A ceramic insulator for high voltage capacitor and preparation method thereof
By using a combined structure of alumina blank and glaze layer in the ceramic insulator of high-voltage capacitors, combining silica micro-nanostructure layer and specific components, the problem of insufficient discharge and insulation capacity of ceramic insulators in harsh environments is solved, which is significantly Improves its insulation and anti-fouling properties and extends its service life.
Patent Information
- Application Number
- CN202310761501.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-06-27
AI Technical Summary
Ceramic insulators in high-voltage capacitors are prone to discharge in harsh environments, resulting in local deterioration and deterioration, shortening service life, and insufficient surface insulation capacity.
A combined structure of alumina blank and glaze layer is adopted, where the glaze layer contains alumina, chromium oxide, hexagonal boron nitride, cerium-zirconium solid solution modified Elosite nanotubes, titanium dioxide coated indium oxide and strontium titanate and other components. , and a silica micro-nanostructure layer is provided between the alumina blank and the glaze layer, so that the insulation performance and soil resistance are improved through specific preparation methods.
It significantly improves the surface voltage resistance, insulation performance, thermal stability, chemical stability and mechanical stability of ceramic insulators, reduces the probability of discharge and breakdown, enhances the anti-fouling and anti-fouling performance, and extends the service life.
Abstract
Description
Technical Field
[0001] The invention relates to the field of composite insulator materials, in particular to a ceramic insulator for a high-voltage capacitor and a preparation method thereof. Background Art
[0002] Ceramic insulators have long been widely used in high-voltage capacitors for their excellent electromechanical properties, playing the role of insulation, sealing and support. In the actual operation of high-voltage capacitors, due to the influence of the surrounding environment such as heavy rain, high humidity, pollution and other harsh environments, various discharge phenomena may occur in the insulators, causing local deterioration and deterioration of the insulators, shortening their service life. Therefore, improving the surface insulation capacity of ceramic insulators has become one of the issues that are concerned and urgently need to be solved in the capacitor field. Summary of the invention
[0003] Purpose of the invention: In view of the above technical problems, the present invention proposes a ceramic insulator for a high-voltage capacitor and a preparation method thereof.
[0004] The technical solutions adopted are as follows:
[0005] A ceramic insulator for a high voltage capacitor, comprising an alumina body and a glaze layer;
[0006] In parts by weight, the glaze layer comprises:
[0007] 40-60 parts of aluminum oxide, 5-10 parts of chromium oxide, 20-30 parts of hexagonal boron nitride, 0.5-1.5 parts of lithium carbonate, 0.1-1 parts of lanthanum oxide, 4-8 parts of dolomite, 5-10 parts of cerium-zirconium solid solution modified halloysite nanotubes, 10-20 parts of titanium dioxide coated indium oxide, 5-10 parts of strontium titanate, and 3-6 parts of glass powder.
[0008] Furthermore, a bonding layer is provided between the alumina substrate and the glaze layer.
[0009] Furthermore, the bonding layer is a silicon dioxide micro-nano structure layer.
[0010] Furthermore, the preparation method of the cerium-zirconium solid solution modified halloysite nanotubes is as follows:
[0011] Cerium salt and zirconium salt are added into water to prepare solution A, cyclohexane, nonionic surfactant and n-pentanol are mixed to prepare solution B, solution B is divided into two parts, namely solution B-1 and solution B-2, solution A and halloysite nanotubes are added into solution B-1 and stirred to obtain reverse microemulsion A, ammonia water is added into solution B-2 and stirred to obtain reverse microemulsion B, reverse microemulsion B is added dropwise into reverse microemulsion A, after adding, the reaction is stirred for 60-120 minutes, the product is separated, washed, dried and calcined.
[0012] Furthermore, the molar ratio of the cerium salt to the zirconium salt is 1-2.5:1.
[0013] Furthermore, the calcination temperature is 500-600° C., and the calcination time is 2-4 hours.
[0014] Furthermore, the preparation method of the titanium dioxide-coated indium oxide is as follows:
[0015] After indium oxide is immersed in tetrabutyl titanate toluene solution for 10-30 minutes, it is separated, washed with toluene and water in a cycle, and calcined at 550-600°C for 5-10 hours. After naturally cooling to room temperature, it is taken out to obtain a pre-coated body. Tetrabutyl titanate is added to a hydrochloric acid / water solution and stirred evenly, and then the pre-coated body is added. The resulting mixed solution is transferred to a hydrothermal reactor, sealed and heated to 120-150°C for reaction for 6-10 hours. After returning to room temperature, the product is separated, washed and dried.
[0016] Furthermore, the glass powder is CBS glass powder.
[0017] The present invention also provides a method for preparing a ceramic insulator:
[0018] Ethyl orthosilicate and acetylacetone are dissolved in anhydrous acetaldehyde, and the obtained first mixed solution is sprayed on the surface of the alumina blank, and then a second mixed solution consisting of nitric acid, ethanol and water is also sprayed on the surface of the alumina blank. After being kept at 60-70°C for 3-6 hours, the temperature is raised to 500-600°C and pre-fired for 1-3 hours to obtain an alumina blank containing a bonding layer. Alumina, chromium oxide, hexagonal boron nitride, lithium carbonate, lanthanum oxide, dolomite, cerium-zirconium solid solution modified halloysite nanotubes, titanium dioxide coated indium oxide, strontium titanate and glass powder are ball-milled and mixed with water to obtain a glaze slurry, which is applied on the surface of the alumina blank. After drying, a glaze layer with a thickness of 0.1-1 mm is obtained, and the obtained semi-finished product is heated to 1350-1450°C, sintered for 2-4 hours, and then restored to room temperature.
[0019] Furthermore, the heating rate during sintering is 5-10°C / min.
[0020] Beneficial effects of the present invention:
[0021] The present invention provides a ceramic insulator for a high-voltage capacitor. The silicon dioxide micro-nano structure layer is arranged between the aluminum oxide blank and the glaze layer to improve the bonding strength and reduce the stress during sintering. The chromium oxide has an extremely low secondary electron emission coefficient and can effectively improve the surface withstand voltage of the ceramic insulator. The addition of hexagonal boron nitride can improve the insulation performance, thermal stability, chemical stability and mechanical stability of the ceramic insulator. The use of dolomite can introduce MgO and CaCO 3The composition can reduce the firing temperature of the glaze layer, promote the formation of the mullite phase between the silicon dioxide micro-nanostructure layer and the glaze layer, and improve the bonding strength. The cerium-zirconium solid solution modified halloysite nanotubes can improve the discharge and breakdown characteristics of the ceramic insulator. It can inhibit the generation of discharge, reduce surface corona discharge, arc discharge and other phenomena, reduce the probability of insulator breakdown, increase the flashover voltage, and improve the mechanical properties of the ceramic insulator. The valence band and conduction band potentials of titanium dioxide are higher than those of indium oxide, and the band gap width of indium oxide is only 2.8eV. After coating, directional transfer of electrons and holes occurs between titanium dioxide and indium oxide, and the degradation ability of dirt is improved. Strontium titanate, as a typical perovskite-type composite oxide, has the advantages of high carrier mobility and high photocatalytic activity. After being added, it can further improve the degradation ability of the ceramic insulator for dirt, and play a good anti-fouling and self-cleaning effect. The ceramic insulator prepared by the present invention has good insulation and anti-fouling flashover ability, stable performance, and also has relatively excellent anti-fouling performance. DETAILED DESCRIPTION
[0022] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.
[0023] Embodiment 1:
[0024] A ceramic insulator for a high-voltage capacitor, comprising an alumina blank, a silicon dioxide micro-nanostructure layer and a glaze layer;
[0025] In parts by weight, the glaze layer comprises:
[0026] 50 parts of aluminum oxide, 6 parts of chromium oxide, 22 parts of hexagonal boron nitride, 1.2 parts of lithium carbonate, 0.5 parts of lanthanum oxide, 6 parts of dolomite, 8 parts of cerium-zirconium solid solution modified halloysite nanotubes, 15 parts of titanium dioxide coated indium oxide, 5 parts of strontium titanate, and 4 parts of CBS glass powder.
[0027] The preparation method of cerium-zirconium solid solution modified halloysite nanotubes is as follows:
[0028] 130.27 g of cerium nitrate hexahydrate and 85.87 g of zirconium nitrate pentahydrate were added to 500 mL of water to prepare solution A, 472 mL of cyclohexane, 210 mL of Triton X-114 and 102 mL of n-pentanol were mixed to prepare solution B, solution B was evenly divided into two parts, recorded as solution B-1 and solution B-2, solution A and 200 g of halloysite nanotubes were added to solution B-1 and stirred to obtain reverse microemulsion A, 500 mL of 4 mol / L ammonia water was added to solution B-2 and stirred to obtain reverse microemulsion B, reverse microemulsion B was added dropwise to reverse microemulsion A, and the reaction was stirred for 120 min after the dropwise addition was completed. The product was separated by centrifugation, washed with water and ethanol, dried at 80°C for 10 h, and finally placed in a muffle furnace and heated to 600°C for calcination for 3 h.
[0029] The preparation method of titanium dioxide coated indium oxide is as follows:
[0030] 100g of indium oxide was stirred and immersed in 500mL of 1mol / L tetrabutyl titanate toluene solution for 30min, then centrifuged, washed 5 times with toluene and water, placed in a muffle furnace and heated to 600℃ for calcination for 8h, and naturally cooled to room temperature to obtain a pre-coated body. 500mL of 37% hydrochloric acid was mixed with 500mL of water, stirred evenly, 50g of tetrabutyl titanate was added and stirred evenly, and then the above-mentioned pre-coated body was added. The obtained mixed solution was transferred to a hydrothermal reactor, sealed and heated to 135℃ for hydrothermal reaction for 10h, and then centrifuged after returning to room temperature. The obtained product was washed with water and ethanol, and dried at 80℃ for 10h.
[0031] The preparation method of the above ceramic insulator:
[0032] 20g of ethyl orthosilicate and 2.5mL of acetylacetone were dissolved in 400mL of anhydrous acetaldehyde to obtain a first mixed solution, which was sprayed on the surface of the alumina blank, and then a second mixed solution consisting of 1g of nitric acid, 12mL of ethanol and 95mL of water was also sprayed on the surface of the alumina blank. The alumina blank was heated to 65°C and kept for 5h, and then heated to 580°C for pre-calcination for 2h to obtain an alumina blank containing a silicon dioxide micro-nanostructure layer, and then alumina, chromium oxide, hexagonal boron nitride, and lithium carbonate were added. , lanthanum oxide, dolomite, cerium-zirconium solid solution modified halloysite nanotubes, titanium dioxide coated indium oxide, strontium titanate, and CBS glass powder are added to the ball mill of a planetary ball mill and ball milled for 5 hours to obtain a mixture, the mixture is mixed with water in a mass ratio of 1:1.5 to obtain a glaze slurry, the glaze slurry is applied on the surface of the alumina blank by a glaze spraying method, and a glaze layer with a thickness of 0.25 mm is obtained after drying, and the semi-finished product is heated to 1400°C at a rate of 5°C / min, sintered for 2.5 hours, and then returned to room temperature.
[0033] Embodiment 2:
[0034] The method is substantially the same as Example 1, except that, by weight, the glaze layer comprises:
[0035] 60 parts of aluminum oxide, 10 parts of chromium oxide, 30 parts of hexagonal boron nitride, 1.5 parts of lithium carbonate, 1 part of lanthanum oxide, 8 parts of dolomite, 10 parts of cerium-zirconium solid solution modified halloysite nanotubes, 20 parts of titanium dioxide coated indium oxide, 10 parts of strontium titanate, and 6 parts of CBS glass powder.
[0036] Embodiment 3:
[0037] The method is substantially the same as Example 1, except that, by weight, the glaze layer comprises:
[0038] 40 parts of aluminum oxide, 5 parts of chromium oxide, 20 parts of hexagonal boron nitride, 0.5 parts of lithium carbonate, 0.1 parts of lanthanum oxide, 4 parts of dolomite, 5 parts of cerium-zirconium solid solution modified halloysite nanotubes, 10 parts of titanium dioxide coated indium oxide, 5 parts of strontium titanate, and 3 parts of CBS glass powder.
[0039] Comparative Example 1:
[0040] The method is basically the same as Example 1, except that no cerium-zirconium solid solution is added to modify the halloysite nanotubes.
[0041] Comparative Example 2:
[0042] The method is basically the same as Example 1, except that the halloysite nanotubes are modified by using the same mass of halloysite nanotubes instead of the cerium-zirconium solid solution.
[0043] Comparative Example 3:
[0044] The method is basically the same as Example 1, except that the cerium-zirconium solid solution of the same mass is used to replace the cerium-zirconium solid solution to modify the halloysite nanotubes.
[0045] Comparative Example 4:
[0046] The method is basically the same as Example 1, except that titanium dioxide is not added to coat indium oxide.
[0047] Comparative Example 5:
[0048] The method is basically the same as Example 1, except that the same mass of titanium dioxide is used instead of titanium dioxide to coat indium oxide.
[0049] Comparative Example 6:
[0050] It is basically the same as Example 1, except that strontium titanate is not added.
[0051] Performance Test:
[0052] The ceramic insulators prepared in Examples 1-3 of the present invention and Comparative Examples 1-6 were used as samples for performance testing;
[0053] ① This test uses the inclined plane method, and the test voltage uses a constant leakage tracking voltage. GB / T6553-2014 "Test method for assessing resistance to tracking and corrosion of electrical insulating materials used under severe environmental conditions" recommends the use of 2.5kV, 3.5kV or 4.5kV voltage. This test uses 4.5kV.
[0054] The contaminated liquid is introduced into the electrode through a plastic flow tube and is obtained by dissolving 0.1% ammonium chloride and 0.02% polyethoxyisocyanate phenyl ether in distilled water to ensure that the resistivity of the contaminated liquid is 395±5Ω·cm, the flow rate of the contaminated liquid is 0.6mL / min, and the ambient temperature during the test is 23±2℃.
[0055] The test lasts for 100 hours, and the wet flashover voltage test is carried out on the sample. Before testing the wet flashover voltage, the surface of the sample is cleaned and wiped with pure distilled water, and then immersed in pure distilled water for 24 hours before being taken out for testing. Unit: kV;
[0056] Table 1 (wet flashover voltage test results):
[0057] 0h 100h 200h 300h 400h 500h 600h 700h Example 1 66.2 65.9 64.0 62.8 61.3 59.2 58.8 56.1 Example 2 64.6 63.3 62.1 61.5 60.1 58.6 56.9 56.0 Example 3 60.5 59.2 58.5 56.4 55.0 54.7 53.3 50.4 Comparative Example 1 43.0 40.8 39.6 38.1 36.2 30.0 25.2 24.6 Comparative Example 2 50.4 48.3 47.5 40.3 39.6 37.0 35.2 34.4 Comparative Example 3 52.6 50.1 47.3 44.8 41.9 39.0 35.2 30.3 Comparative Example 4 47.0 46.4 40.9 38.5 37.2 36.0 34.1 28.9 Comparative Example 5 45.0 41.2 39.5 35.0 34.2 30.7 29.8 27.5 Comparative Example 6 60.3 59.0 57.6 56.8 54.9 53.0 52.2 51.7
[0058] ② Artificial simulated pollution: The artificial pollution test system of the State Grid UHV AC test base was used for experiments, specifically using 50μm TBP / OK simulated pollution, with a rain rate of 1.0mm / min and raining for 10min; artificial spraying for 15min, drying for 60min, and running under light environment for 10d, and artificially observing the pollution on the surface of the sample.
[0059] Table 2 (results of artificial simulated dirt accumulation test):
[0060] Artificial simulation of pollution accumulation Example 1 There is a little dirt on the surface Example 2 There is a little dirt on the surface Example 3 There is a little dirt on the surface Comparative Example 1 N / A Comparative Example 2 N / A Comparative Example 3 N / A Comparative Example 4 The surface is seriously dirty Comparative Example 5 Surface dirtiness Comparative Example 6 Surface dirtiness
[0061] It can be seen from Table 1 and Table 2 above that the ceramic insulator prepared by the present invention has good insulation and anti-pollution flashover capabilities, stable performance, and also has relatively excellent anti-pollution performance.
[0062] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A ceramic insulator for a high voltage capacitor, It is characterized in that It includes an aluminum oxide body and a glaze layer; In parts by weight, the glaze layer comprises: 40-60 parts of aluminum oxide, 5-10 parts of chromium oxide, 20-30 parts of hexagonal boron nitride, 0.5-1.5 parts of lithium carbonate, 0.1-1 parts of lanthanum oxide, 4-8 parts of dolomite, 5-10 parts of cerium-zirconium solid solution modified halloysite nanotubes, 10-20 parts of titanium dioxide coated indium oxide, 5-10 parts of strontium titanate, and 3-6 parts of glass powder; The preparation method of the cerium-zirconium solid solution modified halloysite nanotubes is as follows: Cerium salt and zirconium salt are added into water to prepare solution A, cyclohexane, nonionic surfactant and n-pentanol are mixed to prepare solution B, solution B is divided into two parts, namely solution B-1 and solution B-2, solution A and halloysite nanotubes are added into solution B-1 and stirred to obtain reverse microemulsion A, ammonia water is added into solution B-2 and stirred to obtain reverse microemulsion B, reverse microemulsion B is added dropwise into reverse microemulsion A, after adding, the reaction is stirred for 60-120 minutes, the product is separated, washed, dried and calcined.
2. The ceramic insulator according to claim 1, It is characterized in that A bonding layer is also provided between the alumina blank and the glaze layer.
3. The ceramic insulator according to claim 2, It is characterized in that The bonding layer is a silicon dioxide micro-nano structure layer.
4. The ceramic insulator according to claim 1, It is characterized in that The molar ratio of the cerium salt to the zirconium salt is 1-2.5:
1.
5. The ceramic insulator according to claim 1, It is characterized in that The calcination temperature is 500-600°C and the calcination time is 2-4h.
6. The ceramic insulator according to claim 1, It is characterized in that The preparation method of the titanium dioxide-coated indium oxide is as follows: After indium oxide is immersed in tetrabutyl titanate toluene solution for 10-30 minutes, it is separated, washed with toluene and water in a cycle, and calcined at 550-600°C for 5-10 hours. After naturally cooling to room temperature, it is taken out to obtain a pre-coated body. Tetrabutyl titanate is added to a hydrochloric acid / water solution and stirred evenly, and then the pre-coated body is added. The resulting mixed solution is transferred to a hydrothermal reactor, sealed and heated to 120-150°C for reaction for 6-10 hours. After returning to room temperature, the product is separated, washed and dried.
7. The ceramic insulator according to claim 1, It is characterized in that The glass powder is CBS glass powder.
8. A method for preparing a ceramic insulator according to any one of claims 2 to 7, It is characterized in that Ethyl orthosilicate and acetylacetone are dissolved in anhydrous acetaldehyde to obtain a first mixed solution, and the first mixed solution is sprayed on the surface of the alumina blank. A second mixed solution consisting of nitric acid, ethanol and water is also sprayed on the surface of the alumina blank. The temperature is kept at 60-70°C for 3-6 hours, then the temperature is raised to 500-600°C and pre-fired for 1-3 hours to obtain an alumina blank containing a bonding layer. Alumina, chromium oxide, hexagonal boron nitride, lithium carbonate, lanthanum oxide, dolomite, cerium-zirconium solid solution modified halloysite nanotubes, titanium dioxide coated indium oxide, strontium titanate and glass powder are ball-milled and mixed with water to obtain a glaze slurry. The glaze slurry is applied on the surface of the alumina blank, and a glaze layer with a thickness of 0.1-1 mm is obtained after drying. The semi-finished product is heated to 1350-1450°C, sintered for 2-4 hours, and then restored to room temperature.
9. The method for preparing a ceramic insulator according to claim 8, It is characterized in that The heating rate during sintering is 5-10℃ / min.
Citation Information
Patent Citations
Ceramic preparation process, the ceramic obtained via said process and their use namely as a target for cathode sputtering
CA2547091A1
High-rigidity high-power sheet aluminum oxide porous ceramic used for LED lamp heat dissipation and preparation method thereof
CN105000873A
Low-temperature-resistant high-voltage power transmission porcelain insulator and preparation method thereof
CN112441824A
Hydrocarbon conversion catalyst containing MFI zeolite and preparation method thereof
CN114425376A
High-thermal-conductivity aluminum oxide ceramic material and ceramic circuit substrate
CN116239367A