Surface-modified polymer insulator and preparation method thereof

By grafting high-voltage resistance characteristic molecular groups on the surface of polymer insulators to form a flexible two-dimensional molecular film structure, the problem of insufficient flashover voltage along the vacuum of polymer insulators in the prior art is solved, and significant increase and stability of the withstand voltage is achieved sex.

CN118969415AActive Publication Date: 2024-11-15NORTHWEST INST OF NUCLEAR TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411043793.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The existing surface chemical modification methods cannot prepare chemical components with high vacuum along-plane flashover voltage on the surface of polymer insulators, and the voltage resistance is not obvious and unstable.

Method used

The molecular groups grafted on the surface of polymer insulators using high pressure resistance characteristics to form a flexible two-dimensional molecular film structure, reducing the secondary electron emission coefficient and gas adsorption amount, and grafting on the polymer insulator body through hydrolysis or amine decomposition reactions The characteristic molecular groups are combined with the acylation reaction to form a stable modified layer.

Benefits of technology

The vacuum pressure resistance performance of the insulator is significantly improved, and the pressure resistance is relatively stable, and the bonding strength of the modified layer is high, making it suitable for insulators of various shapes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004972990180000101
    Figure BDA0004972990180000101
  • Figure BDA0004972990180000111
    Figure BDA0004972990180000111
  • Figure HDA0004972990190000011
    Figure HDA0004972990190000011
Patent Text Reader

Abstract

The invention provides a surface-modified polymer insulator and a preparation method thereof, which can solve the problems that chemical components with high vacuum surface flashover voltage cannot be prepared on the surface of the polymer insulator by the existing surface chemical modification method, and the withstand voltage is not obviously improved and is unstable. The insulator comprises a polymer insulator body and high-voltage-resistant molecular groups grafted on the surface of the polymer insulator body, the material of the polymer insulator body can be subjected to hydrolysis or aminolysis reaction, and the high-voltage-resistant molecular groups form a flexible two-dimensional molecular film structure on the surface of the polymer insulator body. The method is used for reducing the secondary electron emission coefficient and the gas adsorption quantity of the surface of a polymer insulator body. The preparation method comprises the following steps: preparing a polymer insulator body; putting the polymer insulator body into a hydrolysis or aminolysis system for reaction; cleaning and drying the polymer insulator obtained by the reaction; reacting with an acylation reagent; and finally, cleaning and drying.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an insulator and a preparation method thereof, in particular to a surface-modified polymer insulator and a preparation method thereof. Background Art

[0002] Vacuum surface flashover is a common surface discharge phenomenon in vacuum high-voltage devices such as pulse power supply equipment, high-power microwave (HPM) transmission windows, klystrons, accelerators, etc. This discharge phenomenon greatly reduces the dielectric surface's withstand voltage, making it the most vulnerable area in the device. In addition, this discharge phenomenon is also a bottleneck problem faced by vacuum high-voltage devices. At present, it is generally believed that secondary electron emission and multiplication on the insulator surface are an important process in the formation of surface flashover. Reducing secondary electron emission can effectively increase the surface flashover voltage. As a surface physical property, the secondary electron emission coefficient (SEY) is determined by the surface state of the insulator. Therefore, in order to reduce the secondary electron emission coefficient and increase the vacuum surface flashover voltage, researchers usually modify the surface of insulators. Among them, the modification of the chemical composition of the insulator surface, as a method to change the intrinsic secondary electron emission coefficient of the surface, plays an important role in improving the vacuum surface withstand voltage level of insulators (see: H.Craig Miller, "Flashover of insulators in vacuum: the last twentyyears," IEEE Transactions on Dielectrics&Electrical Insulation 22(6), 3641-3657(2016). Shengtao Li, Yongjie Nie and Daomin Min et al., "Research Progress on Vacuum Surface Flashover of Solid Dielectrics," Transactions of China Electrotechnical Society 32(8), 1-9(2017).).

[0003] Commonly used methods for chemical modification of vacuum insulator surfaces include fluorination (including direct gas fluorination, plasma-assisted fluorination, and fluorination of fluorine-containing organic molecules), coating preparation, plasma treatment, ion implantation, etc. (see: Tao Shao, Wenjin Yang and Cheng Zhang et al., "Enhanced surface flashover strength in vacuum of polymethylmethacrylate by surface modification using atmospheric-pressure dielectric barrier discharge," Appl Phys Lett 105 (7), 71607 (2014). Chao Wang, Jia Guo and Wen-Dong Li et al., "Enhancing Electrical Strength of Acrylate Polymer by Using Fluorinated Monomer as Surface Modifier," Mater Lett 249 (15), 17-20 (2019).). Through these methods, a variety of chemical components are modified onto the surface of vacuum insulators. However, since the relationship between the surface molecular structure and the vacuum surface withstand voltage characteristics of the insulator has not yet been established, it is unknown which surface chemical composition can effectively improve the vacuum surface flashover voltage of the insulator. Therefore, the existing surface chemical modification methods cannot prepare chemical compositions with high vacuum surface flashover voltage on the surface of polymer insulators, and the withstand voltage improvement is not obvious and unstable. Summary of the invention

[0004] The purpose of the present invention is to solve the technical problems that the existing surface chemical modification method cannot prepare chemical components with high vacuum surface flashover voltage on the surface of polymer insulators, and the withstand voltage improvement is not obvious and unstable, and to provide a surface modified polymer insulator and a preparation method thereof.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] A surface modified polymer insulator, which is special in that:

[0007] It includes a polymer insulator body and a high withstand voltage molecular group grafted on the surface of the polymer insulator body;

[0008] The material of the polymer insulator body can undergo hydrolysis or aminolysis reaction;

[0009] The high voltage-withstand molecular group is a high voltage-withstand molecular group that can be grafted onto the surface of the polymer insulator body according to the chemical reaction characteristics of the polymer insulator body material; the high voltage-withstand molecular group forms a flexible two-dimensional molecular film structure on the surface of the polymer insulator body, which is used to reduce the secondary electron emission coefficient and gas adsorption amount on the surface of the polymer insulator body.

[0010] Furthermore, the material of the polymer insulator body is polyamide, polyimide, polyetherimide, polyester or epoxy resin;

[0011] The high voltage resistance molecular group is a long-chain alkyl group, a carbon fluoride group or a delocalized electron group.

[0012] At the same time, the present invention also provides a method for preparing the surface-modified polymer insulator, which is special in that it comprises the following steps:

[0013] Step 1, preparing a polymer insulator body;

[0014] Step 2, placing the polymer insulator body into a 0.5 mol / L to 2 mol / L hydrolysis system, stirring and reacting at 50° C. to 80° C. for 4 h to 8 h to obtain a hydrolyzed polymer insulator;

[0015] Alternatively, the polymer insulator body is placed in a 10 mg / ml to 50 mg / ml aminolysis system, and stirred for reaction at 50° C. to 60° C. for 3 h to 6 h to obtain an aminolysis polymer insulator;

[0016] Step 3, cleaning and drying the polymer insulator obtained in step 2;

[0017] Step 4, placing the polymer insulator dried in step 3 into a non-polar organic solvent, adding an acylating agent according to a mass volume ratio of 1 g: 100 mL to 2 g: 100 mL of the non-polar organic solvent, stirring and reacting for at least 2 hours at room temperature to obtain a polymer insulator with a high withstand voltage characteristic molecular group grafted on the surface;

[0018] Step 5: Clean and dry the polymer insulator obtained in step 4 to complete the preparation of the surface-modified polymer insulator.

[0019] Furthermore, in step 2, the hydrolysis system is an acidic solution or an alkaline solution; the aminolysis system is an aqueous solution of diamine or an ethanol solution of diamine;

[0020] In step 4, the reaction is stirred for at least 2 hours and then allowed to stand for at least 12 hours;

[0021] The non-polar organic solvent is n-octane, toluene or chloroform; the acylating agent is octadecyl chloride, perfluoroundecyl chloride, perfluorooctyl chloride or phenethyl chloride.

[0022] Further, in step 2, the acidic solution is a hydrochloric acid solution or a sulfuric acid solution; the alkaline solution is a sodium hydroxide solution or a potassium hydroxide solution; the aqueous solution of diamine is an aqueous solution of ethylenediamine or an aqueous solution of hexamethylenediamine; the ethanol solution of diamine is an ethanol solution of ethylenediamine or an ethanol solution of hexamethylenediamine;

[0023] Specifically, step 3 is to place the polymer insulator obtained in step 2 into deionized water, perform ultrasonic washing for at least 30 minutes, and then dry it at 50° C. to 80° C. for at least 12 hours.

[0024] Further, step 5 specifically comprises: washing the polymer insulator obtained in step 4 with tap water, placing it in deionized water, ultrasonically washing it for at least 30 minutes, and then drying it at 50° C. to 80° C. for at least 12 hours to complete the preparation of the surface-modified polymer insulator;

[0025] Step 1 specifically involves machining the polymer insulating material into a polymer insulator body with a preset geometric structure and size.

[0026] Furthermore, step 1 specifically includes, by means of mechanical processing, manufacturing the epoxy resin insulating material into an epoxy resin insulator body with a preset geometric structure and size;

[0027] Step 2 specifically includes placing the epoxy resin insulator body into a 2 mol / L sodium hydroxide solution, stirring and reacting at 80° C. for 4 hours to obtain a hydrolyzed epoxy resin insulator;

[0028] Step 3 specifically includes placing the epoxy resin insulator obtained in step 2 in deionized water, ultrasonically washing for 30 minutes, and then drying at 80° C. for 12 hours.

[0029] Further, step 4 is specifically, putting the epoxy resin insulator dried in step 3 into n-octane, adding perfluoroundecyl chloride in a ratio of 1 g:100 mL of perfluoroundecyl chloride to n-octane by mass volume, stirring the reaction for 2 hours at room temperature and then standing for 12 hours to obtain an epoxy resin insulator with perfluoroundecyl grafted on the surface;

[0030] Step 5 specifically comprises: washing the epoxy resin insulator obtained in step 4 with tap water, placing it in deionized water, ultrasonically washing it for 30 minutes, and then drying it at 80° C. for 12 hours to complete the preparation of the surface-modified epoxy resin insulator.

[0031] Furthermore, step 1 specifically includes, by means of mechanical processing, making the polyamide insulating material into a polyamide insulator body with a preset geometric structure and size;

[0032] Step 2 specifically comprises placing the polyamide insulator body into a 50 mg / ml hexamethylenediamine solution, stirring and reacting at 60° C. for 3 hours to obtain an aminolyzed polyamide insulator;

[0033] Step 3 specifically comprises placing the polyamide insulator obtained in step 2 into deionized water, ultrasonically washing for 30 minutes, and then drying at 80° C. for 12 hours.

[0034] Further, step 4 is specifically, putting the polyamide insulator dried in step 3 into n-octane, adding octadecyl chloride in a ratio of 1 g:100 mL of mass volume ratio of octadecyl chloride to n-octane, stirring the reaction for 2 hours at room temperature and then standing for 12 hours to obtain a polyamide insulator with octadecyl grafted on the surface;

[0035] Step 5 specifically comprises: washing the polyamide insulator obtained in step 4 with tap water, placing it in deionized water, ultrasonically washing it for 30 minutes, and then drying it at 80° C. for 12 hours to complete the preparation of the surface-modified polyamide insulator.

[0036] Beneficial effects of the present invention:

[0037] 1. The present invention provides a surface-modified polymer insulator and a preparation method thereof, wherein high voltage-withstand molecular groups are grafted onto the surface of the polymer insulator body, which can reduce the secondary electron emission coefficient and gas adsorption amount on the surface of the polymer insulator body, thereby achieving a significant improvement in the vacuum surface voltage-withstand performance of the insulator, and the voltage-withstand improvement is relatively stable.

[0038] 2. Compared with the traditional method of preparing a modified layer on the surface of the insulator body by using intermolecular interaction and mechanical riveting, the high voltage-resistant molecular groups in the present invention are chemically connected to the insulator body, and the molecular modified layer will not change over time, and has higher bonding strength and stability.

[0039] 3. In the present invention, liquid phase reaction conditions are adopted, and uniform chemical reaction can occur at the positions where the insulator body contacts the liquid phase, the grafted high-voltage-withstand molecular groups are evenly distributed, and the flashover voltage is stably increased; in addition, the liquid phase reaction conditions can be used for insulators of various shapes and have a wide range of applications.

[0040] 4. In the present invention, the high voltage withstand molecular groups grafted onto the surface of the insulator body will not destroy the bulk structure of the insulator, and can ensure the mechanical strength of the insulator; it only needs to be grafted to function, and will not change any structural parameters of the original insulation system. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 : is a reaction route diagram of the preparation method of the surface-modified epoxy resin insulator in Example 1 of the present invention (R is perfluoroundecyl); in the diagram, Polymer-OH represents the epoxy resin containing hydroxyl groups after hydrolysis;

[0042] Figure 2 is a reaction route diagram of a preparation method of a surface-modified epoxy resin insulator in other embodiments of the present invention (R is a molecular group with high withstand voltage characteristics such as a long-chain alkyl group, a carbon fluoride group or a delocalized electron group); in the figure, HO-Polymer-NH2 represents an epoxy resin containing amino groups and hydroxyl groups after aminolysis;

[0043] Figure 3 This is a reaction route diagram of the preparation method of the surface-modified nylon insulator in Example 2 of the present invention (R is octadecyl); in the diagram, Polymer-NH2 represents nylon containing amino groups after aminolysis;

[0044] Figure 4 : is a reaction route diagram of the preparation method of the surface-modified polyimide insulator in Example 3 of the present invention (R is phenylethyl); in the diagram, Polymer-NH2 represents the polyimide containing amino groups after aminolysis;

[0045] Figure 5 This is a reaction route diagram of the preparation method of the surface-modified nylon insulator in Example 5 of the present invention (R is octadecyl); in the diagram, Polymer-NH2 represents nylon containing amino groups after hydrolysis;

[0046] Figure 6 This is a reaction route diagram of the preparation method of the surface-modified polyimide insulator in Example 6 of the present invention (R is phenylethyl); in the diagram, Polymer-NH2 represents the polyimide containing amino groups after hydrolysis. DETAILED DESCRIPTION

[0047] Embodiment 1

[0048] A surface-modified polymer insulator comprises a polymer insulator body and a high-voltage-withstand molecular group grafted on the surface of the polymer insulator body. The material of the polymer insulator body can undergo hydrolysis or aminolysis reaction, and the high-voltage-withstand molecular group is a high-voltage-withstand molecular group that can be grafted on the surface of the polymer insulator body according to the chemical reaction characteristics of the material of the polymer insulator body. The high-voltage-withstand molecular group is regularly arranged on the surface of the polymer insulator body to form a flexible two-dimensional molecular film structure, which is used to reduce the secondary electron emission coefficient and gas adsorption amount on the surface of the polymer insulator body. In this embodiment, the material of the polymer insulator body is epoxy resin, and the high-voltage-withstand molecular group is perfluoroundecyl. The perfluoroundecyl grafted on the surface of the epoxy resin insulator body is driven by intermolecular forces and arranged regularly on the surface of the epoxy resin insulator body to form a flexible two-dimensional molecular film structure. Since the molecular groups of this structure can swing within a certain range and adjust spontaneously, it has a certain flexibility. This flexible two-dimensional molecular film structure can give the insulator surface higher stability and reduce the adsorption of gas molecules, that is, it can reduce the secondary electron emission coefficient and gas adsorption amount on the surface of the epoxy resin insulator body, thereby inhibiting the development of vacuum surface flashover on the insulator surface and improving the vacuum surface withstand voltage performance of the epoxy resin insulator.

[0049] This embodiment also provides a method for preparing the above-mentioned surface-modified epoxy resin insulator, comprising the following steps:

[0050] Step 1: Through mechanical processing, the epoxy resin insulation material is made into an epoxy resin insulator body with a thickness of 5 mm and a diameter of 30 mm.

[0051] Step 2: Place the epoxy resin insulator body into a 2 mol / L sodium hydroxide solution, stir and react for 4 hours at 80° C. to hydrolyze the epoxy resin insulator to obtain a hydrolyzed epoxy resin insulator.

[0052] Step 3: Place the epoxy resin insulator obtained in step 2 into deionized water, perform ultrasonic washing for 30 minutes, and then dry it in an oven at 80° C. for 12 hours.

[0053] Step 4, the epoxy resin insulator dried in step 3 is placed in 50 mL of n-octane, and 0.5 g of perfluoroundecyl chloride is added according to the mass volume ratio of perfluoroundecyl chloride to n-octane of 1 g:100 mL. Under room temperature, the reaction is stirred for 2 hours and then allowed to stand for 12 hours for amidation to obtain an epoxy resin insulator with perfluoroundecyl grafted on the surface;

[0054] Step 5: After washing the epoxy resin insulator obtained in step 4 with a large amount of tap water, put it into deionized water and perform ultrasonic washing for 30 minutes, and then use an oven at 80° C. to dry it for 12 hours to complete the preparation of the surface-modified epoxy resin insulator, which is recorded as "perfluoroundecyl grafted insulator 1".

[0055] Figure 1 is a reaction route diagram of the preparation method of the surface-modified epoxy resin insulator in this embodiment, comprising Figure 1 It can be seen that according to the chemical reaction characteristics of epoxy resin, hydroxyl groups are grafted onto the epoxy resin molecular chain by hydrolysis, and then the acyl chloride with a terminal group of perfluoroundecyl (i.e., carbon fluoride) is used. With the help of the esterification reaction between the hydroxyl group and the acyl chloride, the perfluoroundecyl group is grafted onto the surface of the epoxy resin insulator body, thereby reducing the secondary electron emission coefficient and the surface gas adsorption amount on the surface of the insulator body, thereby improving the vacuum surface withstand voltage performance of the epoxy resin insulator.

[0056] Figure 2 It is a reaction route diagram of the preparation method of the surface-modified epoxy resin insulator in other embodiments. According to the chemical reaction characteristics of the epoxy resin, the amino group and the hydroxyl group can also be grafted onto the epoxy resin molecular chain by the method of aminolysis, and then the high-voltage-withstand molecular group such as the terminal group being a long-chain alkyl group, a carbon fluoride group or a delocalized electron group is grafted onto the surface of the epoxy resin insulator body by the amidation reaction of the amino group and the acyl chloride and the esterification reaction of the hydroxyl group and the acyl chloride, thereby reducing the secondary electron emission coefficient and the surface gas adsorption amount on the surface of the insulator body, thereby improving the vacuum surface withstand voltage performance of the epoxy resin insulator.

[0057] Embodiment 2

[0058] The difference between the polymer insulator in this embodiment and the polymer insulator in the first embodiment is that:

[0059] The material of the polymer insulator body is polyamide, specifically nylon, and the molecular group with high voltage resistance is octadecyl.

[0060] This embodiment also provides a method for preparing a surface-modified nylon insulator, comprising the following steps:

[0061] Step 1: Use mechanical processing to make the nylon insulating material into a nylon insulator body with a thickness of 5 mm and a diameter of 30 mm.

[0062] Step 2: Place the nylon insulator body into a 50 mg / ml hexamethylenediamine aqueous solution, stir and react for 3 hours at 60° C. to perform aminolysis to obtain an aminolyzed nylon insulator.

[0063] Step 3: Place the nylon insulator obtained in step 2 into deionized water, perform ultrasonic washing for 30 minutes, and then dry it in an oven at 80° C. for 12 hours.

[0064] Step 4: Place the dried nylon insulator in step 3 into 50 mL of n-octane, add 0.5 g of octadecyl chloride in a ratio of 1 g:100 mL of mass volume of octadecyl chloride to n-octane, stir the reaction for 2 h at room temperature, and then let it stand for 12 h for amidation to obtain a nylon insulator with octadecyl grafted on the surface.

[0065] Step 5: After washing the nylon insulator obtained in step 4 with a large amount of tap water, put it into deionized water and ultrasonically wash it for 30 minutes, and then use an oven at 80° C. to dry it for 12 hours to complete the preparation of the surface-modified nylon insulator, which is recorded as "octadecyl grafted insulator 2".

[0066] Figure 3 This is the reaction route of the preparation method of the surface-modified nylon insulator in this embodiment. According to the chemical reaction characteristics of nylon, the amino group is grafted onto the nylon molecular chain by the aminolysis method, and then the octadecyl group is grafted onto the nylon molecular chain by means of the amidation reaction between the amino group and octadecyl chloride.

[0067] Embodiment 3

[0068] The difference between the polymer insulator in this embodiment and the polymer insulator in the first embodiment is that:

[0069] The material of the polymer insulator body is polyimide, and the molecular group with high withstand voltage characteristics is phenylethyl (ie, delocalized electron group). In other embodiments, the polyimide material can be replaced with polyetherimide.

[0070] This embodiment also provides a method for preparing a surface-modified polyimide insulator, comprising the following steps:

[0071] Step 1: Through mechanical processing, the polyimide insulating material is made into a polyimide insulator body with a thickness of 5 mm and a diameter of 30 mm.

[0072] Step 2: Place the polyimide insulator body into a 30 mg / ml aqueous solution of ethylenediamine, stir and react for 4 hours at 55° C. to perform aminolysis to obtain an aminolyzed polyimide insulator. In other embodiments, the aqueous solution of ethylenediamine in this step can be replaced with an aqueous solution of hexamethylenediamine.

[0073] Step 3: Place the polyimide insulator obtained in step 2 into deionized water, perform ultrasonic washing for 35 minutes, and then dry it in an oven at 65° C. for 12.5 hours.

[0074] Step 4: Put the polyimide insulator dried in step 3 into 50 mL of toluene, add 0.75 g of phenylethyl chloride according to the mass volume ratio of phenylethyl chloride to toluene of 1.5 g:100 mL, stir the reaction for 2 hours at room temperature, and then let it stand for 13 hours to carry out amidation to obtain a polyimide insulator with phenylethyl grafted on the surface.

[0075] Step 5: After washing the polyimide insulator obtained in step 4 with a large amount of tap water, put it into deionized water and ultrasonically wash it for 35 minutes, and then use an oven at 65° C. to dry it for 12.5 hours to complete the preparation of the surface-modified polyimide insulator, which is recorded as "phenylethyl grafted insulator 3".

[0076] Figure 4 is a reaction route diagram of the preparation method of the surface-modified polyimide insulator in this embodiment. The reaction principle of this diagram is explained in the same way as in Example 2. Figure 3 The reaction principle is explained similarly.

[0077] Embodiment 4

[0078] The difference between the polymer insulator in this embodiment and the polymer insulator in the first embodiment is that:

[0079] The material of the polymer insulator body is polyester, and the molecular group with high voltage resistance is perfluorooctyl.

[0080] This embodiment also provides a method for preparing a surface-modified polyester insulator, comprising the following steps:

[0081] Step 1: Through mechanical processing, the polyester insulating material is made into a polyester insulator body with a thickness of 5 mm and a diameter of 30 mm.

[0082] Step 2: Place the polyester insulator body into a 10 mg / ml ethylenediamine ethanol solution, stir and react for 6 hours at 50° C. to perform aminolysis to obtain an aminolyzed polyester insulator. In other embodiments, the ethylenediamine ethanol solution in this step can be replaced with a hexamethylenediamine ethanol solution.

[0083] Step 3: Place the polyester insulator obtained in step 2 into deionized water, perform ultrasonic washing for 40 minutes, and then dry it in an oven at 50° C. for 13 hours.

[0084] Step 4: Place the polyester insulator dried in step 3 into 50 mL of chloroform, add 1 g of perfluorooctyl chloride in a mass volume ratio of 2 g:100 mL of chloroform, stir the reaction for 2.5 h at room temperature, and then let it stand for 12 h for amidation to obtain a polyester insulator with perfluorooctyl grafted on the surface.

[0085] Step 5: After washing the polyester insulator obtained in step 4 with a large amount of tap water, put it into deionized water and perform ultrasonic washing for 40 minutes, and then use an oven at 50° C. to dry it for 13 hours to complete the preparation of the surface-modified polyester insulator, which is recorded as "perfluorooctyl grafted insulator 4".

[0086] The reaction principle of this embodiment is explained in the same way as in Example 2. Figure 3 In other embodiments, a polyester insulator with perfluorooctyl grafted on the surface can be obtained by hydrolysis-esterification, and the reaction principle is explained in the same way as in Example 1. Figure 1 The reaction principle explanation is the same.

[0087] Embodiment 5

[0088] The polymer insulator in this embodiment is the same as the polymer insulator in the second embodiment.

[0089] The difference between the preparation method in this embodiment and the preparation method in Example 2 is that:

[0090] Step 2 is specifically as follows: placing the nylon insulator body into a 1 mol / L potassium hydroxide solution, stirring and reacting at 65° C. for 6 hours to perform hydrolysis, thereby obtaining a hydrolyzed nylon insulator.

[0091] In step 3, the ultrasonic washing time is 40 minutes, the drying temperature is 50° C., and the drying time is 13 hours.

[0092] Step 4 is specifically as follows: the nylon insulator dried in step 3 is placed in 50 mL of toluene, 1 g of octadecyl chloride is added in a ratio of 2 g:100 mL of octadecyl chloride to toluene by mass volume, and the reaction is stirred for 2.5 hours at room temperature and then allowed to stand for 12 hours for amidation to obtain a nylon insulator with octadecyl grafted on the surface.

[0093] In step 5, the ultrasonic washing time is 40 minutes, the drying temperature is 50° C., and the drying time is 13 hours. The prepared surface-modified nylon insulator is recorded as “octadecyl grafted insulator 5”.

[0094] Figure 5 This is a reaction route diagram of the preparation method of the surface-modified nylon insulator in this embodiment. According to the chemical reaction characteristics of nylon, the hydrolysis method is selected to graft the amino group on the nylon molecular chain, and then the octadecyl group is grafted on the nylon molecular chain by means of the amidation reaction between the amino group and octadecyl chloride.

[0095] Embodiment 6

[0096] The polymer insulator in this embodiment is the same as the polymer insulator in the third embodiment.

[0097] The difference between the preparation method in this embodiment and the preparation method in embodiment 3 is that:

[0098] Step 2 is specifically as follows: placing the polyimide insulator body into a 0.5 mol / L hydrochloric acid solution, stirring and reacting for 8 hours at 50° C., and hydrolyzing to obtain a hydrolyzed polyimide insulator. In other embodiments, the hydrochloric acid solution can be replaced by a sulfuric acid solution.

[0099] Step 4 is specifically as follows: the polyimide insulator dried in step 3 is placed in 50 mL of chloroform, 0.75 g of phenylethyl chloride is added according to a mass volume ratio of phenylethyl chloride to chloroform of 1.5 g:100 mL, and the reaction is stirred for 2 hours at room temperature and then allowed to stand for 13 hours for amidation to obtain a polyimide insulator with phenylethyl grafted on the surface.

[0100] In step 5, the surface-modified polyimide insulator prepared is recorded as "phenylethyl grafted insulator 6".

[0101] Figure 6 is a reaction route diagram of the preparation method of the surface-modified polyimide insulator in this embodiment. The reaction principle of this diagram is explained in the same way as in Example 5. Figure 5 The reaction principle explanation is the same.

[0102] The surface-modified polymer insulators prepared in the above-mentioned Examples 1 to 6 and the corresponding polymer insulator bodies were subjected to vacuum surface flashover voltage tests on a vacuum surface flashover voltage test bench with a pulse width of 500 ns. The flashover voltage test results are shown in Table 1.

[0103] Table 1

[0104]

[0105]

[0106] As shown in Table 1, the flashover voltage of the insulator with high withstand voltage molecular groups grafted on the surface of the present invention is increased by 30% to 40% compared with the polymer insulator body, indicating that the surface-modified polymer insulator prepared by the present invention can effectively increase the flashover voltage of the insulator.

[0107] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A surface-modified polymer insulator, characterized in that: It includes a polymer insulator body and a high withstand voltage molecular group grafted on the surface of the polymer insulator body; The material of the polymer insulator body can undergo hydrolysis or aminolysis reaction; The high voltage-withstand molecular group is a high voltage-withstand molecular group that can be grafted onto the surface of the polymer insulator body according to the chemical reaction characteristics of the polymer insulator body material; the high voltage-withstand molecular group forms a flexible two-dimensional molecular film structure on the surface of the polymer insulator body, which is used to reduce the secondary electron emission coefficient and gas adsorption amount on the surface of the polymer insulator body.

2. The surface-modified polymer insulator according to claim 1, characterized in that: The polymer insulator body is made of polyamide, polyimide, polyetherimide, polyester or epoxy resin; The high voltage resistance molecular group is a long-chain alkyl group, a carbon fluoride group or a delocalized electron group.

3. A method for preparing the surface-modified polymer insulator according to claim 1 or 2, characterized in that: The following steps are involved: Step 1, preparing a polymer insulator body; Step 2, placing the polymer insulator body into a 0.5 mol / L to 2 mol / L hydrolysis system, stirring and reacting at 50° C. to 80° C. for 4 h to 8 h to obtain a hydrolyzed polymer insulator; Alternatively, the polymer insulator body is placed in a 10 mg / ml to 50 mg / ml aminolysis system, and stirred for reaction at 50° C. to 60° C. for 3 h to 6 h to obtain an aminolysis polymer insulator; Step 3, cleaning and drying the polymer insulator obtained in step 2; Step 4, placing the polymer insulator dried in step 3 into a non-polar organic solvent, adding an acylating agent according to a mass volume ratio of 1 g: 100 mL to 2 g: 100 mL of the non-polar organic solvent, stirring and reacting for at least 2 hours at room temperature to obtain a polymer insulator with a high withstand voltage characteristic molecular group grafted on the surface; Step 5: Clean and dry the polymer insulator obtained in step 4 to complete the preparation of the surface-modified polymer insulator.

4. The method for preparing a surface-modified polymer insulator according to claim 3, characterized in that: In step 2, the hydrolysis system is an acidic solution or an alkaline solution; the aminolysis system is an aqueous solution of diamine or an ethanol solution of diamine; In step 4, the reaction is stirred for at least 2 hours and then allowed to stand for at least 12 hours; The non-polar organic solvent is n-octane, toluene or chloroform; the acylating agent is octadecyl chloride, perfluoroundecyl chloride, perfluorooctyl chloride or phenethyl chloride.

5. The method for preparing a surface-modified polymer insulator according to claim 4, characterized in that: In step 2, the acidic solution is a hydrochloric acid solution or a sulfuric acid solution; the alkaline solution is a sodium hydroxide solution or a potassium hydroxide solution; the aqueous solution of diamine is an aqueous solution of ethylenediamine or an aqueous solution of hexamethylenediamine; the ethanol solution of diamine is an ethanol solution of ethylenediamine or an ethanol solution of hexamethylenediamine; Specifically, step 3 is to place the polymer insulator obtained in step 2 into deionized water, perform ultrasonic washing for at least 30 minutes, and then dry it at 50° C. to 80° C. for at least 12 hours.

6. The method for preparing a surface-modified polymer insulator according to claim 5, characterized in that: Step 5 specifically comprises: washing the polymer insulator obtained in step 4 with tap water, placing it in deionized water, ultrasonically washing it for at least 30 minutes, and then drying it at 50° C. to 80° C. for at least 12 hours to complete the preparation of the surface-modified polymer insulator; Step 1 specifically involves machining the polymer insulating material into a polymer insulator body with a preset geometric structure and size.

7. The method for preparing a surface-modified polymer insulator according to claim 6, characterized in that: Step 1 specifically includes, by means of mechanical processing, manufacturing the epoxy resin insulating material into an epoxy resin insulator body with a preset geometric structure and size; Step 2 specifically includes placing the epoxy resin insulator body into a 2 mol / L sodium hydroxide solution, stirring and reacting at 80° C. for 4 hours to obtain a hydrolyzed epoxy resin insulator; Step 3 specifically includes placing the epoxy resin insulator obtained in step 2 in deionized water, ultrasonically washing for 30 minutes, and then drying at 80° C. for 12 hours.

8. The method for preparing a surface-modified polymer insulator according to claim 7, characterized in that: Step 4 is specifically, putting the epoxy resin insulator dried in step 3 into n-octane, adding perfluoroundecyl chloride in a ratio of 1 g to 100 mL of n-octane by mass volume, stirring the reaction for 2 hours at room temperature and then standing for 12 hours to obtain an epoxy resin insulator with perfluoroundecyl grafted on the surface; Step 5 specifically comprises: washing the epoxy resin insulator obtained in step 4 with tap water, placing it in deionized water, ultrasonically washing it for 30 minutes, and then drying it at 80° C. for 12 hours to complete the preparation of the surface-modified epoxy resin insulator.

9. The method for preparing a surface-modified polymer insulator according to claim 6, characterized in that: Step 1 specifically includes, by means of mechanical processing, making the polyamide insulating material into a polyamide insulator body with a preset geometric structure and size; Step 2 specifically comprises placing the polyamide insulator body into a 50 mg / ml hexamethylenediamine solution, stirring and reacting at 60° C. for 3 hours to obtain an aminolyzed polyamide insulator; Step 3 specifically comprises placing the polyamide insulator obtained in step 2 into deionized water, ultrasonically washing for 30 minutes, and then drying at 80° C. for 12 hours.

10. The method for preparing a surface-modified polymer insulator according to claim 9, characterized in that: Step 4 is specifically, putting the polyamide insulator dried in step 3 into n-octane, adding octadecyl chloride in a ratio of 1 g:100 mL of mass volume ratio of octadecyl chloride to n-octane, stirring the reaction for 2 hours at room temperature and then standing for 12 hours to obtain a polyamide insulator with octadecyl grafted on the surface; Step 5 specifically comprises: washing the polyamide insulator obtained in step 4 with tap water, placing it in deionized water, ultrasonically washing it for 30 minutes, and then drying it at 80° C. for 12 hours to complete the preparation of the surface-modified polyamide insulator.

Citation Information

Patent Citations

  • REsin Composition For Insulating Materials, Insulating Ink, Insulating Film And Organic Field Effect Transistor Using Insulating Film

    CN104981490A

  • Method for improving flashover voltage of ceramic insulator

    CN110136901A

  • Preparation method of ceramic vacuum insulator with conjugated molecule groups on surface and insulator

    CN116313335A

  • Conjugated polymer coating, preparation method of conjugated polymer coating, vacuum insulator and preparation method of vacuum insulator

    CN116396677A

  • Insulator

    JP1993036324A