Deoxime type RTV organic silicon sealant and preparation method thereof
By combining modified tackifier and silica with alkoxy silicone resin, the problem of degradation of mechanical properties of organic silicone adhesives after humid and heat aging is solved, and the resistance of high-temperature water steam cooking and high-temperature water boiling is achieved, and the Good gloss and economy.
Patent Information
- Application Number
- CN202310158201.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-23
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-02-23
AI Technical Summary
The mechanical properties of existing silicone adhesives decrease after moisture and heat aging, making it difficult to meet the application conditions of high-temperature water steam cooking and high-temperature water boiling, and the preparation process is complex and costly.
Prepare from specific monomer reaction using a modified tackifier, combined with silica and alkoxy silicone resin, to form a deoxime-type RTV silicone sealant, and improve its moisture and heat resistance and boiling resistance through improved composition, and maintain good performance. Gloss.
After double 85 test, the mechanical properties retention rate is ≥90%, the mechanical properties retention rate is ≥85% after boiling for 24 hours, and the mechanical properties retention rate is ≥85% after steam aging for 24 hours, while maintaining good gloss. It is suitable for harsh Application occasion.
Smart Images

Figure FDA0004093256110000011 
Figure FDA0004093256110000021 
Figure FDA0004093256110000022
Abstract
Description
Technical Field
[0001] The invention relates to an organic silicon sealant having excellent moisture and heat resistance and water boiling resistance and excellent reliability. Technical Background
[0002] RTV room temperature vulcanized silicone rubber is widely used in construction, electronics, and other fields due to its outstanding high and low temperature resistance, electrical insulation, and weather resistance. The rapidly developing home appliance industry places increasingly stringent requirements on adhesive applications, including higher requirements for adhesive resistance to high temperatures, high temperature moisture, and acid and alkali. However, the mechanical properties of currently produced silicone adhesives on the market often degrade significantly after wet heat aging (double "85"). They can initially bond to substrates, but their bonding performance degrades significantly after wet heat aging testing. They also struggle to meet the more demanding requirements for long-term high-temperature steam cooking and high-temperature water boiling applications. This presents an urgent problem that needs to be addressed for room temperature vulcanized silicone rubber in special applications such as home appliances.
[0003] CN104031389A discloses a room temperature vulcanized silicone rubber composition that is resistant to moisture and heat. By reacting an amino-containing silane coupling agent with an epoxy-containing silane coupling agent under certain conditions, the effect of the amino-containing silane coupling agent on the moisture and heat resistance of the RTV silicone rubber is improved without significantly reducing the bonding strength of the RTV silicone rubber. However, the adhesive is not resistant to boiling water after curing. CN102424742B discloses a two-component condensation-type room temperature vulcanized silicone rubber that is resistant to moisture and heat aging. Component A includes an organic compound with an epoxy group that can react with component B. The aminosilane in the adhesive can react at room temperature to improve the moisture and heat resistance of the silicone rubber. However, the adhesive is not resistant to boiling water after curing, and the two-component adhesive is inconvenient to use. CN115073750A discloses a moisture and heat-resistant room-temperature curing silicone rubber and a preparation method thereof. POSS organic polysilazane is designed. After adding it to silicone rubber, it can effectively prevent the moisture and heat aging of the silicone rubber and improve the heat resistance and mechanical properties of the silicone rubber. However, the synthesis process of POSS organic polysilazane is complicated and the cost is high, and the adhesive is not resistant to boiling water after curing. Summary of the Invention
[0004] In order to solve the problems existing in the above-mentioned prior art, the purpose of the present invention is to disclose a deoximated RTV silicone sealant and a preparation method thereof. The deoximated RTV silicone sealant is a deoximated curing system. By improving the composition, it has excellent resistance to moisture and heat, resistance to boiling water and reliability, and at the same time, the appearance does not deteriorate after aging.
[0005] The technical solutions provided by the present invention are as follows:
[0006] A modified tackifier is prepared by reacting the following monomers:
[0007] R 1 Si(OR6 )3Formula 1,
[0008] R 1 R 2 Si(OR 7 )2Formula 2,
[0009] R 3 Si(OR 8 )3Formula 3,
[0010] R 3 R 4 Si(OR 9 )2Formula 4,
[0011] (OR 10 )3SiR 5 Si(OR 10 )3Formula 5,
[0012] In Formula 1 and Formula 2, R 1 is a group containing an epoxy group, an ester group or an acryloyloxy group. In Formula 3 and Formula 4, R 3 is a group containing -NH-, in formula 5 R 5 is a divalent group containing -NH-, in Formula 2 and Formula 4, R 2 、R 4 Represents the same or different monovalent hydrocarbon groups, R in Formula 1-Formula 5 6 、R 7 、R 8 、R 9 、R 10 represents the same or different alkyl groups.
[0013] The molar amounts of the monomer represented by Formula 1, the monomer represented by Formula 2, the monomer represented by Formula 3, the monomer represented by Formula 4, and the monomer represented by Formula 5 are a, b, c, d, and e, respectively. Preferably, a>0, b≥0, c≥0, d≥0, e≥0, c+d+e≠0, (a+b):(c+d+e)=1:(1~3).
[0014] More preferably, 0≤b / a<0.6.
[0015] More preferably, 0≤d / (c+d+e)<0.25.
[0016] In Formula 1 and Formula 2, R 1 is a group containing epoxy, ester or acryloyloxy, preferably, R 1 for R 0represents a C1-C5 alkyl group, specifically a methyl, ethyl, propyl, tert-butyl or similar saturated alkyl group, more preferably a methyl group, and m, n, and r are all integers greater than zero and less than or equal to 3. R in Formula 1 and Formula 2 1 Can be the same or different.
[0017] In formula 3 and formula 4, the R 3 is a group containing -NH-, preferably, the R 3 The structural formula is x represents an integer greater than zero and less than or equal to 3, R 11 represents a monovalent hydrocarbon group, and examples thereof include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl or similar alkyl groups; cyclopentyl, cyclohexyl or similar cycloalkyl groups; phenyl, tolyl, xylyl or similar aryl groups; benzyl, phenethyl, phenylpropyl or similar aralkyl groups; among the above, alkyl and cycloalkyl groups are most preferred, especially methyl and cyclohexyl groups. 3 Can be the same or different.
[0018] In formula 5, R 5 is a divalent group containing -NH-, preferably, the R 5 The structural formula is
[0019] s and y represent integers greater than zero and less than or equal to 3.
[0020] In Formula 2 and Formula 4, R 2 、R 4 The same or different monovalent hydrocarbon groups may be exemplified by methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl or similar alkyl groups; cyclopentyl, cyclohexyl or similar cycloalkyl groups; phenyl, tolyl, xylyl or similar aryl groups; benzyl, phenethyl, phenylpropyl or similar aralkyl groups; 3,3,3-trifluoropropyl, 3-chloropropyl or similar halogenated alkyl groups; the most preferred of the above are alkyl and aryl groups, especially methyl and phenyl groups.
[0021] In Formula 1-Formula 5, OR 6 , OR 7 , OR 8 , OR 9 , OR 10 It is a group that can undergo hydrolysis and condensation. 6 、R 7 、R 8 、R 9 、R 10 represents the same or different alkyl groups, specifically methyl, ethyl, propyl, tert-butyl and similar saturated alkyl groups, more preferably methyl.
[0022] Further preferably, the monomer represented by formula 1 is one or more of γ-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane or β-(3,4-epoxycyclohexylethyl)trimethoxysilane.
[0023] More preferably, the monomer represented by Formula 2 is one or more of 3-glycidyloxypropylmethyldiethoxysilane, 3-methacryloxypropylmethyldimethoxysilane or β-(3,4-epoxycyclohexylethyl)methyldimethoxysilane.
[0024] Further preferably, the monomer represented by formula 3 is N-(n-butyl)-γ-aminopropyltriethoxysilane, N-(n-butyl)-γ-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-methyl-3-aminopropyltrimethoxysilane, N-methyl-3-aminopropyltriethoxysilane, cyclohexylaminomethyltriethoxysilane One or more of the .
[0025] More preferably, the monomer represented by formula 4 is N-methylaminopropylmethyldimethoxysilane, N-cyclohexyl-γ-aminopropylmethyldimethoxysilane, cyclohexylaminomethylmethyldiethoxysilane or aniline methyl dimethoxysilane
[0026]
[0027] More preferably, the monomer represented by Formula 5 is one or more of di(3-trimethoxysilylpropyl)amine, bis[(3-(triethoxysilyl)propyl)]ethylenediamine or di(3-triethoxysilylpropyl)amine.
[0028] Preferably, the modified tackifier has a dynamic viscosity of 10 to 120 mPa·s at 25°C.
[0029] Preferably, the preparation method of the modified tackifier comprises at least the following steps:
[0030] A. Mix the monomer represented by formula 1, the monomer represented by formula 2, the monomer represented by formula 3, the monomer represented by formula 4, the monomer represented by formula 5, a solvent and a hydrolysis condensation catalyst, stir at a temperature of 40° C. to 60° C. and add water dropwise to react. After the addition is complete, heat to 70° C. to 80° C. and continue the reaction for 1 to 3 hours;
[0031] B. Cool to room temperature, add neutralizing agent to neutralize, wash with water until neutral, and then remove water and solvent by distillation under reduced pressure;
[0032] C. Cool to room temperature, add end-capping agent and alkaline catalyst, heat to 80-100°C and react for 1-3 hours, break the catalyst and remove low molecular weight by vacuum distillation to obtain a modified tackifier.
[0033] Preferably, in step A, the hydrolysis and condensation catalyst is trifluoromethanesulfonic acid, hydrochloric acid, phosphoric acid, acetic acid, or a strongly acidic cationic resin, and its amount is not particularly limited. Preferably, in step A, the mass of the water is 25% to 40% of the total mass of the monomers represented by Formula 1, the monomers represented by Formula 2, the monomers represented by Formula 3, the monomers represented by Formula 4, and the monomers represented by Formula 5.
[0034] Preferably, in step A, the solvent is ethanol or methanol, or a mixed solvent of methanol and toluene, or a mixed solvent of ethanol and toluene, and its mass is 1-3 times the total mass of the monomer represented by Formula 1, the monomer represented by Formula 2, the monomer represented by Formula 3, the monomer represented by Formula 4, and the monomer represented by Formula 5.
[0035] Preferably, in step B, the neutralizing agent is preferably sodium carbonate or sodium bicarbonate, and the amount thereof is not particularly limited.
[0036] Preferably, in step B, the temperature of the reduced pressure distillation is 80-100° C., and the substances removed in this step also include reaction products such as small molecule alcohols.
[0037] In step C, the end-capping agent is preferably hexamethyldisiloxane, and the mass of the end-capping agent is 0.2 to 0.6% of the total mass of the monomers represented by formula 1, the monomers represented by formula 2, the monomers represented by formula 3, the monomers represented by formula 4, and the monomers represented by formula 5.
[0038] Preferably, in step C, the alkaline catalyst is tetramethylammonium hydroxide, and the mass of the alkaline catalyst is 0.003-0.006% of the total mass of the monomer represented by Formula 1, the monomer represented by Formula 2, the monomer represented by Formula 3, the monomer represented by Formula 4, and the monomer represented by Formula 5. The alkaline catalyst can be removed by decomposition by heating, and the removal of low molecular weight substances in step C is the removal of unreacted low molecular weight substances such as the end-capping agent.
[0039] A deoxime-type RTV organosilicon sealant comprising the following components:
[0040] (A) diorganopolysiloxane terminated with hydroxyl or alkoxy groups
[0041] (B) Oxime silane crosslinker
[0042] (C) Filler
[0043] (D) Modified tackifier
[0044] (E) a catalyst and (F) an alkoxy silicone resin;
[0045] The (D) modified tackifier is the modified tackifier described above.
[0046] The (A) is an average composition formula of R'SiO (4-g) / 2 A diorganopolysiloxane wherein R' is a substituted or unsubstituted monovalent hydrocarbon group, preferably a monovalent hydrocarbon group having 1 to 10 carbon atoms. The monovalent hydrocarbon group may be an alkyl group such as methyl, ethyl, propyl, and butyl, an aralkyl group such as benzyl and 2-phenylethyl, or a substituted hydrocarbon group in which some or all of the hydrogen atoms in the above groups are replaced by halogen atoms or similar groups, such as chloromethyl and 3,3,3-trifluoropropyl. Preferably, g is 1.8 to 2.1. Preferably, the alkoxy group is selected from C1-C3 alkoxy groups.
[0047] Preferably, the dynamic viscosity of (A) at 25° C. is 500-80,000 mPa.s. More preferably, the dynamic viscosity of (A) at 25° C. is 5,000-20,000 mPa.s.
[0048] The (B) oxime silane crosslinking agent is preferably one or more of methyltributylanoxime silane, vinyltributylanoxime silane, phenyltributylanoxime silane, and tetrabutylketoxime silane. Preferably, the amount of the (B) oxime silane crosslinking agent is 6 to 12 parts by weight per 100 parts by weight of (A).
[0049] Preferably, the filler (C) comprises fumed silica or precipitated silica, and the specific surface area of the fumed silica or precipitated silica is 100 to 400 m 2 / g. Preferably, the filler (C) is a surface-treated filler, and the surface treatment agent used for the surface treatment includes one or more of hexamethyldisilazane, dimethyldichlorosilane, and hydroxy silicone oil. In applications, the filler (C) may also include other types of functional fillers, such as thermally conductive fillers, flame-retardant fillers, electrically conductive fillers, and pigment fillers, with no particular limitation on the specific types.
[0050] Preferably, the (C) filler is a surface-treated filler. The surface treatment method is not particularly limited and can be carried out by referring to existing methods. Preferably, a wet surface modification treatment is performed, comprising the following steps: dispersing the filler in an organic solvent, adding a surface treatment agent under inert gas conditions and stirring and dispersing the filler, isolating the filler from air at 80-100°C and stirring the mixture for 12-24 hours, cooling the mixture to room temperature, separating, washing, and drying the filler to obtain a surface-treated filler.
[0051] Preferably, the filler (C) is fumed silica or precipitated silica, and the amount of the fumed silica or precipitated silica is 10-15 parts by weight per 100 parts by weight of component (A). The amount of fumed silica or precipitated silica affects the moisture-heat aging resistance of the silica gel composition, including that when the amount is too small, the glossiness of the colloid appearance will be affected after moisture-heat aging, and when the amount is too large, the processing performance of the composition will be poor.
[0052] Preferably, the filler (C) further comprises silicon micropowder, and the amount of the silicon micropowder is 0 to 15 parts per 100 parts by weight of component (A).
[0053] Preferably, for every 100 parts by weight of component (A), the amount of the modified tackifier (D) is 1.5-4 parts by weight.
[0054] The catalyst (E) is preferably a condensation catalyst containing tin, lead, antimony, iron, cadmium, or bismuth. Examples include organotin metal catalysts such as dibutyltin dilaurate, dibutyltin diacetate, dioctyltin dilaurate, stannous octoate, dibutyltin diacetate, bis(tin acetylacetonate), and the like.
[0055] The mass of the (E) catalyst is 0.2%-0.5% of the mass of the (A) diorganopolysiloxane terminated with hydroxyl or alkoxy groups, so as to have a suitable surface drying and curing time. At the same time, excessive use of the (E) catalyst will affect the aging resistance of the sealant, and the performance will seriously deteriorate after aging.
[0056] Preferably, the alkoxy groups in the (F) alkoxy silicone resin are C1-C3 alkoxy groups, and the alkoxy content is 4 to 12%.
[0057] The alkoxy content of the alkoxy silicone resin (F) in the present invention is the mass percentage of the alkoxy group, and the testing method is referred to CN105424642A.
[0058] Preferably, the (F) alkoxy silicone resin has an M / Q value of 0.6 to 0.9 and a weight-average molecular weight of 2000 to 8000, and commercial silicone resin products can be used directly.
[0059] Preferably, the amount of the alkoxy silicone resin (F) is 5 to 15 parts by weight for every 100 parts by weight of component (A). The alkoxy silicone resin in the present invention not only helps improve the mechanical properties of the sealant after curing, but also helps improve the heat and humidity resistance and water boiling resistance of the silicone rubber. The alkoxylated resin is more easily cross-linked with component (A) and the cross-linking agent. If the amount of alkoxy silicone resin is too low, the heat and humidity aging resistance will be severely degraded, and the appearance of the colloid after aging will deteriorate, including a decrease in gloss.
[0060] A deoxime-type RTV organosilicon sealant is prepared from the components (A), (B), (C), (D), (E), and (F). The preparation method comprises: mixing the components (A), (B), (C), (D), (E), and (F) under vacuum conditions, and then sealing and packaging to obtain the deoxime-type RTV organosilicon sealant. Preferably, the preparation method comprises: heating the components (A), (C), and (F), vacuuming and stirring to mix, cooling the components, adding (B), vacuuming and stirring to mix, and then adding (D) and (E), vacuuming and stirring to mix, and sealing and discharging to obtain the deoxime-type RTV organosilicon sealant.
[0061] Compared with the prior art, the present invention has the following advantages:
[0062] The present invention solves the technical problems of moisture and heat resistance and boiling resistance of deoxime type RTV organic silicone sealant after curing by combining a modified tackifier, silicon dioxide and silicone resin, thereby obtaining a single-component deoxime type RTV organic silicone sealant with excellent curing performance, moisture and heat resistance and boiling resistance. In application, the sealant has a mechanical property retention rate of ≥90% after 168 hours of double 85 test, a mechanical property retention rate of ≥85% after 24 hours of boiling in water, and a mechanical property retention rate of ≥85% after 24 hours of water vapor aging test, while still maintaining good gloss. The product has good application prospects. DETAILED DESCRIPTION
[0063] The present invention is further illustrated by the following specific examples.
[0064] Example 1
[0065] 200 g of ethanol, 50 g of γ-glycidyloxypropyltrimethoxysilane, 150 g of bis(3-trimethoxysilylpropyl)amine and 0.1 g of hydrochloric acid with a mass fraction of approximately 37% were weighed and added to a flask. The mixture was heated to 50° C. and stirred while adding water dropwise to react. The amount of water added was 60 g. After the addition was complete, the mixture was heated to 70° C. and the reaction was continued for 2 hours. The mixture was cooled to room temperature and 2 g of sodium bicarbonate was added for neutralization and washed with water until neutral. The mixture was then heated to 100° C. and distilled under reduced pressure to remove water and ethanol. Subsequently, 1 g of hexamethyldisiloxane and 0.01 g of tetramethylammonium hydroxide were added at room temperature. The mixture was heated to 90° C. and reacted for 2 hours, followed by breaking the medium and removing low molecular weight substances by distillation under reduced pressure to obtain a modified tackifier 1. The dynamic viscosity at 25° C. was 80 mPa·s.
[0066] In a planetary mixer, add 100g of α, ω-dihydroxypolydimethylsiloxane (dynamic viscosity at 25°C is 5000mPa.s), add 10g of hydrophobic fumed silica (manufacturer: Evonik Degussa, model: R202), add 15g of alkoxy silicone resin (manufacturer: Longsheng Sihai, model: SH-3021S, weight average molecular weight: 2500, mass percentage of alkoxy group: 12%), heat to 100°C, vacuum-mix, and mix for 1h, then cool to room temperature, first add 12g of methyl tributylidene oxime silane, vacuum-mix, and mix for 30min, then add 4g of modified tackifier 1 and 0.3g of dibutyltin dilaurate, vacuum-mix, and mix for 30min, finally put into a sealed tube and seal for storage to obtain a silicone sealant.
[0067] Example 2
[0068] Weigh 215g of ethanol, 70g of γ-glycidyloxypropyltrimethoxysilane, 15g of 3-glycidyloxypropylmethyldiethoxysilane, 130g of di(3-trimethoxysilylpropyl)amine and 0.1g of hydrochloric acid with a mass fraction of about 37% and add them to a flask. Heat to 50°C and add water dropwise while stirring to react. The amount of water added is 64.5g. After the addition is complete, heat to 80°C and continue to react for 3 hours. Cool to room temperature, add 2g of sodium bicarbonate to neutralize and wash with water until neutral. Heat to 100°C and remove water and ethanol by vacuum distillation. Then cool to room temperature and add 0.43g of hexamethyldisiloxane and 0.01g of tetramethylammonium hydroxide. After reacting at 100°C for 3 hours, break the medium and remove low-molecular substances by vacuum distillation to obtain modified tackifier 2. The dynamic viscosity value at 25°C is 100mPa·s.
[0069] In a planetary mixer, add 100g of α, ω-dihydroxypolydimethylsiloxane (dynamic viscosity at 25°C is 20000mPa.s), add 15g of hydrophobic fumed silica (manufacturer: Cabot, model: TS530), add 5g of alkoxy silicone resin (manufacturer: Longsheng Sihai, model: SH-5201, weight average molecular weight: 5000, mass percentage of alkoxy: 6%), heat to 100°C, vacuum stir and mix for 1h, then cool to room temperature, first add 8g of methyl tributylidene oxime silane, vacuum stir and mix for 30min, then add 1.5g of modified tackifier 2 and 0.3g of dibutyltin dilaurate, vacuum stir and mix for 30min, finally put into a sealed tube and seal and store to obtain a silicone sealant.
[0070] Example 3
[0071] Weigh 350g of ethanol, 80g of γ-glycidyloxypropyltrimethoxysilane, 50g of 3-glycidyloxypropylmethyldiethoxysilane, 120g of N-phenyl-3-aminopropyltrimethoxysilane, 100g of di(3-triethoxysilylpropyl)amine and 0.175g of acetic acid into a flask, and add water dropwise while stirring at 50°C to react. The amount of water added is 105g. After the addition is complete, heat to 70°C and continue the reaction for 1 hour. Cool to room temperature, add 0.2g of sodium bicarbonate to neutralize and wash with water until neutral. Then heat to 100°C and distill under reduced pressure to remove water and ethanol. Then cool to room temperature and add 1.4g of hexamethyldisiloxane and 0.0175g of tetramethylammonium hydroxide. After reacting at 80°C for 1 hour, the medium is broken and low-molecular substances are removed by distillation under reduced pressure to obtain a modified tackifier 3. The dynamic viscosity value at 25°C is 10mPa·s.
[0072] In a planetary mixer, add 100g of α, ω-dihydroxypolydimethylsiloxane (dynamic viscosity at 25°C is 10000mPa.s), add 12g of hydrophobic fumed silica (manufacturer: Cabot, model: TS622), add 10g of alkoxy silicone resin (manufacturer: Longsheng Sihai, model: SH-3021, weight-average molecular weight: 6500, mass percentage of alkoxy: 4%), heat to 100°C, vacuum-mix and mix for 1h, then cool to room temperature, first add 10g of methyl tributylidene oxime silane, vacuum-mix and mix for 30min, then add 3g of modified tackifier 3 and 0.3g of dibutyltin dilaurate, vacuum-mix and mix for 30min, finally put into a sealed tube and seal and store to obtain a silicone sealant.
[0073] Example 4
[0074] Weigh 200g of ethanol, 60g of γ-(methacryloyloxy)propyltrimethoxysilane, 110g of N-methyl-3-aminopropyltrimethoxysilane, 30g of N-cyclohexyl-γ-aminopropylmethyldimethoxysilane and 0.1g of hydrochloric acid with a mass fraction of about 37% and add them to a flask. Heat to 50°C and add water dropwise while stirring to react. The amount of water added is 60g. After the addition is complete, heat to 70°C and continue to react for 2 hours. Cool to room temperature and add 2g of sodium bicarbonate to neutralize and wash with water until neutral. Then heat to 100°C and distill under reduced pressure to remove water and alcohol. Then cool to room temperature and add 0.7g of hexamethyldisiloxane and 0.01g of tetramethylammonium hydroxide. After reacting at 90°C for 1 hour, break the medium and remove low molecular weight substances by distillation under reduced pressure to obtain modified tackifier 4. The dynamic viscosity value at 25°C is 30mPa·s.
[0075] In a planetary mixer, add 100g of α, ω-dihydroxypolydimethylsiloxane (dynamic viscosity at 25°C is 20000mPa.s), add 15g of hydrophobic fumed silica (manufacturer: Cabot, model: TS530), add 5g of alkoxy silicone resin (manufacturer: Longsheng Sihai, model: SH-3021, weight average molecular weight: 5000, mass percentage of alkoxy: 6%), heat to 100°C, vacuum-mix and mix for 1h, then cool to room temperature, first add 8g of methyl tributylidene oxime silane, vacuum-mix and mix for 30min, then add 1.5g of modified tackifier 4 and 0.3g of dibutyltin dilaurate, vacuum-mix and mix for 30min, finally put into a sealed tube and seal for storage to obtain a silicone sealant.
[0076] Example 5
[0077] Weigh 220g of ethanol, 60g of γ-(methacryloyloxy)propyltrimethoxysilane, 40g of 3-glycidoxypropylmethyldiethoxysilane, 60g of N-phenyl-3-aminopropyltrimethoxysilane, 10g of N-cyclohexyl-γ-aminopropylmethyldimethoxysilane, 50g of bis(3-trimethoxysilylpropyl)amine and 0.11g of hydrochloric acid with a mass fraction of about 37% and add them to a flask. Heat to 50°C and stir while adding water dropwise to react. , the amount of water added was 66 g, and after the addition was completed, the mixture was heated to 70°C and the reaction was continued for 2 hours. The mixture was cooled to room temperature, 2 g of sodium bicarbonate was added for neutralization, and the mixture was washed with water until neutral. The mixture was then heated to 100°C and distilled under reduced pressure to remove water and alcohol. The mixture was then cooled to room temperature and 0.7 g of hexamethyldisiloxane and 0.01 g of tetramethylammonium hydroxide were added. The mixture was reacted at 90°C for 1 hour, and the medium was broken, and low molecular weight substances were removed by distillation under reduced pressure to obtain a modified tackifier 5. The dynamic viscosity value at 25°C was 20 mPa·s.
[0078] In a planetary mixer, add 100g of α, ω-dihydroxypolydimethylsiloxane (dynamic viscosity at 25°C is 20000mPa.s), add 15g of hydrophobic fumed silica (manufacturer: Cabot, model: TS530), add 5g of alkoxy silicone resin (manufacturer: Longsheng Sihai, model: SH-3021, weight average molecular weight: 5000, mass percentage of alkoxy: 6%), heat to 100°C, vacuum-mix and mix for 1h, then cool to room temperature, first add 8g of methyl tributylidene oxime silane, vacuum-mix and mix for 30min, then add 1.5g of modified tackifier 5 and 0.3g of dibutyltin dilaurate, vacuum-mix and mix for 30min, finally put into a sealed tube and seal for storage to obtain a silicone sealant.
[0079] Example 6
[0080] 230 g of ethanol, 70 g of γ-glycidyloxypropyltrimethoxysilane, 160 g of N-phenyl-3-aminopropyltrimethoxysilane and 0.11 g of hydrochloric acid with a mass fraction of approximately 37% were weighed and added to a flask. The temperature was raised to 50° C. and water was added dropwise with stirring to react. The amount of water added was 67 g. After the addition was complete, the mixture was heated to 80° C. and the reaction was continued for 2 hours. The mixture was cooled to room temperature and 2 g of sodium bicarbonate was added for neutralization and washed with water until neutral. The mixture was then heated to 100° C. and distilled under reduced pressure to remove water and alcohol. The mixture was then cooled to room temperature and 0.7 g of hexamethyldisiloxane and 0.011 g of tetramethylammonium hydroxide were added. After reacting at 100° C. for 2 hours, the mixture was broken into pieces and low-molecular substances were removed by distillation under reduced pressure to obtain a modified tackifier 6. The dynamic viscosity value at 25° C. was 60 mPa·s.
[0081] In a planetary mixer, add 100g of α, ω-dihydroxypolydimethylsiloxane (dynamic viscosity at 25°C is 20000mPa.s), add 15g of hydrophobic fumed silica (manufacturer: Cabot, model: TS530), add 5g of alkoxy silicone resin (manufacturer: Longsheng Sihai, model: SH-3021, weight average molecular weight: 5000, mass percentage of alkoxy: 6%), heat to 100°C, vacuum and stir and mix for 1h, then cool to room temperature, first add 8g of phenyltributylanoximesilane, vacuum and stir and mix for 30min, then add 1.5g of modified tackifier 6 and 0.3g of dibutyltin dilaurate, vacuum and stir and mix for 30min, finally put into a sealed tube and store airtight to obtain a silicone sealant.
[0082] Comparative Example 1
[0083] In a planetary mixer, add 100g of α, ω-dihydroxypolydimethylsiloxane (dynamic viscosity at 25°C is 5000mPa.s), add 10g of hydrophobic fumed silica (manufacturer: Evonik Degussa, model: R202), add 15g of alkoxy silicone resin (manufacturer: Longsheng Sihai, model: SH-3021S, weight average molecular weight: 2500, mass percentage of alkoxy: 12%), heat to 100°C, vacuum stir and mix for 1h, then cool to room temperature, first add 12g of methyl tributylanoxime silane, vacuum stir and mix for 30min, then add 1g of γ-glycidyloxypropyltrimethoxysilane, 3g of bis(3-trimethoxysilylpropyl)amine and 0.3g of dibutyltin dilaurate, vacuum stir and mix for 30min, finally put into a sealed tube and seal for storage to obtain a silicone sealant.
[0084] Comparative Example 2
[0085] In a planetary mixer, add 100g of α, ω-dihydroxypolydimethylsiloxane (dynamic viscosity at 25°C is 20000mPa.s), add 15g of hydrophobic fumed silica (manufacturer: Cabot, model: TS530), heat to 100°C, vacuum and stir and mix for 1h, then cool to room temperature, first add 8g of methyl tributylidene oxime silane, vacuum and stir and mix for 30min, then add 1.5g of modified tackifier 4 and 0.3g of dibutyltin dilaurate, vacuum and stir and mix for 30min, finally put into a sealed tube and store in a sealed manner to obtain a silicone sealant.
[0086] Comparative Example 3
[0087] In a planetary mixer, add 100g of α, ω-dihydroxypolydimethylsiloxane (dynamic viscosity at 25°C is 5000mPa.s), add 15g of alkoxy silicone resin (manufacturer: Longsheng Sihai, model SH-3021S, weight average molecular weight is 2500, mass percentage of alkoxy group is 12%), heat to 100°C, vacuum and stir and mix for 1h, then cool to room temperature, first add 12g of methyl tributylanoxime silane, vacuum and stir and mix for 30min, then add 4g of modified tackifier 1 and 0.3g of dibutyltin dilaurate, vacuum and stir and mix for 30min, finally put into a sealed tube and store airtight to obtain a silicone sealant.
[0088] Comparative Example 4
[0089] Weigh 200g of ethanol, 50g of γ-glycidyloxypropyltrimethoxysilane, 150g of aminopropyltriethoxysilane and 0.1g of strong acid cationic resin into a flask, heat to 50°C, stir and add water dropwise to react, the amount of water added is 60g, heat to 70°C after the addition is complete, continue to react for 2 hours, cool to room temperature, add 2g of sodium bicarbonate to neutralize and wash with water until neutral, then heat to 100°C and remove water and alcohol by vacuum distillation, then cool to room temperature and add 1g of hexamethyldisiloxane and 0.01g of tetramethylammonium hydroxide, react at 90°C for 2 hours to break the medium, and finally remove low molecular weight substances by vacuum distillation to obtain a comparative modified tackifier, the dynamic viscosity value at 25°C is 60mPa·s.
[0090] In a planetary mixer, add 100g of α,ω-dihydroxypolydimethylsiloxane (dynamic viscosity at 25°C is 5000mPa.s), add 10g of hydrophobic fumed silica (manufacturer: Evonik Degussa, model: R202), add 15g of alkoxy silicone resin (manufacturer: Longsheng Sihai, model: SH-3021S, weight-average molecular weight: 2500, mass percentage of alkoxy group: 12%), heat to 100°C, vacuum-mix, and mix for 1h, then cool to room temperature, first add 12g of methyl tributylidene oxime silane, vacuum-mix, and mix for 30min, then add 4g of comparative tackifier and 0.3g of dibutyltin dilaurate, vacuum-mix, and mix for 30min, finally put into a sealed tube and seal for storage to obtain a silicone sealant.
[0091] Test Examples
[0092] The performance of the silicone sealants of Examples 1-6 and Comparative Examples 1-4 was tested. The specific testing method is as follows:
[0093] Tensile strength: tested according to GB / T 528-2009
[0094] Elongation at break: Tested according to GB / T 528-2009
[0095] Hardness: Tested according to GB / T531.1-2008
[0096] Shear strength: tested according to GB / T 7124-2008
[0097] Glossiness: Tested according to GB / T 9754
[0098] Preparation method of tensile strength and elongation at break test specimens: Use a polytetrafluoroethylene container with a wedge-shaped groove with a depth of 2mm, a length of 25cm, and a width of 20cm. Evenly pour the prepared room temperature vulcanized silicone rubber into the polytetrafluoroethylene container, and then place it at a temperature of (23±2)℃ and a relative humidity of 55% to cure for 7 days. Take it out and cut it to obtain the test specimens for performance testing.
[0099] Preparation method of hardness test specimens: Use a polytetrafluoroethylene container with a wedge-shaped groove with a depth of 6mm, a length of 5cm, and a width of 5cm. Evenly pour the prepared room temperature vulcanized silicone rubber into the polytetrafluoroethylene container, and then place it at a temperature of (23±2)℃ and a relative humidity of 55% to cure for 7 days. Take it out to obtain a test specimen and then perform a hardness test.
[0100] Preparation method of shear strength test specimens: According to the sample preparation method of GB / T 7124-2008, room temperature vulcanized silicone rubber is coated on the surface of 6 series aluminum alloy test specimens, and then the test specimens are overlapped. The specimen dimensions are 100mm±0.25mm in length, 25mm±0.25mm in width, and 2mm±0.1mm in thickness. The bonding area is 12.5mm*25mm, and the overlap glue thickness is 0.2mm. The overlapped specimens are placed at a temperature of (23±2)℃ and a relative humidity of 55% for curing for 7 days before the shear strength test is carried out.
[0101] Preparation method of gloss test sample: Use a polytetrafluoroethylene container with a wedge-shaped groove with a depth of 2mm, a length of 10cm, and a width of 5cm. Evenly pour the prepared room temperature vulcanized silicone rubber into the polytetrafluoroethylene container, and then place it at a temperature of (23±2)℃ and a relative humidity of 55% to cure for 7 days. Take it out to obtain the test sample, which can be used for gloss testing. The gloss testing instrument is a YG6060° gloss meter.
[0102] Aging performance tests, including the following:
[0103] Test method for moisture and heat resistance: Place the test specimens (including hardness, tensile strength, elongation at break, shear strength, and gloss test specimens) after curing at room temperature for 7 days in a constant temperature and humidity test chamber, and place them at a temperature of 85°C and a humidity of 85% for 168 hours. Take them out and place them at room temperature for 2 hours, then observe the changes in appearance, and conduct hardness, tensile strength, elongation at break, shear strength, and gloss tests respectively.
[0104] Water vapor resistance test method: Place the steamer into the electric heating pot, heat the water until it boils and steam continuously emerges, place the test specimens (including hardness, tensile strength, elongation at break, shear strength, and gloss test specimens) that have been cured at room temperature for 7 days on the steamer, start timing, place the test specimens under water vapor conditions for 24 hours, then take them out and place them at room temperature for 2 hours, then observe the changes in appearance, and conduct hardness, tensile strength, elongation at break, shear strength and gloss tests respectively.
[0105] Boiling resistance test method: Heat water to boiling, immerse the test specimens (including hardness, tensile strength, elongation at break, shear strength, and gloss test specimens) that have been cured at room temperature for 7 days in boiling water, start timing, boil the test specimens for 24 hours, take them out and place them at room temperature for 2 hours, then observe the changes in appearance, and conduct hardness, tensile strength, elongation at break, shear strength, and gloss tests respectively.
[0106] Table 1 shows the performance test data of the deoxime RTV silicone sealant before aging. In Table 1, viscosity is measured in mPa·s, open time is measured in minutes, tensile strength is measured in MPa, elongation at break is measured in percent, and hardness is Shore A hardness.
[0107] Table 1 Performance test data
[0108]
[0109] Table 2 shows the performance test data of deoxime RTV silicone sealant after heat and humidity aging.
[0110] Table 2 Test data of heat and humidity aging resistance
[0111]
[0112] Table 3 shows the performance test data of the deoxime RTV silicone sealant after water vapor aging.
[0113] Table 3 Water vapor aging resistance test data
[0114]
[0115] Table 4 shows the performance test data of deoxime RTV silicone sealant after water boiling aging.
[0116] Table 4 Test data of water boiling aging resistance
[0117]
[0118] From the data in Table 1, Table 2, Table 3 and Table 4, it can be seen that Comparative Example 1 uses a conventional coupling agent as a tackifier, Comparative Example 3 does not add white carbon black, and Comparative Example 4 uses an epoxy coupling agent and a primary amino coupling agent to react to prepare a tackifier. Compared with Example 1, the mechanical properties of the sealant of Comparative Example 1 are significantly reduced after aging, while the mechanical properties of the sealants of Comparative Examples 3 and Comparative Examples 4 are significantly reduced after aging, and the gloss of the colloid itself is also reduced; while Comparative Example 2 does not add silicone resin. Compared with Example 4, the mechanical properties of the sealant of Comparative Example 2 are significantly reduced after aging, and the appearance deteriorates and the gloss is reduced. That is, the present invention effectively improves the heat and humidity resistance, boiling resistance, and water vapor aging resistance of the sealant through the combination of white carbon black, modified tackifier, and alkoxy silicone resin.
[0119] The above is a further detailed description of the present invention in conjunction with specific preferred embodiments, and the specific implementation of the present invention should not be considered to be limited to these descriptions. For those skilled in the art of the present invention, without departing from the concept of the present invention, several simple deductions or substitutions can be made, which should be considered to fall within the scope of protection of the present invention.
Claims
1. A deoxime type RTV silicone sealant comprising the following components: (A) diorganopolysiloxane terminated with hydroxyl or alkoxy groups (B) Oxime silane crosslinking agent (C) Filling (D) Modified Thickener (E) a catalyst and (F) an alkoxy silicone resin; The (D) modified tackifier is prepared by reacting the following monomers: R 1 Si(OR 6 )3 Formula 1 R 1 R 2 Si(OR 7 )2 Formula 2, R 3 Si(OR 8 )3 Formula 3, R 3 R 4 Si(OR 9 )2 formula 4, (OR 10 )3SiR 5 Si(OR 10 )3 formula 5, In Formula 1 and Formula 2, R 1 is a group containing an epoxy group, an ester group or an acryloxy group. In Formula 3 and Formula 4, R 3 is a group containing -NH-, and R in Formula 5 5 is a divalent group containing -NH-, in Formula 2 and Formula 4, R 2 , R 4 represents the same or different monovalent hydrocarbon groups, and R in Formula 1 to Formula 5 6 , R 7 , R 8 , R 9 , R 10 represents the same or different alkyl groups.
2. The deoxime RTV silicone sealant according to claim 1, characterized in that: The molar amounts of the monomers shown in Formula 1, the monomers shown in Formula 2, the monomers shown in Formula 3, the monomers shown in Formula 4, and the monomers shown in Formula 5 are a, b, c, d, and e, respectively, where a>0, b≥0, c≥0, d≥0, e≥0, c+d+e≠0, (a+b):(c+d+e)=1:(1~3).
3. The deoxime RTV silicone sealant according to claim 2, characterized in that: 0≤b / a<0.
6.
4. The deoxime RTV silicone sealant according to claim 2, characterized in that: 0≤d / (c+d+e)<0.
25.
5. The deoxime RTV silicone sealant according to claim 1, characterized in that: In Formula 1 and Formula 2, R 1 for R 0 represents a C1-C5 alkyl group, and m, n and r are all integers greater than zero and less than or equal to 3.
6. The deoxime RTV silicone sealant according to claim 2, characterized in that: In Formula 3 and Formula 4, the R 3 The structural formula is x represents an integer greater than zero and less than or equal to 3, R 11 It represents a monovalent hydrocarbon group.
7. The deoxime RTV silicone sealant according to claim 2, characterized in that: In Formula 5, the R 5 The structural formula is s and y represent integers greater than zero and less than or equal to 3.
8. The deoxime RTV silicone sealant according to any one of claims 1 to 7, characterized in that: The filler (C) includes fumed silica or precipitated white carbon black, and the amount of the fumed silica or precipitated white carbon black is 10-15 parts by weight for every 100 parts by weight of component (A).
9. The deoxime RTV silicone sealant according to any one of claims 1 to 7, characterized in that: For every 100 parts by weight of the component (A), the (F) alkoxy silicone resin is 5 to 15 parts by weight.
10. The method for preparing a deoxime RTV organosilicon sealant according to any one of claims 1 to 7, wherein the components (A), (B), (C), (D), (E) and (F) are mixed under vacuum conditions and then sealed and packaged to obtain the deoxime RTV organosilicon sealant.