A method for preparing black glazed ceramic tile using slag and glaze used therein
By using apatite-containing phosphorus-containing fuses and slag with high iron oxide to make phase-separated black glaze, the existing black glaze process is solved, and the low-temperature fast firing and environmentally friendly ceramic tiles are achieved Production ensures the pure color and stable performance of the glaze surface.
Patent Information
- Application Number
- CN202310313388.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-03-28
AI Technical Summary
The existing black glaze process is high, complex, and energy consumption, making it difficult to achieve fast firing at low temperatures, which limits the application of ceramic tiles and has a high environmental pollution.
Phase-separated black glaze is made of apatite-containing fused phosphorus and high iron oxide slag. Through specific glaze formulas and process flow, production costs are reduced, low-temperature fast firing is achieved, and ball grinding fineness and raw material groups are used. Optimize the points to avoid pinholes and other defects on the glaze surface.
It has achieved low temperature and rapid firing of black glazed ceramic tiles, reducing production costs, the glaze has a pure color and stable performance, meeting the needs of energy conservation and emission reduction, and avoiding environmental pollution.
Smart Images

Figure BDA0004149324660000041 
Figure BDA0004149324660000071 
Figure BDA0004149324660000081
Abstract
Description
Technical Field
[0001] The invention belongs to the field of building ceramic tiles, and in particular relates to a preparation method of black glazed ceramic tiles using slag and the glaze used. Background Art
[0002] With the development of modern ceramic industry, metal oxides such as Co2O3, Fe2O3, Cr2O3, and Mn2O3 are often used in production to prepare colorants first, and then added to the base glaze to make black glaze. Although this method of glaze firing is not affected by the atmosphere, it needs to be used in a zinc-free lime glaze, and the colorant is affected by the price of raw materials such as Co2O3, and the cost is very high. In recent years, some scholars have made Co-free Fe-Cr-Mn-Ni system black materials and Fe-Cr-Cu-Ni system black materials, but this kind of black glaze is still a kind of mixed spinel colorant with a child crystal and a high content of coloring oxides such as Fe2O3 and Mn2O3. It is necessary to pre-synthesize the colorant through calcination, washing and other processes. The process is relatively complex and energy-intensive, with high pollution and relatively high cost.
[0003] Glaze refers to a layer of glassy material covering the surface of a ceramic body. At a certain temperature, the glaze melts to form a uniform liquid phase. In this silicate melt, due to the differences in cation radius and ion field strength, the forces acting on anions are also different, so there will be a state of coexistence of multiple liquid phases, which is manifested as isolated spherical droplets dispersed in a continuous liquid phase, which is what we often call liquid-liquid phase separation. It is precisely because of the phase separation effect that the glaze of artistic ceramics shows a colorful and ever-changing peculiar effect. Liquid phase separation structures are common in the glazes of many ancient famous Chinese porcelains. Ancient Chinese ceramics were generally fired in semi-downdraft mantou kilns and dragon kilns, and coal or wood was used as fuel. The firing cycle was long, the cooling rate was slow, and a reducing atmosphere was often used, all of which provided good kinetic conditions for the phase separation of the glaze.
[0004] In recent years, some scholars have also conducted research on the phase separation glaze system and firing system. They are all based on the firing system of porcelain. The cooling stage requires a certain amount of insulation time and the entire firing cycle is long, which limits its application in wall and floor tiles.
[0005] How to use iron ore slag to replace ferric oxide raw materials for glaze, reduce production costs, and adopt reasonable processes to ensure the purity of glaze color and stable performance while achieving low-temperature fast firing, meeting the firing conditions of ceramic tiles, and complying with the current needs of the international community for energy conservation and emission reduction, still urgently needs technical improvements. Summary of the invention
[0006] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for preparing black glazed tiles using slag and the glaze used therein, and to produce phase-separated black glaze using phosphorus-containing frits melted from apatite and slag-based low-temperature materials with high iron oxide content, thereby reducing production costs and realizing a low-temperature, fast-firing glaze firing process.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is:
[0008] A glaze used for black glazed tiles using slag, characterized in that it includes a surface glaze and a polishing glaze, the surface glaze contains the following components, calculated by weight: 10-15 parts of phosphorus frit, 25-30 parts of slag, 8-12 parts of Jingyuan mud, 30-35 parts of potassium feldspar, 12-15 parts of quartz, and 3-5 parts of burned talc; the polishing glaze contains the following components, calculated by weight: 30-38 parts of phosphorus frit, 20-25 parts of slag, 17-25 parts of sodium feldspar, 5-8 parts of zinc oxide, 4-6 parts of yttrium oxide, 6-8 parts of Jingyuan mud, and 8-10 parts of quartz.
[0009] Preferably, the surface glaze contains the following components, calculated by weight: 15 parts of phosphorus frit, 27 parts of slag, 10 parts of Jingyuan mud, 30 parts of potassium feldspar, 15 parts of quartz, and 3 parts of burned talc; the polishing glaze contains the following components, calculated by weight: 35 parts of phosphorus frit, 20 parts of slag, 20 parts of sodium feldspar, 8 parts of zinc oxide, 6 parts of yttrium oxide, 8 parts of Jingyuan mud, and 9 parts of quartz.
[0010] Furthermore, the raw material composition of the phosphorus frit is calculated by weight: 50-58 parts of apatite, 8-12 parts of talc, 5-8 parts of potassium carbonate, 9-11 parts of sodium carbonate, 5-18 parts of washed soil, and 9-15 parts of quartz.
[0011] Furthermore, the preparation process of the phosphorus frit is: weigh the above raw materials apatite, talc, potassium carbonate, sodium carbonate, water-washed soil, and quartz according to weight proportions, then mix them evenly, melt them at a high temperature of 1400° C., keep them warm for 30 minutes, then quench them with water to obtain a glass block, and finally crush them into particles below 20 mesh for standby use.
[0012] Furthermore, the slag treatment process is: finely grinding the slag into 320-mesh slag slurry, passing through a 120-mesh sieve, and storing in a slurry pool for standby use.
[0013] Furthermore, the preparation method of the surface glaze and the polishing glaze is: the surface glaze components of phosphorus frit, slag, Jingyuan mud, potassium feldspar, quartz, and burned talc are mixed according to weight, or the polishing glaze components of phosphorus frit, slag, sodium feldspar, zinc oxide, yttrium oxide, Jingyuan mud, and quartz are mixed according to weight, and then 50% of water, 0.1% of sodium carboxymethyl cellulose, and 0.3-0.5% of sodium tripolyphosphate are added, and the glaze slurry is obtained by ball milling for standby use, and the ball milling fineness is 0.6-1.0% of the residue on a 320-mesh sieve, and the specific gravity is 1.88-1.92g / cm 3 .
[0014] A method for preparing black glazed ceramic tiles using slag, characterized in that it includes the following preparation process: applying top glaze and polishing glaze in sequence on the dried ceramic tile blanks, and then sending them into a kiln for firing at 1160-1200°C for 50 minutes to obtain black glazed ceramic tiles, and finally polishing, grinding edges, sorting, and packaging them into finished products for storage.
[0015] Furthermore, the surface glaze pouring parameters are: specific gravity 1.86±0.02g / cm 3 , flow rate 26-28s, glaze application amount 470±5g / m 2 .
[0016] Furthermore, the glaze polishing parameters are: specific gravity 1.86±0.02g / cm 3 , flow rate 26-28s, glaze application amount 660±5g / m 2 .
[0017] The beneficial effects of the present invention are as follows: (1) The surface glaze used for the black polished glaze ceramic tile prepared by the present invention uses slag as a colorant, the iron oxide content in the slag is as high as 50%, and coloring oxides such as titanium oxide, manganese oxide, and chromium oxide are also introduced. After high-temperature firing, it appears black and plays a role in isolating the phase-separated glaze and the body, thereby avoiding discoloration and defects such as pinholes and glaze bubbles caused by the reaction between the polished glaze and the body;
[0018] (2) The glaze used in the present invention is Na2O(K2O)-CaO-MgO-SiO2-Al2O3-Fe2O3-P2O 5-Y2O3 system phase-separated glaze, during the firing process of the phase-separated glaze, the glaze melt produces a liquid-liquid immiscible microphase, and iron oxide exists in the microphase rather than the entire glass phase. Therefore, the iron ion concentration in the microphase can be increased, and at the same time, the microphase has a wrapping effect on the coloring particles to improve the color stability, so that a small amount of colored oxide can produce a greater coloring ability. The microphase with a higher degree of coloring acts on the entire glaze layer due to the transmission and refraction of light, just like a layer of black film on the glass and the entire glass appears black; the zinc oxide contained in the polishing glaze is relatively good for the coloring of other iron-containing pigments, but in the black series, it is not conducive to the coloring of black. Therefore, yttrium oxide is also added to the polishing glaze to enhance the brightness of the polishing glaze color, especially for the purer black color, which is helpful for the high Research and development of warm-fired products; yttrium oxide can effectively reduce the crystal grain size during firing. Yttrium oxide, as the second phase, has an inhibitory effect on the growth of grains. If the glaze crystal fineness is too fine, it is easy to hinder the degassing of the body, resulting in large-area pinholes on the glaze surface during the sintering process. It is better to add slag and Jingyuan mud to the glaze. The slag contains more than 50% iron oxide, and the Jingyuan mud also contains a large amount of iron oxide. During the melting and firing, the iron oxide component is greatly saturated, and the crystallization is not affected by the yttrium oxide phase. In addition, the ball mill fineness in the preparation of the glaze is 320 mesh, which is neither too fine nor too coarse. The fineness is controlled within an appropriate range, and combined with the raw material components used, the problem of pinholes on the glaze surface during sintering caused by the reduction of the grain size is solved;
[0019] (3) The present invention uses P as a promoter to control the Si / P molar ratio by adjusting the formula, and the phosphosilicate glass melt with high sodium, low magnesium and low aluminum has low viscosity, so that the saturated ferric oxide in the melt quickly forms tiny iron-rich droplets during the cooling process, thereby achieving a phase-separated black glaze effect;
[0020] (4) Apatite, a natural mineral, contains substances that affect the performance of glaze slurry. When it is directly used in glaze firing, it is easy to produce glaze bubbles and pinholes. Therefore, low-temperature phosphorus-containing frit is made to provide phosphorus components for phase-separated glaze, and industrial calcium phosphate is not used, which reduces costs. The iron oxide required for phase-separated glaze is provided by slag. The slag used is an intermediate product of steel smelting, containing up to 50% iron oxide. The firing temperature is low, which is conducive to reducing the firing temperature of the glaze. The use of slag avoids the direct use of industrial iron oxide. The slurry properties of different batches of industrial iron oxide are different, resulting in unstable glaze slurry properties. , which seriously causes the glaze slurry to be thixotropic and unusable. At the same time, ferric oxide has a strong dyeing effect, which seriously pollutes the use environment. However, the slag used in the present invention contains a large amount of iron oxide, and at the same time, it brings in coloring elements such as titanium, manganese, vanadium, and chromium, so that the black glaze color is pure and stable; the silicon, aluminum, calcium, iron, and phosphorus in the slag and apatite are used to replace part of the quartz, limestone, aluminum oxide, calcium phosphate, etc. in the glaze materials, which also saves mineral resources and avoids environmental pollution; the use of local Jingyuan mud provides the necessary slurry properties for the glaze, provides iron oxide components, and reduces material costs;
[0021] (5) The glaze prepared by the present invention has high blackness, pure color and stable performance. The prepared black glazed ceramic tiles have a firing temperature of 1160-1200°C and a firing cycle of 50 minutes, which meets the needs of low-temperature and fast firing of wall and floor tiles and complies with the current international community's policy of energy conservation and emission reduction. DETAILED DESCRIPTION
[0022] In order to better understand the present invention, the embodiments of the present invention are described in detail below in conjunction with examples. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention.
[0023] The Jingyuan mud mine in the following examples is located 50 kilometers away from Yueyang County, in Sanjiang Town, Miluo City. It is a clay soil with a small sand content. Its appearance is light yellow. After removing the surface red soil and vegetation, it contains little organic impurities and can be directly mined and used as a raw material for green bodies. When used as a raw material for glaze, it is first stirred in a slurry pool to a specific gravity of 1.45g / cm 3 The mud is passed through a 100-mesh vibrating screen to remove branches and large particles of sand and gravel, and is squeezed into mud cakes and dried for later use.
[0024] The reference chemical compositions of slag, apatite and Jingyuan mud used in this embodiment are shown in Table 1.
[0025] Table 1
[0026]
[0027] Embodiment 1:
[0028] A glaze used for black polished glaze tiles using slag, including a surface glaze and a polished glaze, wherein the surface glaze comprises the following components, by weight: 15 parts of phosphorus frit, 27 parts of slag, 10 parts of Jingyuan mud, 30 parts of potassium feldspar, 15 parts of quartz, and 3 parts of burned talc; the polished glaze comprises the following components, by weight: 35 parts of phosphorus frit, 20 parts of slag, 20 parts of sodium feldspar, 8 parts of zinc oxide, 6 parts of yttrium oxide, 8 parts of Jingyuan mud, and 9 parts of quartz; the raw material composition of the phosphorus frit is by weight: 55 parts of apatite, 8 parts of talc, 5 parts of potassium carbonate, 10 parts of sodium carbonate, 7 parts of washed soil, and 15 parts of quartz; the preparation process of phosphorus frit is: weigh the above raw materials apatite, talc, potassium carbonate, sodium carbonate, washed soil, and quartz according to weight parts, then mix them evenly, melt them at a high temperature of 1400°C, keep them warm for 30 minutes, then quench them with water to obtain glass blocks, and finally break them into particles below 20 mesh for standby use; the processing process of the slag is: finely grind the slag into 320 mesh slag slurry, pass it through a 120 mesh sieve, and store it in a slurry pool for standby use.
[0029] The preparation method of the surface glaze and the polishing glaze is as follows: the surface glaze components of phosphorus frit, slag, Jingyuan mud, potassium feldspar, quartz, and calcined talc are mixed according to weight, or the polishing glaze components of phosphorus frit, slag, sodium feldspar, zinc oxide, yttrium oxide, Jingyuan mud, and quartz are mixed according to weight, and then 50% of water, 0.1% of sodium carboxymethyl cellulose, and 0.3% of sodium tripolyphosphate are added, and the glaze slurry is obtained by ball milling for standby use, wherein the ball milling fineness is 0.6% of the residue on a 320-mesh sieve, and the specific gravity is 1.92 g / cm 3 .
[0030] A method for preparing black glazed ceramic tiles using slag, characterized in that it includes the following preparation process: applying top glaze and polishing glaze on the dried ceramic tile blank in sequence, and then sending it into a kiln for firing at 1180°C for 50 minutes to obtain black glazed ceramic tiles, and finally polishing, grinding edges, sorting, and packaging into finished products for storage; the top glaze glazing parameters: specific gravity 1.86g / cm 3 , flow rate 26s, glaze application amount 470g / m 2 ; Further, the glaze polishing parameters: specific gravity 1.86g / cm 3 , flow rate 26s, glaze amount 660g / m 2 .
[0031] Embodiment 2:
[0032] A glaze used for black polished glaze tiles using slag, including a surface glaze and a polished glaze, wherein the surface glaze comprises the following components, by weight: 10 parts of phosphorus frit, 25 parts of slag, 12 parts of Jingyuan mud, 35 parts of potassium feldspar, 14 parts of quartz, and 4 parts of burned talc; the polished glaze comprises the following components, by weight: 38 parts of phosphorus frit, 23 parts of slag, 17 parts of sodium feldspar, 6 parts of zinc oxide, 4 parts of yttrium oxide, 6 parts of Jingyuan mud, and 10 parts of quartz; the raw material composition of the phosphorus frit is by weight: 50 parts of apatite, 12 parts of talc, 8 parts of potassium carbonate, 9 parts of sodium carbonate, 18 parts of washed soil, and 13 parts of quartz; the preparation process of phosphorus frit is: weigh the above raw materials apatite, talc, potassium carbonate, sodium carbonate, washed soil, and quartz according to weight parts, then mix them evenly, melt them at a high temperature of 1400°C, keep them warm for 30 minutes, then quench them with water to obtain glass blocks, and finally break them into particles below 20 mesh for standby use; the processing process of the slag is: finely grind the slag into 320 mesh slag slurry, pass it through a 120 mesh sieve, and store it in a slurry pool for standby use.
[0033] The preparation method of the surface glaze and the polishing glaze is as follows: the surface glaze components of phosphorus frit, slag, Jingyuan mud, potassium feldspar, quartz, and calcined talc are mixed according to weight, or the polishing glaze components of phosphorus frit, slag, sodium feldspar, zinc oxide, yttrium oxide, Jingyuan mud, and quartz are mixed according to weight, and then 50% of water, 0.1% of sodium carboxymethyl cellulose, and 0.5% of sodium tripolyphosphate are added, and the glaze slurry is obtained by ball milling for standby use, wherein the ball milling fineness is 1.0% of the residue on a 320-mesh sieve, and the specific gravity is 1.88 g / cm 3 .
[0034] A method for preparing black glazed ceramic tiles using slag, characterized in that it includes the following preparation process: applying top glaze and polishing glaze on the dried ceramic tile blank in sequence, and then sending it into a kiln for firing at 1200°C for 50 minutes to obtain black glazed ceramic tiles, and finally polishing, edge grinding, sorting, and packaging into finished products for storage; the top glaze glazing parameters: specific gravity 1.88g / cm 3 , flow rate 28s, glaze application amount 475g / m 2 ; Further, the glaze polishing parameters: specific gravity 1.88g / cm 3 , flow rate 28s, glaze application amount 665g / m 2 .
[0035] Embodiment 3:
[0036] A glaze used for black polished glaze tiles using slag, including a surface glaze and a polished glaze, wherein the surface glaze comprises the following components, by weight: 12 parts of phosphorus frit, 30 parts of slag, 8 parts of Jingyuan mud, 33 parts of potassium feldspar, 12 parts of quartz, and 5 parts of burned talc; the polished glaze comprises the following components, by weight: 30 parts of phosphorus frit, 25 parts of slag, 25 parts of sodium feldspar, 5 parts of zinc oxide, 5 parts of yttrium oxide, 7 parts of Jingyuan mud, and 8 parts of quartz; the raw material composition of the phosphorus frit is by weight: 58 parts of apatite, 10 parts of talc, 7 parts of potassium carbonate, 11 parts of sodium carbonate, 5 parts of washed soil, and 9 parts of quartz; the preparation process of phosphorus frit is: weigh the above raw materials apatite, talc, potassium carbonate, sodium carbonate, washed soil, and quartz according to weight parts, then mix them evenly, melt them at a high temperature of 1400°C, keep them warm for 30 minutes, then quench them with water to obtain glass blocks, and finally break them into particles below 20 mesh for standby use; the processing process of the slag is: finely grind the slag into 320 mesh slag slurry, pass it through a 120 mesh sieve, and store it in a slurry pool for standby use.
[0037] The preparation method of the surface glaze and the polishing glaze is as follows: the surface glaze components of phosphorus frit, slag, Jingyuan mud, potassium feldspar, quartz, and calcined talc are mixed according to weight, or the polishing glaze components of phosphorus frit, slag, sodium feldspar, zinc oxide, yttrium oxide, Jingyuan mud, and quartz are mixed according to weight, and then 50% of water, 0.1% of sodium carboxymethyl cellulose, and 0.4% of sodium tripolyphosphate are added, and the glaze slurry is obtained by ball milling for standby use, wherein the ball milling fineness is 0.8% of the residue on a 320-mesh sieve, and the specific gravity is 1.90 g / cm 3 .
[0038] A method for preparing black glazed ceramic tiles using slag, characterized in that it includes the following preparation process: applying top glaze and polishing glaze on the dried ceramic tile blank in sequence, and then sending it into a kiln for firing at 1160°C for 50 minutes to obtain black glazed ceramic tiles, and finally polishing, grinding edges, sorting, and packaging into finished products for storage; the top glaze glazing parameters: specific gravity 1.84g / cm 3 , flow rate 27s, glaze application amount 465g / m 2 ; Further, the glaze polishing parameters: specific gravity 1.84g / cm 3 , flow rate 27s, glaze amount 655g / m 2 .
[0039] Comparative Example 1:
[0040] The difference between Comparative Example 1 and Example 1 is that the glaze raw material does not contain yttrium oxide component, and other technical contents are the same as those of Example 1.
[0041] Comparative Example 2:
[0042] The difference between Comparative Example 2 and Example 1 is that the glaze polishing raw materials do not contain Jingyuan mud, and the other technical contents are the same as those of Example 1.
[0043] Comparative Example 3:
[0044] The difference between Comparative Example 3 and Example 1 is that in the glaze preparation step, the glaze slurry ball grinding fineness is set to 400 mesh sieve, and the other contents are the same as Example 1.
[0045] Comparative Example 4:
[0046] The difference between Comparative Example 4 and Example 1 is that in the glaze preparation step, the glaze slurry ball grinding fineness is set to 300 mesh sieve, and the other contents are the same as Example 1.
[0047] Comparative Example 5:
[0048] The difference between Comparative Example 5 and Example 1 is that its glaze polishing raw materials do not contain Jingyuan mud and yttrium oxide components, and the other contents are the same as Example 1.
[0049] The black glazed tiles prepared in each embodiment and comparative example were tested, and the results are shown in the following table.
[0050] Table 1 Glaze color difference test results
[0051] L a b Example 1 35.95 1.63 -1.38 Example 2 34.15 2.32 -2.19 Example 3 37.23 3.16 -1.34 Comparative Example 1 28.37 4.97 -5.65 Comparative Example 2 34.68 2.14 -3.21 Comparative Example 3 36.17 1.52 -1.16 Comparative Example 4 35.58 1.73 -1.36 Comparative Example 5 32.74 3.96 -3.48
[0052] Table 2 Glaze appearance observation results
[0053]
[0054]
[0055] The above description of the embodiments is to facilitate the understanding and use of the present invention by those skilled in the art. Those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments. Improvements and modifications made by those skilled in the art based on the principles of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A glaze for black glazed tiles using slag, characterized in that: The invention comprises a top glaze and a polishing glaze, wherein the top glaze comprises the following components, calculated by weight: 10-15 parts of phosphorus frit, 25-30 parts of slag, 8-12 parts of Jingyuan mud, 30-35 parts of potassium feldspar, 12-15 parts of quartz, and 3-5 parts of burned talc; the polishing glaze comprises the following components, calculated by weight: 30-38 parts of phosphorus frit, 20-25 parts of slag, 17-25 parts of sodium feldspar, 5-8 parts of zinc oxide, 4-6 parts of yttrium oxide, 6-8 parts of Jingyuan mud, and 8-10 parts of quartz; the Jingyuan mud comprises the following chemical components, calculated by weight percentage: SiO2 58.28%, Al2O3 22.35%, Fe2O3 7.24%, TiO2 0.75%, CaO 0.3%, MgO 1.22%, K2O 2.55%, Na2O The raw material composition of the phosphorus frit is calculated by weight as follows: 50-58 parts of apatite, 8-12 parts of talc, 5-8 parts of potassium carbonate, 9-11 parts of sodium carbonate, 5-18 parts of washed soil, and 9-15 parts of quartz.
2. The glaze used for black glazed tiles using slag according to claim 1, characterized in that: The surface glaze contains the following components, calculated by weight: 15 parts of phosphorus frit, 27 parts of slag, 10 parts of Jingyuan mud, 30 parts of potassium feldspar, 15 parts of quartz, and 3 parts of burned talc; the polishing glaze contains the following components, calculated by weight: 35 parts of phosphorus frit, 20 parts of slag, 20 parts of sodium feldspar, 8 parts of zinc oxide, 6 parts of yttrium oxide, 8 parts of Jingyuan mud, and 9 parts of quartz.
3. The glaze used for black glazed tiles using slag according to claim 1, characterized in that: The phosphorus frit is prepared by weighing the raw materials of apatite, talc, potassium carbonate, sodium carbonate, water-washed soil and quartz according to parts by weight, mixing them uniformly, melting them at a high temperature of 1400°C, keeping the temperature for 30 minutes, quenching them with water to obtain a glass block, and finally crushing them into particles below 20 mesh for later use.
4. The glaze used for black glazed tiles using slag according to claim 1, characterized in that: The slag treatment process is as follows: finely grinding the slag into 320-mesh slag slurry, passing through a 120-mesh sieve, and storing in a slurry pool for standby use.
5. The glaze used for black glazed tiles using slag according to claim 1, characterized in that: The preparation method of the surface glaze and the polishing glaze is as follows: the surface glaze components of phosphorus frit, slag, Jingyuan mud, potassium feldspar, quartz, and burned talc are mixed according to weight parts, or the polishing glaze components of phosphorus frit, slag, sodium feldspar, zinc oxide, yttrium oxide, Jingyuan mud, and quartz are mixed according to weight parts, and then 50% of water, 0.1% of sodium carboxymethyl cellulose, and 0.3-0.5% of sodium tripolyphosphate are added, and the glaze slurry is obtained by ball milling for use, wherein the ball milling fineness is 0.6-1.0% of the residue on a 320-mesh sieve, and the specific gravity is 1.88-1.92 g / cm 3 .
6. A method for preparing black glazed tiles using slag, characterized in that: The method comprises the following preparation process: sequentially pouring the surface glaze and polishing glaze as described in any one of claims 1 to 5 on the dried ceramic tile blank, and then sending the blank into a kiln for firing at 1160-1200°C for 50 minutes to obtain black glazed ceramic tiles, and finally polishing, grinding edges, sorting, and packaging the finished products for storage.
7. The method for preparing black glazed tiles using slag according to claim 6, characterized in that: The glaze pouring parameters: specific gravity 1.86±0.02g / cm 3 , flow rate 26-28s, glaze amount 470±5g / m 2 .
8. The method for preparing black glazed tiles using slag according to claim 7, characterized in that: Glaze polishing parameters: specific gravity 1.86±0.02g / cm 3 , flow rate 26-28s, glaze amount 660±5g / m 2 .