2) Raw material pretreatment: drying quartz sand, natural river sand, crushed stone powder, filler and mortar additives, and grinding them into uniform particles;
[0044] The quartz sand and natural river sand are ground to a particle size of 100 to 150 meshes;
[0045] The crushed stone powder, filler and mortar additive are ground to a particle size of 100 to 200 meshes;
[0046] 3) Preparation of mortar additives: prepare a water retaining agent and a retarder respectively, and mix the water retaining agent, the retarder and the polycarboxylate water reducer in a mass ratio of 2:3:2 to obtain a mortar additive;
[0047] The water retaining agent is prepared by: stirring phosphorus slag powder, sulfur-fixing ash and chitosan nano whisker aqueous solution evenly with magnetic force, then adding dilute hydrochloric acid solution of cellulose ether and stirring evenly with magnetic force to obtain the water retaining agent, wherein the mixing mass ratio of phosphorus slag powder, cellulose ether, chitosan nano whisker and sulfur-fixing ash is 6:3:2:6;
[0048] The retarder is prepared by: mixing sodium rosin acid and glucose uniformly, adding an organic phosphonic acid solution, and performing ultrasonic stirring at 35° C. to obtain the retarder, wherein the mixing mass ratio of sodium rosin acid, glucose and organic phosphonic acid is 2:6:3;
[0049] 4) Preparation of wet-mixed mortar: According to the mass fraction ratio, 30% silicate cement, 16% modified pipe pile waste slurry, 4% mortar auxiliary agent silicon nitride and 8% mortar additive are mixed and stirred evenly. Then, 10% quartz sand, 7% natural river sand, 6% crushed stone powder, 8% filler (quartz powder, fly ash, sintered brick powder mass ratio of 1:1:1) and 11% water are added and stirred evenly to obtain wet-mixed mortar.
[0050] Example 2
[0051] Preparation of environmentally friendly wet-mixed mortar based on waste slurry from pipe pile factory
[0052] 1) Preparation of modified pipe pile waste slurry:
[0053] a) mixing the waste slurry from the pipe pile factory with 30 wt% of porous ceramsite and 15 wt% of nano sodium aluminosilicate at a stirring speed of 600 rpm to obtain a pretreated waste slurry from the pipe pile factory;
[0054] The particle size of the porous ceramsite is 0.5 to 1 cm;
[0055] b) heating the pretreated waste slurry of pipe piles to 60° C., adding 3 wt % 3-aminopropyltriethoxysilane, and then heating to 130° C., adding 15 wt % chlorinated polyvinyl chloride (CPVC) resin, stirring at a speed of 200 rpm, and stirring to obtain modified waste pipe piles;
[0056] The waste slurry of the pipe pile factory comes from the waste generated by the production of the pipe pile factory, and mainly contains water, silicate cement and ground sand, etc., with a water content of 30-40%;
[0057] 2) Raw material pretreatment: drying quartz sand, natural river sand, crushed stone powder, filler and mortar additives, and grinding them into uniform particles;
[0058] The quartz sand and natural river sand are ground to a particle size of 100 to 150 meshes;
[0059] The crushed stone powder, filler and mortar additive are ground to a particle size of 100 to 200 meshes;
[0060] 3) Preparation of mortar additives: prepare a water retaining agent and a retarder respectively, and mix the water retaining agent, the retarder and the polycarboxylate water reducer in a mass ratio of 3:4:3 to obtain a mortar additive;
[0061] The water retaining agent is prepared by: magnetically stirring phosphorus slag powder, sulfur-fixing ash and chitosan nano whisker aqueous solution, then adding dilute hydrochloric acid solution of cellulose ether, and magnetically stirring to obtain the water retaining agent, wherein the mass ratio of phosphorus slag powder, cellulose ether, chitosan nano whisker and sulfur-fixing ash is 7:3:3:7;
[0062] The retarder is prepared by: mixing sodium rosin acid and glucose evenly, adding an organic phosphonic acid solution, and performing ultrasonic stirring at 40° C. to obtain the retarder, wherein the mixing mass ratio of sodium rosin acid, glucose and organic phosphonic acid is 3:7:4;
[0063] 4) Preparation of wet-mixed mortar: According to the mass fraction ratio, 31% phosphate cement, 18% modified pipe pile waste slurry, 3% mortar auxiliary agent silicon carbide and 8% mortar additive are mixed and stirred evenly. Then, 10% quartz sand, 8% natural river sand, 5% crushed stone powder, 7% filler (fly ash, silica fume powder, sintered brick powder mass ratio of 1:1:1) and 10% water are added and stirred evenly to obtain wet-mixed mortar.
[0064] Example 3
[0065] Preparation of environmentally friendly wet-mixed mortar based on waste slurry from pipe pile factory
[0066] 1) Preparation of modified pipe pile waste slurry:
[0067] a) mixing the waste slurry from the pipe pile factory with 40 wt% of porous ceramsite and 10 wt% of nano sodium aluminosilicate at a stirring speed of 600 rpm to obtain a pretreated waste slurry from the pipe pile factory;
[0068] The particle size of the porous ceramsite is 0.5 to 1 cm;
[0069] b) heating the pretreated waste slurry of pipe piles to 70° C., adding 6 wt % 3-aminopropyltriethoxysilane, and then heating to 120° C., adding 17 wt % chlorinated polyvinyl chloride (CPVC) resin, stirring at a speed of 100 rpm, and stirring to obtain modified waste pipe piles;
[0070] The waste slurry of the pipe pile factory comes from the waste generated by the production of the pipe pile factory, and mainly contains water, silicate cement and ground sand, etc., with a water content of 30-40%;
[0071] 2) Raw material pretreatment: drying quartz sand, natural river sand, crushed stone powder, filler and mortar additives, and grinding them into uniform particles;
[0072] The quartz sand and natural river sand are ground to a particle size of 100 to 150 meshes;
[0073] The crushed stone powder, filler and mortar additive are ground to a particle size of 100 to 200 meshes;
[0074] 3) Preparation of mortar additives: prepare a water retaining agent and a retarder respectively, and mix the water retaining agent, the retarder and the polycarboxylate water reducer in a mass ratio of 2:2:1 to obtain a mortar additive;
[0075] The water retaining agent is prepared by: stirring phosphorus slag powder, sulfur-fixing ash and chitosan nano whisker aqueous solution evenly with magnetic force, then adding dilute hydrochloric acid solution of cellulose ether and stirring evenly with magnetic force to obtain the water retaining agent, wherein the mixing mass ratio of phosphorus slag powder, cellulose ether, chitosan nano whisker and sulfur-fixing ash is 4:2:1:5;
[0076] The retarder is prepared by: mixing sodium rosin acid and glucose evenly, adding an organic phosphonic acid solution, and performing ultrasonic stirring at 30° C. to obtain the retarder, wherein the mixing mass ratio of sodium rosin acid, glucose and organic phosphonic acid is 1:5:3;
[0077] 4) Preparation of wet-mixed mortar: According to the mass fraction ratio, 28% fluoroaluminate cement, 15% modified pipe pile waste slurry, 3% mortar auxiliary agent silicon carbide and 10% mortar additive are mixed and stirred evenly. Then, 12% quartz sand, 8% natural river sand, 7% crushed stone powder, 9% filler (silica fume powder, mica powder, sintered brick powder mass ratio of 1:1:1) and 8% water are added and stirred evenly to obtain wet-mixed mortar.
[0078] Example 4
[0079] Preparation of environmentally friendly wet-mixed mortar based on waste slurry from pipe pile factory
[0080] 1) Preparation of modified pipe pile waste slurry:
[0081] a) mixing the waste slurry from the pipe pile factory with 37 wt% of porous ceramsite and 13 wt% of nano sodium aluminosilicate at a stirring speed of 580 rpm to obtain a pretreated waste slurry from the pipe pile factory;
[0082] The particle size of the porous ceramsite is 0.5 to 1 cm;
[0083] b) heating the pretreated waste slurry of pipe piles to 63° C., adding 4 wt % 3-aminopropyltrimethoxysilane, and then heating to 125° C., adding 16 wt % chlorinated polyvinyl chloride (CPVC) resin, stirring at a speed of 160 rpm, and stirring to obtain modified waste pipe piles;
[0084] The waste slurry of the pipe pile factory comes from the waste generated by the production of the pipe pile factory, and mainly contains water, silicate cement and ground sand, etc., with a water content of 30-40%;
[0085] 2) Raw material pretreatment: drying quartz sand, natural river sand, crushed stone powder, filler and mortar additives, and grinding them into uniform particles;
[0086] The quartz sand and natural river sand are ground to a particle size of 100 to 150 meshes;
[0087] The crushed stone powder, filler and mortar additive are ground to a particle size of 100 to 200 meshes;
[0088] 3) Preparation of mortar additives: prepare a water retaining agent and a retarder respectively, and mix the water retaining agent, the retarder and the polycarboxylate water reducer in a mass ratio of 3:2:2 to obtain a mortar additive;
[0089] The water retaining agent is prepared by: magnetically stirring phosphorus slag powder, sulfur-fixing ash and chitosan nano whisker aqueous solution, then adding dilute hydrochloric acid solution of cellulose ether, and magnetically stirring to obtain the water retaining agent, wherein the mass ratio of phosphorus slag powder, cellulose ether, chitosan nano whisker and sulfur-fixing ash is 6:3:3:4;
[0090] The retarder is prepared by: mixing sodium rosin acid and glucose evenly, adding an organic phosphonic acid solution, and performing ultrasonic stirring at 38° C. to obtain the retarder, wherein the mixing mass ratio of sodium rosin acid, glucose and organic phosphonic acid is 2:5:3;
[0091] 4) Preparation of wet-mixed mortar: According to the mass fraction ratio, 40% phosphate cement, 17% modified pipe pile waste slurry, 2% mortar auxiliary agent silicon nitride and 7% mortar additive are mixed and stirred evenly. Then, 6% quartz sand, 6% natural river sand, 7% crushed stone powder, 5% filler (quartz powder, fly ash, silica fume powder mass ratio of 1:1:1) and 10% water are added and stirred evenly to obtain wet-mixed mortar.
[0092] Comparative Example 1
[0093] As a control group of Example 1, in the preparation of the wet-mixed mortar of Comparative Example 1, the waste slurry from the pipe pile factory was not modified, and the waste slurry from the pipe pile factory was directly used for the preparation of the wet-mixed mortar, and other conditions remained unchanged.
[0094] Comparative Example 2
[0095] As a control group of Example 1, in the preparation of the wet mixed mortar of Comparative Example 2, in the mortar additive of step 3), the water retaining agent is phosphorus slag powder, the retarder is glucose, and other conditions remain unchanged.
[0096] Comparative Example 3
[0097] As a control group of Example 1, in the preparation of the wet-mixed mortar of Comparative Example 3, no mortar additives and fillers were added. According to the mass fraction, 30% of Portland cement, 16% of modified pipe pile waste slurry and 8% of mortar additives were mixed and stirred evenly. Then, 14% of quartz sand, 11% of natural river sand, 10% of crushed stone powder and 11% of water were added and stirred evenly to obtain wet-mixed mortar.
[0098] The wet-mixed mortars prepared in the examples and comparative examples were subjected to the following performance tests, and the plastic retention time, 2h consistency loss and water retention rate of the mortars were measured according to JGJ / T70-2009 "Standard for Basic Performance Test Methods of Building Mortars";
[0099] The wet mixed mortars prepared in the embodiment and the comparative example were respectively loaded into molds of 40 mm×40 mm×160 mm and 40 mm×40 mm×2 mm, and placed in a curing box at a temperature of (25±1)°C and a humidity of (70±1)% for curing to different ages. The 7d and 28d compressive strengths and 14d tensile bond strengths of the mortars were measured according to JGJ / T70-2009 "Standard for Test Methods for Basic Properties of Building Mortars".
[0100] 1. Plastic preservation time of wet mixed mortar
[0101] Table 1 Plastic preservation time of wet mixed mortar
[0102]
[0103] It can be seen from Table 1 that, compared with Comparative Examples 1 to 3, the plastic preservation time of the wet-mixed mortar prepared in the embodiment of the present invention exceeds 15 hours, and the plastic preservation time of the comparative example is reduced. This is because the addition of the prepared modified pipe pile waste slurry, mortar additives, fillers, and additives reduces the dispersion of the mortar and the inhibition of cement hydration, prolongs the plastic preservation time of the mortar, and at the same time enhances the operable space of the mortar, so that the prepared wet-mixed mortar can meet the construction requirements.
[0104] 2. 24h consistency and water retention of wet-mixed mortar
[0105] Table 2 Consistency and water retention of wet mixed mortar
[0106]
[0107]
[0108] As can be seen from Table 2, the water retention rate of the wet-mixed mortar prepared in Examples 1 to 4 of the present invention can reach 94%, and the consistency after 24 hours can reach 87 mm. Compared with the comparative example, this is mainly because the synergistic effect of the modified pipe pile waste slurry, mortar additives, mortar auxiliary agents and fillers enhances the thickening and water retention effects of the wet-mixed mortar, which helps to maintain the plasticity of the wet-mixed mortar while extending its operability time.
[0109] 3. Mechanical properties of wet-mix mortar
[0110] Table 3 Compressive strength of wet mixed mortar (Mpa)
[0111]
[0112] Table 4 Tensile bond strength of wet-mixed mortar (Mpa)
[0113]
[0114]
[0115] It can be seen from Table 3 and Table 4 that, compared with the comparative example, the wet-mixed mortar prepared in Examples 1 to 4 of the present invention is superior in compressive strength and tensile bonding strength. It can be seen that the synergistic effect of the modified pipe pile waste mortar, mortar additives, mortar adjuvants and fillers helps to improve the mechanical properties of the wet-mixed mortar, especially the influence of the prepared modified pipe pile waste mortar and mortar additives. The modified pipe pile waste mortar improves the physical bonding ability of molecules, helps to bond cement, sand and gravel, mortar additives, fillers and other materials, enhances the bonding strength between materials, and at the same time helps to utilize the waste of pipe pile waste mortar, and also enhances the mechanical properties of the wet-mixed mortar, creating utilization value for the pipe pile waste mortar and expanding its application.
Claims
1. An environmentally friendly wet-mixed mortar based on waste slurry from a pile factory, characterized in that: The environmentally friendly wet-mixed mortar includes the following components: cement, modified pipe pile waste slurry, quartz sand, natural river sand, crushed stone powder, filler, mortar additive, mortar additive and water; By mass fraction, the cement accounts for 28-40%, the modified pipe pile waste slurry accounts for 15-18%, the quartz sand accounts for 6-12%, the natural river sand accounts for 6-8%, the crushed stone powder accounts for 5-7%, the filler accounts for 5-9%, the mortar additive accounts for 2-4%, the mortar additive accounts for 7-10%, and the water is supplemented to 100%; The mortar additive comprises a water retaining agent, a retarder and a water reducing agent, and the mixing mass ratio of the water retaining agent, the retarder and the water reducing agent is (2-3): (2-4): (1-3); The water retaining agent is a mixture of phosphorus slag powder, cellulose ether, chitosan nano whiskers and fixed sulfur ash, wherein the mass ratio of the phosphorus slag powder, cellulose ether, chitosan nano whiskers and fixed sulfur ash is (4-7): (2-3): (1-3): (5-7). The preparation of the water retaining agent comprises the following steps: magnetically stirring the phosphorus slag powder, fixed sulfur ash and chitosan nano whisker aqueous solution, then adding a dilute hydrochloric acid solution of cellulose ether and magnetically stirring to obtain the water retaining agent; The retarder is a mixture of sodium rosin acid, glucose and organic phosphonic acid, wherein the mixing mass ratio of the sodium rosin acid, glucose and organic phosphonic acid is (1-3): (5-7): (3-4). The preparation of the retarder comprises the following steps: after the sodium rosin acid and glucose are uniformly mixed, an organic phosphonic acid solution is added, and ultrasonic stirring is performed at 30-40° C., and the retarder is obtained by uniformly stirring.
2. The environmentally friendly wet-mixed mortar based on waste slurry from a pile factory according to claim 1 is characterized in that: The filler includes one or more of quartz powder, fly ash, silica fume powder, mica powder and sintered brick powder.
3. The environmentally friendly wet-mixed mortar based on waste slurry from a pipe pile factory according to claim 1 is characterized in that: The mortar additive includes silicon nitride or silicon carbide.
4. The environmentally friendly wet-mixed mortar based on waste slurry from a pipe pile factory according to claim 1 is characterized in that: The modified pipe pile waste is prepared by using the waste pulp of pipe pile factory, porous ceramsite, nano sodium aluminosilicate and chlorinated polyvinyl chloride (CPVC) resin as raw materials; The waste slurry from the pipe pile factory comes from the waste generated by the production of the pipe pile factory, and mainly contains water, silicate cement and ground sand, with a water content of 30-40%.
5. A method for preparing an environmentally friendly wet-mixed mortar based on waste slurry from a pipe pile factory according to any one of claims 1 to 4, characterized in that: The steps include: 1) Preparation of modified pipe pile waste slurry: a) The waste slurry from the pipe pile factory is fully mixed with the porous ceramsite and nano sodium aluminosilicate at a stirring speed of 500-600 rpm to obtain a pretreated waste slurry from the pipe pile factory; b) The pretreated waste slurry of pipe piles is heated to 60-70°C, a silane coupling agent is added, and then the temperature is raised to 120-130°C, chlorinated polyvinyl chloride (CPVC) resin is added, and the stirring speed is 100-200 rpm. The modified waste pipe piles are obtained by stirring evenly; 2) Raw material pretreatment: drying quartz sand, natural river sand, crushed stone powder, filler and mortar additives, and grinding them into uniform particles; 3) Preparation of mortar additives: prepare a water retaining agent and a retarder respectively, and mix the water retaining agent, the retarder and the water reducing agent according to a mass ratio to obtain a mortar additive, wherein the mixing mass ratio of the water retaining agent, the retarder and the water reducing agent is (2-3): (2-4): (1-3); 4) Preparation of wet-mixed mortar: According to the mass fraction, cement, modified pipe pile waste slurry, mortar auxiliary agent and mortar additive are mixed and stirred evenly. Then, quartz sand, natural river sand, crushed stone powder, filler and water are added and stirred evenly to obtain wet-mixed mortar.
6. The method for preparing environmentally friendly wet-mixed mortar based on waste slurry from a pipe pile factory according to claim 5, characterized in that: Step 1) the porous ceramsite accounts for 30-40 wt% of the waste slurry, and the nano sodium aluminosilicate accounts for 10-15 wt% of the waste slurry; The particle size of the porous ceramsite is 0.5-1 cm.
7. The method for preparing environmentally friendly wet-mixed mortar based on waste slurry from a pipe pile factory according to claim 5, characterized in that: In step 1), the amount of the silane coupling agent added is 3-6 wt%, and the amount of the chlorinated polyvinyl chloride (CPVC) resin added is 15-17 wt%.