A sealing strip and its production process
By using TPU resin, modified nano-scale silica, coupling agent and slippery agent formulas, combined with specific production processes, the problem of high viscosity of TPU sealing strips in the production process is solved, and the stretching of the sealing strips is improved Performance and toughness reduce the risk of infection and extend the service life.
Patent Information
- Application Number
- CN202211105577.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-09-09
AI Technical Summary
The existing TPU sealing strips are highly sticky during the production process, resulting in uneven mixing and machine adhesion problems, affecting the tensile performance and toughness of the sealing strips, and increasing the risk of infection for medical staff.
The formula of TPU resin, modified nano-grade silica, coupling agent, composite antioxidant and slippery agent is prepared by drying, stirring, plasticizing, extruding and embossing. and tear-resistant sealing strips, reducing viscosity and improving the compactness and mechanical strength of finished sealing strips.
Effectively reduce the stickiness of the TPU seal strip, improve the tensile performance and tear resistance of the seal strip, enhance the toughness and waterproof and aging resistance of the finished seal strip, extend the service life, and reduce the adhesion problem for the next production Influence.
Smart Images

Figure BDA0003841705190000191 
Figure BDA0003841705190000192
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sealing strip materials, and in particular to a sealing strip and a production process thereof. Background Art
[0002] Sealing strips are products that seal something and make it difficult to open, and play the role of shock absorption, waterproofing, sound insulation, heat insulation, dust prevention, fixing, etc. Sealing strips are made of rubber, paper, metal, plastic and other materials.
[0003] The seams of medical protective clothing must be sealed with professional adhesive strips. After treatment, there will be no gaps on the surface of the protective clothing, which can be waterproof and dustproof, and block bacteria, viruses and pollutants from entering the protective clothing, thereby protecting the medical staff wearing protective clothing from interference and pollution from the external environment.
[0004] The material of the sealing strip on the protective clothing currently on the market is EVA. Although EVA is acid and alkali resistant, has excellent electrical insulation and is resistant to low temperatures, it is easily decomposed by heat, has low surface hardness, and is easily scratched, which increases the risk of cracking at the seams of the protective clothing, increases the risk of infection for medical staff, and is not conducive to the use of medical staff.
[0005] In order to solve the above technical problems, China's patent publication number is CN113072805A, in which TPU resin is used as the main raw material, which has the effects of flexibility, wear resistance and non-cracking; surfactants, grafting components, chain extenders, catalysts and antioxidants are added, and the elongation and stretchability of the TPU film are improved to produce a film used in protective clothing.
[0006] However, based on the applicant's understanding of TPU, TPU has high viscosity during the production process, which makes it difficult to mix evenly with other additives when TPU is mixed and melted, and it adheres to the machine, causing materials to stick inside the machine and be mixed into the film produced next time, resulting in the final finished sealing strip being of low uniformity, the tensile properties and toughness of the sealing strip being reduced, the actual use effect being unsatisfactory, and there is a potential risk of medical staff being infected due to the rupture of the sealing strip.
[0007] Therefore, it is urgent to develop a new formula of TPU film for use in the sealing strips of protective clothing to improve the above defects. Summary of the invention
[0008] One of the purposes of the present invention is to provide a sealing strip having excellent tensile strength and tearing strength, which is particularly suitable for use on protective clothing.
[0009] 1. A sealing strip, characterized in that: by weight, it comprises the following components:
[0010] TPU resin: 85-95 parts;
[0011] Modified nano-scale silicon dioxide: 1-5 parts;
[0012] Coupling agent: 1-5 parts;
[0013] Lubricant: 1-5 parts;
[0014] Compound antioxidant: 1-5 parts.
[0015] Preferably, the modified nano-scale silicon dioxide is prepared by grinding the nano-scale silicon dioxide into a nano-grinder at least once to obtain the modified nano-scale silicon dioxide.
[0016] Preferably, the coupling agent is at least one of a silane coupling agent, an aluminate coupling agent, a rare earth coupling agent, and an aluminum-titanium coupling agent.
[0017] Preferably, the composite antioxidant is a phenolic antioxidant and an amine antioxidant in any ratio.
[0018] Preferably, the phenolic antioxidant is at least one of diaryl secondary amine, tetraethylenepentamine, ADPA, and OPD.
[0019] Preferably, the amine antioxidant is at least one of 2,6-dimethylphenol, 2,4,5-trihydroxybutyrophenone, PTBP, BHT, BHA, PG, and TBHQ.
[0020] Preferably, the lubricant is one of oleamide, erucamide and stearamide.
[0021] By adopting the above technical solution, the viscosity of the sealing strip made of TPU as the main resin during the production process is reduced, and the tensile performance and tear resistance of the sealing strip are improved.
[0022] The second object of the present invention is to provide a sealing strip production process, which is applicable to any of the sealing strips described in claims 1 to 7, and comprises the following preparation steps:
[0023] S1: Put TPU resin into the first drying oven for drying, and put modified nano-silica, coupling agent, lubricant and composite antioxidant into the second drying oven;
[0024] S2: Mix the dried TPU resin, modified nano-silica, coupling agent, lubricant and composite antioxidant in S1 and put them into a high-speed kneader for stirring and mixing evenly;
[0025] S3: Put the mixed materials in S2 into an internal mixer for preliminary plasticization;
[0026] S4: heating the material in S3 and continuing plasticization;
[0027] S5: heating the material in S4 until it is completely plasticized and begins to be used for feeding;
[0028] S6: The completely plasticized material in S5 is passed through a filter to remove impurities.
[0029] S7: the material from which impurities are removed in S6 is extruded through an extruder and sent to a casting machine, and pressed to a desired thickness to form a film;
[0030] S8: pulling the film in S7 onto the embossing wheel;
[0031] S9: embossing one side of the film in S8;
[0032] S10: embossing the other side of the film in S9;
[0033] S11: Cooling the film after embossing in S10 through a cooling mechanism;
[0034] S12: rolling up the film cooled in S11 and placing it for cooling and solidification;
[0035] S13: Cutting the film cured in S12 into required specifications to obtain a finished sealing strip.
[0036] Preferably, the first drying box in S1 is heated at a temperature of 100° C. for four hours, and the second drying box is heated at a temperature of 70° C. for three hours;
[0037] The initial plasticizing temperature in S3 is 135°C-145°C;
[0038] The continued plasticizing temperature in S4 is 150°C-160°C;
[0039] The complete plasticization temperature in S5 is 155°C-175°C;
[0040] The S6 filter screen is 20 mesh × 40 mesh × 150 mesh × 40 mesh × 20 mesh;
[0041] The extrusion temperature of the extruder in S7 is 180° C.-185° C., and the screw compression ratio in the extruder is 2.5-3.5:1.
[0042] By adopting the above technical solution, the raw materials can be dehumidified to avoid the formation of bubbles in the mixed materials during the production process, so that the produced sealing strip has good density, thereby improving the toughness and mechanical strength of the sealing strip.
[0043] In summary, the beneficial effects of this application are:
[0044] The invention provides a sealing strip and a production process thereof. The TPU resin is used as a main resin. The particle size of the modified nano-scale silicon dioxide is small, and the modified nano-scale silicon dioxide can penetrate into the vicinity of the unsaturated bond of the hard segment of the TPU resin and react with the electron cloud of the unsaturated bond, thereby shortening the distance between the hard segments, making the hydrogen bond effect between the hard segments more obvious, facilitating the aggregation of the hard segment molecules, promoting the microphase separation of the TPU molecules, making the TPU resin more compact, and thus improving the toughness, strength, waterproofness, anti-aging and chemical resistance of the sealing strip; the addition of a coupling agent can increase the viscosity of the system, improve the toughness and mechanical properties of the system, and enable the modified nano-scale silicon dioxide to better improve the compatibility with the mixed resin material, and further make the modified nano-scale silicon dioxide Fully dispersed in the mixed resin raw materials; the phenolic antioxidants and amine antioxidants in the composite antioxidants are used together, and the multiple antioxidant components have a synergistic effect, which prolongs the service life of the antioxidants, improves the antioxidant capacity, and enhances the service life of the finished sealing strips; the lubricant can improve the fluidity and viscosity of the mixed resin raw materials, increase the dispersion effect of the composite antioxidant, thereby improving the antioxidant properties of the sealing strips, and synergize with the modified nano-scale silica to further reduce the viscosity of the mixed resin materials, so that other additives are fully and evenly dispersed in the TPU resin, and reduce the amount of adhesion to the machine, reduce the impact of the adhesion on the film produced next time, and improve the tensile properties and toughness of the finished sealing strips. DETAILED DESCRIPTION
[0045] It should be noted that a matte additive is added in the following embodiments. The matte additive is capable of producing a matte effect, which materializes the sealing strip, thereby covering the seams of the protective object, which is beneficial to the appearance.
[0046] It should be noted that the term "modification" in the application document of the present invention refers to the process of physical grinding to make the powder to be ground smaller than the powder before grinding and the degree of uniformity of the particle size is more consistent.
[0047] Example 1
[0048] By weight, the following substances
[0049] TPU resin: 85 parts;
[0050] Modified nano-silica: 1 part;
[0051] Silane coupling agent: 1 part;
[0052] Stearic acid amide: 1 part;
[0053] ADPA: 0.5 parts;
[0054] BHA: 0.5 parts;
[0055] Matte additive: 1 part.
[0056] The preparation was carried out by the following steps.
[0057] Preparation of the modified nano-scale silicon dioxide: The nano-scale silicon dioxide is put into a nano-grinder at least once for grinding to obtain the modified nano-scale silicon dioxide.
[0058] S1: Put TPU resin into the first drying oven for drying, and put modified nano-silica, coupling agent, lubricant, composite antioxidant and matte additive into the second drying oven;
[0059] S2: Mix the dried TPU resin, modified nano-silica, coupling agent, lubricant, composite antioxidant and matte additive in S1 and put them into a high-speed kneader for stirring and mixing evenly;
[0060] S3: Put the mixed materials in S2 into an internal mixer for preliminary plasticization;
[0061] S4: heating the material in S3 and continuing plasticization;
[0062] S5: heating the material in S4 until it is completely plasticized and begins to be used for feeding;
[0063] S6: The completely plasticized material in S5 is passed through a filter to remove impurities.
[0064] S7: the material from which impurities are removed in S6 is extruded through an extruder and sent to a casting machine, and pressed to a desired thickness to form a film;
[0065] S8: pulling the film in S7 onto the embossing wheel;
[0066] S9: embossing one side of the film in S8;
[0067] S10: embossing the other side of the film in S9;
[0068] S11: Cooling the film after embossing in S10 through a cooling mechanism;
[0069] S12: rolling up the film cooled in S11 and placing it for cooling and solidification;
[0070] S13: Cutting the film cured in S12 into required specifications to obtain a finished sealing strip.
[0071] The first drying oven in S1 is heated at 100° C. for four hours, and the second drying oven is heated at 70° C. for three hours;
[0072] The initial plasticizing temperature in S3 is 135°C-145°C;
[0073] The continued plasticizing temperature in S4 is 150°C-160°C;
[0074] The complete plasticization temperature in S5 is 155°C-175°C;
[0075] The S6 filter screen is 20 mesh × 40 mesh × 150 mesh × 40 mesh × 20 mesh;
[0076] The extrusion temperature of the extruder in S7 is 180° C.-185° C., and the screw compression ratio in the extruder is 2.5-3.5:1.
[0077] Example 2
[0078] By weight, the following substances
[0079] TPU resin: 90 parts;
[0080] Modified nano-scale silica: 3 parts;
[0081] Silane coupling agent: 3 parts;
[0082] Stearic acid amide: 3 parts;
[0083] ADPA: 1.5 parts;
[0084] BHA: 1.5 parts;
[0085] Matting agent: 3 parts.
[0086] The preparation was carried out by the following steps.
[0087] Preparation of the modified nano-scale silicon dioxide: The nano-scale silicon dioxide is put into a nano-grinder at least once for grinding to obtain the modified nano-scale silicon dioxide.
[0088] S1: Put TPU resin into the first drying oven for drying, and put modified nano-silica, coupling agent, lubricant, composite antioxidant and matte additive into the second drying oven;
[0089] S2: Mix the dried TPU resin, modified nano-silica, coupling agent, lubricant, composite antioxidant and matte additive in S1 and put them into a high-speed kneader for stirring and mixing evenly;
[0090] S3: Put the mixed materials in S2 into an internal mixer for preliminary plasticization;
[0091] S4: heating the material in S3 and continuing plasticization;
[0092] S5: heating the material in S4 until it is completely plasticized and begins to be used for feeding;
[0093] S6: The completely plasticized material in S5 is passed through a filter to remove impurities.
[0094] S7: the material from which impurities are removed in S6 is extruded through an extruder and sent to a casting machine, and pressed to a desired thickness to form a film;
[0095] S8: pulling the film in S7 onto the embossing wheel;
[0096] S9: embossing one side of the film in S8;
[0097] S10: embossing the other side of the film in S9;
[0098] S11: Cooling the film after embossing in S10 through a cooling mechanism;
[0099] S12: rolling up the film cooled in S11 and placing it for cooling and solidification;
[0100] S13: Cutting the film cured in S12 into required specifications to obtain a finished sealing strip.
[0101] The first drying oven in S1 is heated at 100° C. for four hours, and the second drying oven is heated at 70° C. for three hours;
[0102] The initial plasticizing temperature in S3 is 135°C-145°C;
[0103] The continued plasticizing temperature in S4 is 150°C-160°C;
[0104] The complete plasticization temperature in S5 is 155°C-175°C;
[0105] The S6 filter screen is 20 mesh × 40 mesh × 150 mesh × 40 mesh × 20 mesh;
[0106] The extrusion temperature of the extruder in S7 is 180° C.-185° C., and the screw compression ratio in the extruder is 2.5-3.5:1.
[0107] Example 3
[0108] By weight, the following substances
[0109] TPU resin: 95 parts;
[0110] Modified nano-scale silica: 5 parts;
[0111] Silane crosslinking agent: 5 parts;
[0112] Stearic acid amide: 5 parts;
[0113] ADPA: 2.5 parts;
[0114] BHA: 2.5 parts;
[0115] Matte additive: 5 parts.
[0116] The preparation was carried out by the following steps.
[0117] Preparation of the modified nano-scale silicon dioxide: The nano-scale silicon dioxide is put into a nano-grinder at least once for grinding to obtain the modified nano-scale silicon dioxide.
[0118] S1: Put TPU resin into the first drying oven for drying, and put modified nano-silica, coupling agent, lubricant, composite antioxidant and matte additive into the second drying oven;
[0119] S2: Mix the dried TPU resin, modified nano-silica, coupling agent, lubricant, composite antioxidant and matte additive in S1 and put them into a high-speed kneader for stirring and mixing evenly;
[0120] S3: Put the mixed materials in S2 into an internal mixer for preliminary plasticization;
[0121] S4: heating the material in S3 and continuing plasticization;
[0122] S5: heating the material in S4 until it is completely plasticized and begins to be used for feeding;
[0123] S6: The completely plasticized material in S5 is passed through a filter to remove impurities.
[0124] S7: the material from which impurities are removed in S6 is extruded through an extruder and sent to a casting machine, and pressed to a desired thickness to form a film;
[0125] S8: pulling the film in S7 onto the embossing wheel;
[0126] S9: embossing one side of the film in S8;
[0127] S10: embossing the other side of the film in S9;
[0128] S11: Cooling the film after embossing in S10 through a cooling mechanism;
[0129] S12: rolling up the film cooled in S11 and placing it for cooling and solidification;
[0130] S13: Cutting the film cured in S12 into required specifications to obtain a finished sealing strip.
[0131] The first drying oven in S1 is heated at 100° C. for four hours, and the second drying oven is heated at 70° C. for three hours;
[0132] The initial plasticizing temperature in S3 is 135°C-145°C;
[0133] The continued plasticizing temperature in S4 is 150°C-160°C;
[0134] The complete plasticization temperature in S5 is 155°C-175°C;
[0135] The S6 filter screen is 20 mesh × 40 mesh × 150 mesh × 40 mesh × 20 mesh;
[0136] The extrusion temperature of the extruder in S7 is 180° C.-185° C., and the screw compression ratio in the extruder is 2.5-3.5:1.
[0137] Comparative Example 1
[0138] By weight, the following substances
[0139] TPU resin: 90 parts;
[0140] Nano-silicon dioxide: 3 parts;
[0141] Silane coupling agent: 3 parts;
[0142] Stearic acid amide: 3 parts;
[0143] ADPA: 1.5 parts;
[0144] BHA: 1.5 parts;
[0145] Matting agent: 3 parts.
[0146] The preparation was carried out by the following steps.
[0147] S1: Put TPU resin into the first drying oven for drying, and put nano-silica, coupling agent, lubricant, composite antioxidant and matte additive into the second drying oven;
[0148] S2: Mix the dried TPU resin, nano-silica, coupling agent, lubricant, composite antioxidant and matte additive in S1 and put them into a high-speed kneader for stirring and mixing evenly;
[0149] S3: Put the mixed materials in S2 into an internal mixer for preliminary plasticization;
[0150] S4: heating the material in S3 and continuing plasticization;
[0151] S5: heating the material in S4 until it is completely plasticized and begins to be used for feeding;
[0152] S6: The completely plasticized material in S5 is passed through a filter to remove impurities.
[0153] S7: the material from which impurities are removed in S6 is extruded through an extruder and sent to a casting machine, and pressed to a desired thickness to form a film;
[0154] S8: pulling the film in S7 onto the embossing wheel;
[0155] S9: embossing one side of the film in S8;
[0156] S10: embossing the other side of the film in S9;
[0157] S11: Cooling the film after embossing in S10 through a cooling mechanism;
[0158] S12: rolling up the film cooled in S11 and placing it for cooling and solidification;
[0159] S13: Cutting the film cured in S12 into required specifications to obtain a finished sealing strip.
[0160] The first drying oven in S1 is heated at 100° C. for four hours, and the second drying oven is heated at 70° C. for three hours;
[0161] The initial plasticizing temperature in S3 is 135°C-145°C;
[0162] The continued plasticizing temperature in S4 is 150°C-160°C;
[0163] The complete plasticization temperature in S5 is 155°C-175°C;
[0164] The S6 filter screen is 20 mesh × 40 mesh × 150 mesh × 40 mesh × 20 mesh;
[0165] The extrusion temperature of the extruder in S7 is 180° C.-185° C., and the screw compression ratio in the extruder is 2.5-3.5:1.
[0166] Comparative Example 2
[0167] By weight, the following substances
[0168] TPU resin: 90 parts;
[0169] Silane coupling agent: 3 parts;
[0170] Stearic acid amide: 3 parts;
[0171] ADPA: 1.5 parts;
[0172] BHA: 1.5 parts;
[0173] Matting agent: 3 parts.
[0174] S1: Put TPU resin into the first drying oven for drying, and put coupling agent, lubricant, composite antioxidant and matte additive into the second drying oven;
[0175] S2: Mix the dried TPU resin, coupling agent, lubricant, composite antioxidant and matte additive in S1 and put them into a high-speed kneader for stirring and mixing evenly;
[0176] S3: Put the mixed materials in S2 into an internal mixer for preliminary plasticization;
[0177] S4: heating the material in S3 and continuing plasticization;
[0178] S5: heating the material in S4 until it is completely plasticized and begins to be used for feeding;
[0179] S6: The completely plasticized material in S5 is passed through a filter to remove impurities.
[0180] S7: the material from which impurities are removed in S6 is extruded through an extruder and sent to a casting machine, and pressed to a desired thickness to form a film;
[0181] S8: pulling the film in S7 onto the embossing wheel;
[0182] S9: embossing one side of the film in S8;
[0183] S10: embossing the other side of the film in S9;
[0184] S11: Cooling the film after embossing in S10 through a cooling mechanism;
[0185] S12: rolling up the film cooled in S11 and placing it for cooling and solidification;
[0186] S13: Cutting the film cured in S12 into required specifications to obtain a finished sealing strip.
[0187] The first drying oven in S1 is heated at 100° C. for four hours, and the second drying oven is heated at 70° C. for three hours;
[0188] The initial plasticizing temperature in S3 is 135°C-145°C;
[0189] The continued plasticizing temperature in S4 is 150°C-160°C;
[0190] The complete plasticization temperature in S5 is 155°C-175°C;
[0191] The S6 filter screen is 20 mesh × 40 mesh × 150 mesh × 40 mesh × 20 mesh;
[0192] The extrusion temperature of the extruder in S7 is 180° C.-185° C., and the screw compression ratio in the extruder is 2.5-3.5:1.
[0193] Comparative Example 3
[0194] By weight, the following substances
[0195] TPU resin: 90 parts;
[0196] Modified nano-scale silica: 3 parts;
[0197] Silane coupling agent: 3 parts;
[0198] ADPA: 1.5 parts;
[0199] BHA: 1.5 parts;
[0200] Matting agent: 3 parts.
[0201] The preparation was carried out by the following steps.
[0202] Preparation of the modified nano-scale silicon dioxide: The nano-scale silicon dioxide is put into a nano-grinder at least once for grinding to obtain the modified nano-scale silicon dioxide.
[0203] S1: Put TPU resin into the first drying oven for drying, and put modified nano-silica, coupling agent, composite antioxidant and matte additive into the second drying oven;
[0204] S2: Mix the dried TPU resin, modified nano-silica, coupling agent, composite antioxidant and matte additive in S1 and put them into a high-speed kneader for stirring and mixing evenly;
[0205] S3: Put the mixed materials in S2 into an internal mixer for preliminary plasticization;
[0206] S4: heating the material in S3 and continuing plasticization;
[0207] S5: heating the material in S4 until it is completely plasticized and begins to be used for feeding;
[0208] S6: The completely plasticized material in S5 is passed through a filter to remove impurities.
[0209] S7: the material from which impurities are removed in S6 is extruded through an extruder and sent to a casting machine, and pressed to a desired thickness to form a film;
[0210] S8: pulling the film in S7 onto the embossing wheel;
[0211] S9: embossing one side of the film in S8;
[0212] S10: embossing the other side of the film in S9;
[0213] S11: Cooling the film after embossing in S10 through a cooling mechanism;
[0214] S12: rolling up the film cooled in S11 and placing it for cooling and solidification;
[0215] S13: Cutting the film cured in S12 into required specifications to obtain a finished sealing strip.
[0216] The first drying oven in S1 is heated at 100° C. for four hours, and the second drying oven is heated at 70° C. for three hours;
[0217] The initial plasticizing temperature in S3 is 135°C-145°C;
[0218] The continued plasticizing temperature in S4 is 150°C-160°C;
[0219] The complete plasticization temperature in S5 is 155°C-175°C;
[0220] The S6 filter screen is 20 mesh × 40 mesh × 150 mesh × 40 mesh × 20 mesh;
[0221] The extrusion temperature of the extruder in S7 is 180° C.-185° C., and the screw compression ratio in the extruder is 2.5-3.5:1.
[0222] Comparative Example 4
[0223] By weight, the following substances
[0224] TPU resin: 90 parts;
[0225] Modified nano-scale silica: 3 parts;
[0226] Silane coupling agent: 3 parts;
[0227] Stearic acid amide: 3 parts;
[0228] ADPA: 1.5 parts;
[0229] BHA: 1.5 parts;
[0230] Matting agent: 3 parts.
[0231] The preparation was carried out by the following steps.
[0232] Preparation of the modified nano-scale silicon dioxide: The nano-scale silicon dioxide is put into a nano-grinder at least once for grinding to obtain the modified nano-scale silicon dioxide.
[0233] S1: putting the TPU resin into the first drying box for drying;
[0234] S2: Mix the dried TPU resin, modified nano-silica, coupling agent, lubricant, composite antioxidant and matte additive in S1 and put them into a high-speed kneader for stirring and mixing evenly;
[0235] S3: Put the mixed materials in S2 into an internal mixer for preliminary plasticization;
[0236] S4: heating the material in S3 and continuing plasticization;
[0237] S5: heating the material in S4 until it is completely plasticized and begins to be used for feeding;
[0238] S6: The completely plasticized material in S5 is passed through a filter to remove impurities.
[0239] S7: the material from which impurities are removed in S6 is extruded through an extruder and sent to a casting machine, and pressed to a desired thickness to form a film;
[0240] S8: pulling the film in S7 onto the embossing wheel;
[0241] S9: embossing one side of the film in S8;
[0242] S10: embossing the other side of the film in S9;
[0243] S11: Cooling the film after embossing in S10 through a cooling mechanism;
[0244] S12: rolling up the film cooled in S11 and placing it for cooling and solidification;
[0245] S13: Cutting the film cured in S12 into required specifications to obtain a finished sealing strip.
[0246] The first drying box in S1 is heated to 100° C. for four hours;
[0247] The initial plasticizing temperature in S3 is 135°C-145°C;
[0248] The continued plasticizing temperature in S4 is 150°C-160°C;
[0249] The complete plasticization temperature in S5 is 155°C-175°C;
[0250] The S6 filter screen is 20 mesh × 40 mesh × 150 mesh × 40 mesh × 20 mesh;
[0251] The extrusion temperature of the extruder in S7 is 180° C.-185° C., and the screw compression ratio in the extruder is 2.5-3.5:1.
[0252] Comparative Example 5
[0253] By weight, the following substances
[0254] TPU resin: 90 parts;
[0255] Silane coupling agent: 3 parts;
[0256] ADPA: 1.5 parts;
[0257] BHA: 1.5 parts;
[0258] Matting agent: 3 parts.
[0259] The preparation was carried out by the following steps.
[0260] S1: Put the TPU resin into the first drying oven for drying, and put the coupling agent, composite antioxidant and matte additive into the second drying oven;
[0261] S2: Mix the dried TPU resin, coupling agent, composite antioxidant and matte additive in S1 and put them into a high-speed kneader for stirring and mixing evenly;
[0262] S3: Put the mixed materials in S2 into an internal mixer for preliminary plasticization;
[0263] S4: heating the material in S3 and continuing plasticization;
[0264] S5: heating the material in S4 until it is completely plasticized and begins to be used for feeding;
[0265] S6: The completely plasticized material in S5 is passed through a filter to remove impurities.
[0266] S7: the material from which impurities are removed in S6 is extruded through an extruder and sent to a casting machine, and pressed to a desired thickness to form a film;
[0267] S8: pulling the film in S7 onto the embossing wheel;
[0268] S9: embossing one side of the film in S8;
[0269] S10: embossing the other side of the film in S9;
[0270] S11: Cooling the film after embossing in S10 through a cooling mechanism;
[0271] S12: rolling up the film cooled in S11 and placing it for cooling and solidification;
[0272] S13: Cutting the film cured in S12 into required specifications to obtain a finished sealing strip.
[0273] The first drying oven in S1 is heated at 100° C. for four hours, and the second drying oven is heated at 70° C. for three hours;
[0274] The initial plasticizing temperature in S3 is 135°C-145°C;
[0275] The continued plasticizing temperature in S4 is 150°C-160°C;
[0276] The complete plasticization temperature in S5 is 155°C-175°C;
[0277] The S6 filter screen is 20 mesh × 40 mesh × 150 mesh × 40 mesh × 20 mesh;
[0278] The extrusion temperature of the extruder in S7 is 180° C.-185° C., and the screw compression ratio in the extruder is 2.5-3.5:1.
[0279] The sealing strip samples prepared in the above-mentioned Examples 1-3 and Comparative Examples 1-5 were tested, as shown in Table 1 and Table 2 for details.
[0280] Table 1
[0281]
[0282] Table 2
[0283]
[0284] From Examples 1-3 in Table 1 above, it can be seen that with the increase of each component, the performance of the finished film is gradually improved; from Comparative Examples 1-3 in Table 2 above, it can be seen that modified nano-scale silica, nano-scale silica and lubricant all improve the various properties of the finished film to a certain extent. It should be noted here that the modified nano-scale silica is better than nano-scale silica; from Comparative Example 4 in Table 2 above compared with Example 2 in Table 1, it can be seen that TPU has a large polarity and is hygroscopic, so it must be dehumidified before use. In addition, dehumidification of other raw materials greatly increases the various properties of the obtained finished product: from Comparative Example 5 in Table 2 above compared with Example 2 in Table 1, the lubricant and modified silica produce a synergistic effect, which greatly increases the performance of TPU.
[0285] The embodiments described above are only preferred implementation modes of the present invention and cannot be used to limit the protection scope of the present invention. Any non-substantial changes and modifications made by those skilled in the art on the basis of the present invention shall fall within the protection scope of the present invention.
Claims
1. A sealing strip, characterized in that: By weight, it includes the following components: TPU resin: 85-95 parts; Modified nano-scale silicon dioxide: 1-5 parts, the nano-scale silicon dioxide is put into a nano-grinder at least once for grinding to obtain the modified nano-scale silicon dioxide; Coupling agent: 1-5 parts, the coupling agent is at least one of a silane coupling agent, an aluminate coupling agent, a rare earth coupling agent, and an aluminum-titanium coupling agent; Lubricant: 1-5 parts; Compound antioxidant: 1-5 parts; The composite antioxidant is a phenolic antioxidant and an amine antioxidant in any ratio; The sealing strip production process comprises the following preparation steps: S1: Put TPU resin into the first drying oven for drying, and put modified nano-silica, coupling agent, lubricant and composite antioxidant into the second drying oven; S2: Mix the dried TPU resin, modified nano-silica, coupling agent, lubricant and composite antioxidant in S1 and put them into a high-speed kneader for stirring and mixing evenly; S3: Put the mixed materials in S2 into an internal mixer for preliminary plasticization; S4: heating the material in S3 and continuing plasticization; S5: heating the material in S4 until it is completely plasticized and begins to be used for feeding; S6: passing the completely plasticized material in S5 through a filter to remove impurities; S7: the material from which impurities are removed in S6 is extruded through an extruder and sent to a casting machine, and pressed to a desired thickness to form a film; S8: pulling the film in S7 onto the embossing wheel; S9: embossing one side of the film in S8; S10: embossing the other side of the film in S9; S11: Cooling the film after embossing in S10 through a cooling mechanism; S12: rolling up the film cooled in S11 and placing it for cooling and solidification; S13: cutting the film cured in S12 into required specifications, thereby obtaining a finished sealing strip; The first drying oven in S1 is heated at 100° C. for four hours, and the second drying oven is heated at 70° C. for three hours; The initial plasticizing temperature in S3 is 135°C-145°C; The continued plasticizing temperature in S4 is 150°C-160°C; The complete plasticization temperature in S5 is 155°C-175°C; The S6 filter screen is 20 mesh × 40 mesh × 150 mesh × 40 mesh × 20 mesh; The extrusion temperature of the extruder in S7 is 180° C.-185° C., and the screw compression ratio in the extruder is 2.5-3.5:
1.
2. A sealing strip according to claim 1, characterized in that: The amine antioxidant is at least one of diaryl secondary amine and tetraethylenepentamine.
3. A sealing strip according to claim 2, characterized in that: The phenolic antioxidant is at least one of 2,6-dimethylphenol, 2,4,5-trihydroxybutyrophenone, PTBP, BHT, BHA, PG and TBHQ.
4. A sealing strip according to claim 1, characterized in that: The lubricant is one of oleamide, erucamide and stearamide.