A kind of iron oxide red powder and preparation method thereof
By using a mixture of dilute acid solution and dispersant in the preparation of iron oxide red powder, grinding and demagnetization and airflow crushing treatment, the problems of purity and morphology requirements of existing iron oxide red powder in battery new energy materials are solved. It realizes efficient and low-cost spherical treatment, suitable for large-scale production.
Patent Information
- Application Number
- CN202210625406.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-06-02
AI Technical Summary
The existing iron oxide red powder cannot meet the requirements of high purity, low impurity, spherical, uniformization and miniaturization in the application of new battery energy materials, and the production process has the disadvantages of high impurity content, high energy consumption and small output.
The suspension is prepared by mixing dilute acid solution, dispersant and iron oxide red powder. After grinding, magnetization removal, filtration, cleaning and airflow crushing, impurities are removed and spherical treatment is achieved to improve the iron oxide content and particle morphology.
It realizes high purity, low impurity, spherical, uniform and miniaturization of iron oxide red powder, reduces energy consumption and cost, and is suitable for large-scale industrial production.
Smart Images

Figure CN116768279B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a red iron oxide powder and a preparation method thereof, and specifically to a production process for increasing the iron oxide content in red iron oxide and sphericalization of particles, belonging to the field of battery new energy materials. Background Art
[0002] There are many methods for preparing red iron oxide. There are two main process routes for large-scale production of red iron oxide. One is that the pigment factory uses waste iron sheets to react with acid to obtain ferrous solution, which is then alkalized to generate ferrous hydroxide, and then continuously oxidized and precipitated in the reaction barrel, commonly known as the precipitation method; the other is that the steel plant uses the ferrous solution after pickling the steel plate and sprays it under high temperature conditions, commonly known as the roasting method or the Roots method. The red iron oxide produced by the precipitation method has the advantages of small particle size, high specific surface area, and high hiding power, but the production process is long, the impurity content is high, the iron oxide content in the product is less than 97%, and the particle morphology is difficult to control; the red iron oxide produced by the roasting method has the advantages of iron oxide content greater than 97%, simple process, large output, and short production cycle, but the resulting product has the disadvantages of large particle size, small specific surface area, high chlorine content, and large fluctuations in metal impurity content.
[0003] Patent Document 1, Patent Document 2 and Patent Document 3 all use water to wash the iron oxide powder, but have limited ability to remove metal impurities in the iron oxide powder and cannot remove most of the metal impurities to below 100 ppm; moreover, no grinding aid is used in the processing, the grinding time is long, and the energy consumption is high; and the increase in the iron oxide content is limited.
[0004] The overall performance of the above products cannot meet the requirements of new energy battery materials for high purity, low impurities, spherical, uniform and small grain morphology of red iron oxide, and cannot be used on a large scale in this field.
[0005] Citations
[0006] Patent document 1: CN107601575A
[0007] Patent document 2: CN100366544A
[0008] Patent document 3: CN105399143A Summary of the invention
[0009] Problem that the invention aims to solve
[0010] In view of the above reasons, the present invention provides a production process for increasing the iron oxide content and spheroidizing particles, which can effectively reduce various impurities in the iron oxide red produced by the above two processes, increase the iron oxide content, and make the grain morphology spheroidized, uniform, and small. The present invention has simple process, low cost, low energy consumption, high output, and is suitable for industrial large-scale production.
[0011] Solutions for solving problems
[0012] The purpose of the present invention can be achieved by the following technical solutions:
[0013] [1] A red iron oxide powder comprising 98.0% by mass or more of Fe2O3 and 0.01% by mass or less of each of K, Na, Ca, Mg, Zn, Cu and Ti,
[0014] The red iron oxide has a substantially spherical shape and a median particle size D50 of 0.2 μm to 1.0 μm.
[0015] [2] The red iron oxide powder according to the above [1], wherein the K content is 15 ppm or less, preferably 10 ppm or less; and / or the Na content is 95 ppm or less, preferably 85 ppm or less; and / or the Ca content is 80 ppm or less, preferably 50 ppm or less; and / or the Mg content is 60 ppm or less, preferably 40 ppm or less; and / or the Zn content is 65 ppm or less, preferably 45 ppm or less; and / or the Cu content is 60 ppm or less, preferably 40 ppm or less; and / or the Ti content is 90 ppm or less, preferably 86 ppm or less.
[0016] [3] The red iron oxide powder according to [1] or [2] above, further comprising a Mn content of 0.18 mass % or less, preferably 0.15 mass % or less; and / or, further comprising an Al content of 0.1 mass % or less, preferably 0.08 mass % or less; and / or, further comprising a Cl content of 0.1 mass % or less.
[0017] [4] The red iron oxide powder according to any one of [1] to [3] above, wherein the median particle size D50 of the red iron oxide powder is 0.3 μm to 0.8 μm; and / or the D10 of the red iron oxide powder is 0.1 μm to 0.5 μm, and the D97 is 0.8 μm to 1.5 μm; and / or the volume average particle size of the red iron oxide powder is 0.3 to 0.9 μm; and / or the specific surface area of the red iron oxide powder is 2000 m 2 / kg or more.
[0018] [5] A method for preparing the red iron oxide powder described in any one of [1] to [4] above, comprising the following steps:
[0019] A suspension preparation step of mixing a dilute acid solution, a dispersant and red iron oxide powder to obtain a red iron oxide suspension;
[0020] The obtained suspension is ground to obtain a grinding slurry, and then demagnetized to obtain a demagnetized grinding slurry;
[0021] The step of filtering, washing and drying the demagnetized grinding slurry to obtain a crude iron oxide red product; and
[0022] The step of spheroidizing the crude red iron oxide is performed by pulverizing the crude red iron oxide to obtain a spherical red iron oxide powder as a product.
[0023] [6] The preparation method according to the above [5], wherein the dilute acid is one or more of sulfuric acid, nitric acid, formic acid, acetic acid, carbonic acid, oxalic acid, citric acid, malic acid, tartaric acid, succinic acid, benzoic acid, and salicylic acid; and / or the concentration of the dilute acid solution is 0.2 to 2.0% by mass.
[0024] [7] The preparation method according to the above [5] or [6], wherein the dispersant is a non-ionic surfactant, and the non-ionic surfactant includes one or more of polyoxyethylene ethers, polyols, polyol esters, and amides; and / or the polyoxyethylene ethers include one or more of alkylphenol polyoxyethylene ethers, fatty alcohol polyoxyethylene ethers, and fatty acid polyoxyethylene ethers; and / or the polyols include one or more of polyethylene glycol 200, polyethylene glycol 400, polyethylene glycol 600, polypropylene glycol, and polybutylene glycol; and / or the polyol esters include one or more of Tween 20, Tween 40, Tween 60, and Tween 80; and / or the amides include one or more of stearic acid diethanolamide, coconut acid diethanolamide, and coconut acid monoethanolamide.
[0025] [8] The preparation method according to any one of [5] to [7] above, wherein the proportion of the dispersant in the red iron oxide suspension is 0.2 to 2.0 mass %; and / or the proportion of the red iron oxide powder in the red iron oxide suspension is 40 to 80 mass %.
[0026] [9] The preparation method according to any one of [5] to [8] above, wherein the demagnetization is performed by passing the polishing slurry through a pipeline demagnetizer during the process of sending the polishing slurry to the filtering device; and / or, the cleaning is performed using pure water with a conductivity of 10 megohms.
[0027]
[10] A preparation method according to any one of [5] to [9] above, wherein the spheroidization step comprises coarsely crushing the crude red iron oxide product, and then finely crushing and spheroidizing the product by using a jet mill to obtain a spherical red iron oxide powder as a product.
[0028] Effects of the Invention
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1) The red iron oxide powder of the present invention has a substantially spherical shape, a narrow particle size distribution, a greatly reduced content of metal impurities, and an increased content of red iron oxide.
[0031] 2) In the preparation method of the present invention, various impurities and magnetic impurities wrapped inside the iron oxide powder are removed by acid leaching, grinding and refining, and magnetic separation, and then the iron oxide content in the red iron oxide powder is increased by washing with pure water, and the particles are spheroidized by a jet mill, so that the produced red iron oxide powder can meet the requirements of battery new energy materials for raw materials.
[0032] 3) The invention has simple process, room temperature operation, low cost, low energy consumption, high output, and is suitable for industrial large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1A This is the particle size distribution diagram of the untreated iron oxide red powder in Example 1.
[0034] Figure 1B This is the particle size distribution diagram of the red iron oxide product after treatment in Example 1.
[0035] Figure 2A Particle size distribution diagram of the untreated iron oxide red powder in Example 2.
[0036] Figure 2B This is the particle size distribution diagram of the red iron oxide product after treatment in Example 2.
[0037] Figure 3A This is the particle size distribution diagram of the untreated iron oxide red powder in Example 3.
[0038] Figure 3B This is the particle size distribution diagram of the red iron oxide product after treatment in Example 3.
[0039] Figure 4A This is a scanning electron microscope photograph of the untreated iron oxide red powder in Example 1.
[0040] Figure 4B This is a scanning electron microscope photo of the iron oxide red product after treatment in Example 1. DETAILED DESCRIPTION
[0041] The following describes the embodiments of the present invention, but the present invention is not limited thereto. The present invention is not limited to the various structures described below, and various changes can be made within the scope of the invention claim, and the embodiments and embodiments obtained by appropriately combining the technical means disclosed in different embodiments and embodiments are also included in the technical scope of the present invention. In addition, all the documents recorded in this specification are cited in this specification as references.
[0042] Unless defined otherwise, technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0043] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values A and B.
[0044] In this specification, unless otherwise stated, "multiple" in "multiple", "multiple", "plurality", etc. means a numerical value of 2 or more.
[0045] In the present specification, “substantially” means that the difference is 5% or less, 3% or less, or 1% or less compared to the relevant perfect standard or theoretical standard.
[0046] In this specification, unless otherwise specified, "%" means mass percentage.
[0047] In this specification, "ppm" means mass ppm unless otherwise specified.
[0048] In this specification, "D10", "D50" and "D97" have the usual meanings in this field. For example, D10 is the particle size corresponding to when the cumulative particle size distribution number of a sample reaches 10%, and its physical meaning is that particles with a particle size smaller than it account for 10%. Similarly, D50 is the particle size corresponding to when the cumulative particle size distribution percentage of a sample reaches 50%, and its physical meaning is that particles with a particle size larger than it account for 50%, and particles with a particle size smaller than it also account for 50%, so D50 is also called the median diameter or median particle size. Similarly, D97 is the particle size corresponding to when the cumulative particle size distribution number of a sample reaches 97%, and its physical meaning is that particles with a particle size smaller than it account for 97%.
[0049] In this specification, the "span" is a value calculated by the formula (D90-D10) / D50.
[0050] In this specification, the word "may" includes both performing a certain process and not performing a certain process.
[0051] In the present specification, "optional" or "optionally" means that the event or situation described below may or may not occur, and the description includes cases where the event occurs and cases where it does not occur.
[0052] In this specification, "include" and any variation thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device comprising a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to these processes, methods, products or devices.
[0053] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.
[0054] [First aspect]
[0055] A first aspect of the present invention relates to a red iron oxide powder having a spherical shape or a substantially spherical shape and a narrow particle size distribution.
[0056] In a specific embodiment of the present invention, the median particle size D50 of the iron oxide red powder is 0.2 μm to 1.0 μm, preferably 0.3 μm to 0.8 μm, D10 is 0.1 μm to 0.5 μm, and D97 is 0.8 μm to 1.5 μm. The volume average particle size of the iron oxide red powder is 0.3 μm to 0.9 μm, preferably 0.4 μm to 0.8 μm. In the particle size distribution of the iron oxide red powder, the span is 1.0 to 1.8, preferably 1.0 to 1.6.
[0057] In some specific embodiments of the present invention, the specific surface area of the red iron oxide powder can be 2000m 2 / kg or more, preferably 2500m 2 Although there is no particular upper limit on the specific surface area, the specific surface area of red iron oxide powder is usually 8000 m 2 / kg or less, preferably 7000m 2 / kg or less. For example, the specific surface area of red iron oxide powder can be 2000m 2 / kg and above and 8000m 2 / kg or less.
[0058] The iron oxide red powder of the present invention also has the characteristics of high Fe2O3 content and greatly reduced impurity content. Specifically, the iron oxide red powder of the present invention contains more than 98.0% by mass of Fe2O3, and contains K, Na, Ca, Mg, Zn, Cu, and Ti each with a content of less than 0.01% by mass (i.e., less than 100 ppm).
[0059] In the present invention, the iron oxide red powder contains 98.0 mass % or more of Fe2O3. For example, the Fe2O3 content may be 98.0 mass %, 98.2 mass %, 98.4 mass %, 98.6 mass %, 98.8 mass %, 99.0 mass %, 99.2 mass %, 99.5 mass %, etc. These values may be arbitrarily combined to form a numerical range. For example, the Fe2O3 content may be 98.0 mass % to 99.5 mass %, or 98.4 mass % to 99.5 mass %, etc.
[0060] In some embodiments of the present invention, the content of K is less than 15ppm, preferably less than 10ppm, more preferably less than 5ppm, or even less than 1ppm. On the other hand, the content of K can be more than 0.5ppm. For example, the content of K can be 0.5ppm, 1ppm, 2ppm, 3ppm, 4ppm, 5ppm, 6ppm, 7ppm, 8ppm, 9ppm, 10ppm, 12ppm, 15ppm, etc. These values can be arbitrarily combined to form a numerical range. For example, the content of K can be 0.5ppm to 15ppm, 0.5ppm to 5ppm, etc.
[0061] In some embodiments of the present invention, the content of Na is 95ppm or less, preferably 85ppm or less, more preferably 50ppm or less. On the other hand, the content of Na may be 20ppm or more. For example, the content of Na may be 20ppm, 30ppm, 40ppm, 50ppm, 60ppm, 70ppm, 80ppm, 85ppm, 90ppm, 95ppm. These values may be arbitrarily combined to form a numerical range. For example, the content of Na may be 20ppm to 95ppm, 20ppm to 85ppm, etc.
[0062] In some embodiments of the present invention, the content of Ca is less than 80ppm, preferably less than 50ppm. On the other hand, the content of Ca can be more than 10ppm. For example, the content of Ca can be 10ppm, 20ppm, 30ppm, 40ppm, 50ppm, 60ppm, 70ppm, 80ppm. These values can be arbitrarily combined to form a numerical range. For example, the content of Ca can be 10ppm to 80ppm, 10ppm to 50ppm, etc.
[0063] In some embodiments of the present invention, the content of Mg is less than 60ppm, preferably less than 40ppm, and more preferably less than 30ppm. On the other hand, the content of Mg may be greater than 5ppm. For example, the content of Mg may be 5ppm, 10ppm, 20ppm, 30ppm, 40ppm, 50ppm, 60ppm. These values may be arbitrarily combined to form a numerical range. For example, the content of Mg may be 5ppm to 60ppm, 5ppm to 40ppm, etc.
[0064] In some embodiments of the present invention, the content of Zn is 65ppm or less, preferably 45ppm or less, more preferably 40ppm or less. On the other hand, the content of Zn may be 10ppm or more. For example, the content of Zn may be 10ppm, 15ppm, 20ppm, 25ppm, 30ppm, 35ppm, 40ppm, 45ppm, 50ppm, 55ppm, 60ppm, 65ppm. These values may be arbitrarily combined to form a numerical range. For example, the content of Zn may be 10ppm to 65ppm, 10ppm to 40ppm, etc.
[0065] In some embodiments of the present invention, the content of Cu is less than 60ppm, preferably less than 40ppm. On the other hand, the content of Cu can be more than 15ppm. For example, the content of Cu can be 15ppm, 20ppm, 25ppm, 30ppm, 35ppm, 40ppm, 45ppm, 50ppm, 55ppm, 60ppm. These values can be arbitrarily combined to form a numerical range. For example, the content of Cu can be 15ppm to 60ppm, 15ppm to 50ppm, etc.
[0066] In some embodiments of the present invention, the content of Ti is 90ppm or less, preferably 86ppm or less. On the other hand, the content of Ti can be 30ppm or more. For example, the content of Ti can be 30ppm, 40ppm, 45ppm, 50ppm, 55ppm, 60ppm, 65ppm, 70ppm, 75ppm, 80ppm, 86ppm, 90ppm. These values can be arbitrarily combined to form a numerical range. For example, the content of Ti can be 30ppm to 90ppm, etc.
[0067] In other embodiments of the present invention, the iron oxide red powder also includes Mn having a content of less than 0.18 mass %, preferably less than 0.15 mass %. On the other hand, the content of Mn may be more than 10ppm. Specifically, the content of Mn may be 10ppm, 20ppm, 30ppm, 40ppm, 50ppm, 60ppm, 70ppm, 80ppm, 90ppm, 100ppm (i.e. 0.01 mass %), 0.05 mass %, 0.08 mass %, 0.1 mass %, 0.12 mass %, 0.15 mass %, 0.18 mass %. These values may be arbitrarily combined to form a numerical range. For example, the content of Mn may be 10ppm~0.18 mass %, 20ppm~0.15 mass %, etc.
[0068] In other embodiments of the present invention, the iron oxide red powder also includes Al in an amount of less than 0.1 mass %, preferably less than 0.08 mass %. On the other hand, the content of Al may be more than 30 ppm. Specifically, the content of Al may be 30 ppm, 40 ppm, 50 ppm, 60 ppm, 70 ppm, 80 ppm, 90 ppm, 100 ppm (i.e., 0.01 mass %), 0.03 mass %, 0.05 mass %, 0.07 mass %, 0.09 mass %, 0.1 mass %. These values may be arbitrarily combined to form a numerical range. For example, the content of Al may be 30 ppm to 0.1 mass %, 30 ppm to 0.07 mass %, etc.
[0069] In other embodiments of the present invention, the iron oxide red powder also includes Cl having a content of less than 0.1 mass %. On the other hand, the content of Cl may be more than 1ppm. Specifically, the content of Cl may be 1ppm, 5ppm, 10ppm, 30ppm, 50ppm, 80ppm, 100ppm (i.e. 0.01 mass %), 0.03 mass %, 0.05 mass %, 0.07 mass %, 0.09 mass %, 0.1 mass %. These values may be arbitrarily combined to form a numerical range. For example, the content of Cl may be 1ppm to 0.1 mass %, 1ppm to 0.09 mass %, etc.
[0070] [Second aspect]
[0071] The second aspect of the present invention relates to a method for preparing red iron oxide powder (or a method for purifying and spheroidizing red iron oxide).
[0072] The preparation method of the iron oxide red powder of the present invention comprises the following steps:
[0073] A suspension preparation step of mixing a dilute acid solution, a dispersant and red iron oxide powder to obtain a red iron oxide suspension;
[0074] The obtained suspension is ground to obtain a grinding slurry, and then demagnetized to obtain a demagnetized grinding slurry;
[0075] The step of filtering, washing and drying the demagnetized grinding slurry to obtain a crude iron oxide red product; and
[0076] The step of spheroidizing the crude red iron oxide is performed by pulverizing the crude red iron oxide to obtain a spherical red iron oxide powder as a product.
[0077] These steps are described in detail below.
[0078] Suspension preparation steps
[0079] In an embodiment of the present invention, the red iron oxide suspension is prepared by mixing a dilute acid solution, a dispersant and red iron oxide powder.
[0080] The dilute acid used for preparing the suspension can be one or more of sulfuric acid, nitric acid, formic acid, acetic acid, carbonic acid, oxalic acid, citric acid, malic acid, tartaric acid, succinic acid, benzoic acid, and salicylic acid. When using multiple of them, the ratio between them is not particularly limited and can be any ratio.
[0081] In some specific embodiments of the present invention, the concentration of the dilute acid solution used is 0.2-2.0 mass %, preferably 0.5-1.5 mass %. In the present invention, the dilute acid solution can be used directly, or it can be obtained by diluting concentrated acid with water. In addition, it should be noted that the acid used in the present invention can be an industrial acid.
[0082] In the present invention, the dispersant may be a nonionic surfactant. The nonionic surfactant includes one or more of polyoxyethylene ethers, polyols, polyol esters, and amides. When multiple of these are used, the ratio between them is not particularly limited and may be any ratio.
[0083] Examples of the polyoxyethylene ethers include alkylphenol polyoxyethylene ethers, fatty alcohol polyoxyethylene ethers, fatty acid polyoxyethylene ethers, and the like.
[0084] Among them, examples of alkylphenol polyoxyethylene ethers may include octylphenol polyoxyethylene ether and nonylphenol polyoxyethylene ether. Examples of octylphenol polyoxyethylene ethers may include OP-10. Examples of nonylphenol polyoxyethylene ethers may include NP-10, NP-30, NP-40, etc. Examples of fatty alcohol polyoxyethylene ethers may include AEO-9, AEO-15, AEO-30, etc. Examples of fatty acid polyoxyethylene ethers may include SG-40, SG-100, etc.
[0085] Examples of the polyols may include polyethylene glycol 200, polyethylene glycol 400, polyethylene glycol 600, polypropylene glycol, polybutylene glycol, and the like.
[0086] Examples of the polyol esters may include Tween 20, Tween 40, Tween 60, Tween 80, and the like.
[0087] Examples of the amide type may include stearic acid diethanolamide, coconut acid diethanolamide, coconut acid monoethanolamide, and the like.
[0088] In the present invention, there is no particular limitation on the iron oxide red powder, and the iron oxide red powder produced by a steel plant or a pigment plant can be directly used.
[0089] In some specific embodiments of the present invention, the proportion of the dispersant in the red iron oxide suspension is 0.2-2.0 mass%, preferably 0.5-1.5 mass%. The proportion of the red iron oxide powder in the red iron oxide suspension is 40-80 mass%, preferably 50-70 mass%.
[0090] It should be noted that, since the iron oxide suspension of the present invention is acidic, the mixing and dispersing container needs to be acid-resistant.
[0091] Grinding and demagnetization steps
[0092] After the iron oxide red suspension is obtained, the suspension is ground to obtain a grinding slurry, and then the grinding slurry is demagnetized to obtain a demagnetized grinding slurry. Through grinding and demagnetization (or magnetic separation), various impurities and magnetic impurities contained in the iron oxide powder can be removed.
[0093] In a specific embodiment of the present invention, the grinder used for grinding the suspension is not particularly limited, and a commonly used grinder can be used, examples of which may include a sand mill, a ball mill, and the like. For example, a vertical sand mill using zirconium oxide having a diameter of 0.5 to 2.5 mm can be used. Since the red iron oxide suspension of the present invention is acidic, the grinder needs to be acid-resistant.
[0094] There are no particular limitations on the grinding speed and grinding time. For example, the grinding speed may be 150 to 450 rpm, preferably 200 to 400 rpm. The grinding time may be 0.5 to 2 hours, preferably 0.8 to 1.2 hours.
[0095] In the present invention, there is no particular limitation on the magnetic separation or demagnetization equipment, as long as it can remove magnetic impurities. In some specific embodiments of the present invention, in order to simplify the operation, the grinding slurry is demagnetized by a pipeline demagnetizer during the process of sending the grinding slurry to the filtering device. There is no particular limitation on the magnetic field strength during the demagnetization process, for example, it can be about 12,000 gauss.
[0096] The above-mentioned steps of preparing suspension with acid and grinding for demagnetization are key steps for removing impurities. Of course, grinding also affects particle size and sphericity. If the iron oxide powder is soaked in acid to make a suspension but is not ground and dispersed, the impurities are wrapped in large particles and cannot be removed quickly. If it is only soaked and ground and dispersed with pure water, water-insoluble impurities such as aluminum, titanium, zinc, copper, etc. cannot be effectively removed.
[0097] Crude product preparation steps
[0098] In the embodiment of the present invention, after the demagnetizing polishing slurry is prepared, it is filtered, washed and dried to obtain a crude red iron oxide.
[0099] In a specific embodiment of the present invention, the filtration may be a filter press using a chamber filter press. The cleaning process may be multiple washings, for example, 2 to 5 times, each time using 40 to 60% of the dry weight of the iron oxide powder, and the total amount of water used may be 1 to 3 times the dry weight of the iron oxide powder, thereby obtaining an iron oxide red filter cake having a moisture content of 20 to 35% by mass.
[0100] In some specific embodiments of the present invention, in order to reduce impurities in red iron oxide and increase the iron oxide content, the water used in the cleaning process is pure water with a conductivity of 10 megohms.
[0101] In a specific embodiment of the present invention, the drying temperature of the iron oxide red filter cake is not particularly limited, and may be, for example, 120 to 220° C., preferably 180 to 220° C. The drying degree may be such that the moisture content of the filter cake is 0.8% by mass or less, preferably 0.5% by mass or less.
[0102] Spheronization steps
[0103] In the present invention, after the crude red iron oxide is prepared, it is pulverized to be sphericalized, thereby obtaining a spherical red iron oxide powder as a product.
[0104] In some specific embodiments of the present invention, the pulverizing step includes coarsely pulverizing the crude red iron oxide, and then finely pulverizing and spheroidizing the crude red iron oxide by using a jet mill. The pulverizer used in the coarse pulverizing step is not particularly limited, and a pulverizer commonly used in the art can be used, examples of which include a hammer mill, a turbine mill, a tooth mill, a knife mill, a pressure mill, a milling mill, and the like.
[0105] In the steps of fine crushing and spheroidization, the air flow mill used may be a disc type air flow mill, a circulating type air flow mill, a fluidized bed type air flow mill, or the like.
[0106] The above two steps of grinding and air flow milling both have an impact on the sphericalization of particle size. If only grinding is performed without air flow milling, the sphericalization degree of the particle surface is not high. On the other hand, if only air flow milling is performed without grinding, the particle size is too large and the uniformity of the particle size is poor.
[0107] Example
[0108] The embodiments of the present invention will be described in detail below in conjunction with examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If specific conditions are not specified in the examples, they are carried out under normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially. In the examples, unless otherwise specified, "%" refers to "mass %".
[0109] The testing method of the present invention is described below.
[0110] (1) Particle size distribution test
[0111] The particle size distribution test of the samples in the following examples of the present invention was carried out using a BT-9300S laser particle size distribution analyzer (manufactured by Dandong Better Instrument Co., Ltd.).
[0112] (2) Element content test
[0113] The element content test of the samples in the following embodiments of the present invention was carried out using an ICP7400 element analyzer (manufactured by Thermo Fisher Scientific (China) Co., Ltd.).
[0114] (3) Scanning electron microscope test
[0115] The morphology of the samples in the following examples of the present invention was measured using a S4700 scanning electron microscope (manufactured by Hitachi, Japan).
[0116] Example 1
[0117] The particle size test data of iron oxide red powder produced by a steel plant are: D10 = 1.147μm, D50 = 13.42μm, D97 = 41.11μm, and the volume average particle size is 14.73μm. Its specific surface area is 618.9m 2 / kg. For specific particle size distribution curve, see Figure 1A .
[0118] The test data of each element content in iron oxide red powder are as follows:
[0119] <![CDATA[Fe2O3,%]]> K Na Ca Mg Cu Mn Al Ti Zn Cl 98.5 29ppm 1081ppm 386ppm 85ppm 85ppm 2112ppm 276ppm 196ppm 87ppm 2450ppm
[0120] The iron oxide red product was prepared as follows.
[0121] 1) While slowly stirring, add 21 kg of 96% concentrated sulfuric acid to 3969 kg of pure water using an acid-resistant pump, add 10 kg of oxalic acid powder to dissolve, and after forming a 0.75% dilute acid solution, add 20 kg of polyoxyethylene ether nonionic surfactant OP-10, stir well, add 1 ton of the above-mentioned iron oxide red powder, and stir for 1 hour to form a slurry;
[0122] 2) The slurry was put into a vertical sand mill at a speed of 200 rpm for 1 hour;
[0123] 3) When the ground slurry is pumped to the filter press, the magnetic substances in the red iron oxide are adsorbed by the pipeline demagnetizer (QL-159050 and Foshan Qinli Magnetic and Electric Equipment Co., Ltd.);
[0124] 4) Using a filter press to filter the ground slurry, washing the filter material with 2 tons of 10 megohm pure water to obtain a red iron oxide filter cake with a water content of 27%;
[0125] 5) After drying the filter cake at 180° C. with a 30-meter-long belt dryer until the moisture content is less than 0.5%, the crude red iron oxide is crushed with a hammer mill (PC400x300, Zhengzhou Yangke Machinery Co., Ltd.), and then crushed with a disc airflow mill (STJ475, Yixing Qingxin Powder Machinery Co., Ltd.) to obtain a purified red iron oxide product with refined particles.
[0126] Particle size test data: D10 = 0.399 μm, D50 = 0.708 μm, D97 = 1.415 μm, the volume average particle size is 0.761 μm. Its specific surface area is 3463 m 2 / kg. For specific particle size distribution curve, see Figure 1B .
[0127] The test data of each element content of the purified red iron oxide product are as follows:
[0128] <![CDATA[Fe2O3,%]]> K Na Ca Mg Cu Mn Al Ti Zn Cl 99.30 4ppm 83ppm 41ppm 19ppm 25ppm 1369ppm 82ppm 48ppm 25ppm 852ppm
[0129] From the comparison of the above data, it can be seen that compared with the red iron oxide powder used as the raw material, the particle size of the red iron oxide product after purification is greatly reduced, the specific surface area is increased, the impurity content is greatly reduced, and the iron oxide content is increased.
[0130] In addition, from Figure 4B and Figure 4A It can be seen from the electron microscope photos shown that after being processed by the production process of increasing the iron oxide content in red iron oxide and sphericalizing the particles of the present invention, the particles of red iron oxide are more spherical, uniform and fine.
[0131] Example 2
[0132] The particle size test data of iron oxide red powder produced by a steel plant are: D10 = 1.077μm, D50 = 17.35μm, D97 = 55.49μm, and the volume average particle size is 19.90μm. Its specific surface area is 618.2m 2 / kg. For specific particle size distribution curve, see Figure 2A .
[0133] The test data of each element content in iron oxide red powder are as follows:
[0134] <![CDATA[Fe2O3,%]]> K Na Ca Mg Cu Mn Al Ti Zn Cl 98.06 21ppm 932ppm 338ppm 85ppm 64ppm 1930ppm 1233ppm 921ppm 94ppm 1720ppm
[0135] The iron oxide red product was prepared as follows.
[0136] 1) While slowly stirring, add 50 kg of 65% concentrated nitric acid to 3930 kg of pure water using an acid-resistant pump, add 20 kg of oxalic acid powder to dissolve, and after forming a 1.3% dilute acid solution, add 40 kg of polyol-type nonionic surfactant polyethylene glycol 600, stir well, add 1 ton of the above-mentioned iron oxide red powder, and stir for 1 hour to form a slurry;
[0137] 2) The slurry was put into a vertical sand mill at a speed of 300 rpm for 1 hour;
[0138] 3) When the ground slurry is pumped to the filter press, the magnetic substances in the red iron oxide are adsorbed by the pipeline demagnetizer;
[0139] 4) Using a filter press to filter the ground slurry, washing the filter material with 2 tons of 10 megohm pure water to obtain an iron oxide red filter cake with a water content of 29%;
[0140] 5) Dry the filter cake at 200° C. with a 30-meter-long belt dryer until the moisture content is less than 0.3%, crush the crude red iron oxide with a hammer mill, and then crush the crude red iron oxide with a disc-type airflow mill to obtain a purified red iron oxide product with fine particles.
[0141] Particle size test data: D10 = 0.315 μm, D50 = 0.677 μm, D97 = 1.307 μm, the volume average particle size is 0.703 μm. Its specific surface area is 3778 m 2 / kg. For specific particle size distribution curve, see Figure 2B .
[0142] The test data of each element content of the purified red iron oxide product are as follows:
[0143] <![CDATA[Fe2O3,%]]> K Na Ca Mg Cu Mn Al Ti Zn Cl 98.92 2ppm 41ppm 22ppm 11ppm 33ppm 823ppm 624ppm 57ppm 15ppm 676ppm
[0144] From the comparison of the above data, it can be seen that compared with the red iron oxide powder used as the raw material, the particle size of the red iron oxide product after purification is greatly reduced, the specific surface area is increased, the impurity content is greatly reduced, and the iron oxide content is increased.
[0145] Example 3
[0146] The particle size test data of iron oxide red powder produced by a pigment factory are: D10 = 0.276μm, D50 = 0.589μm, D97 = 1.048μm, and the volume average particle size is 0.579μm. Its specific surface area is 4633m 2 / kg. For specific particle size distribution curve, see Figure 3A .
[0147] The test data of each element content in iron oxide red powder are as follows:
[0148] <![CDATA[Fe2O3,%]]> K Na Ca Mg Cu Mn Al Ti Zn Cl 96.32 19ppm 432ppm 514ppm 218ppm 42ppm 31ppm 711ppm 1621ppm 652ppm 22ppm
[0149] The iron oxide red product was prepared as follows.
[0150] 1) While slowly stirring, add 21 kg of 96% concentrated sulfuric acid to 3969 kg of pure water using an acid-resistant pump, add 10 kg of 99.5% glacial acetic acid to form a 0.75% dilute acid solution, add 30 kg of alcohol ester nonionic surfactant Tween 40, stir well, add 1 ton of the above-mentioned iron oxide red powder, and stir for 1 hour to form a slurry;
[0151] 2) The slurry was put into a vertical sand mill at a speed of 400 rpm for 1 hour;
[0152] 3) When the ground slurry is pumped to the filter press, the magnetic substances in the red iron oxide are adsorbed by the pipeline demagnetizer;
[0153] 4) Using a filter press to filter the ground slurry, washing the filter material with 2 tons of 10 megohm pure water to obtain an iron oxide red filter cake with a water content of 34%;
[0154] 5) After drying the filter cake at 220° C. in a 30-meter-long belt dryer until the moisture content is less than 0.3%, the crude red iron oxide is crushed in a hammer mill, and then crushed in a disc-type airflow mill until D50 is 0.44 μm to obtain a purified red iron oxide product with refined particles.
[0155] Particle size test data: D10 = 0.225 μm, D50 = 0.319 μm, D97 = 0.865 μm, the volume average particle size is 0.418 μm. Its specific surface area is 6506 m 2 / kg. For specific particle size distribution curve, see Figure 3B .
[0156] The test data of each element content of the purified red iron oxide product are as follows:
[0157] <![CDATA[Fe2O3,%]]> K Na Ca Mg Cu Mn Al Ti Zn Cl 98.29 <1ppm 44ppm 33ppm 32ppm 23ppm 26ppm 59ppm 86ppm 38ppm 5ppm
[0158] From the comparison of the above data, it can be seen that the particle size of the purified red iron oxide product is smaller, the specific surface area is larger, the impurity content is greatly reduced, and the iron oxide content is increased compared with the red iron oxide powder used as the raw material.
[0159] Comparative Example 1
[0160] Except that only pure water was used to prepare the slurry without using acid, other conditions were the same as those in Example 1. The content of each element of the obtained red iron oxide product was detected as follows:
[0161] <![CDATA[Fe2O3,%]]> K Na Ca Mg Cu Mn Al Ti Zn Cl 98.6 13ppm 577ppm 214ppm 54ppm 82ppm 2036ppm 289ppm 185ppm 81ppm 1138ppm
[0162] It can be seen from the data in the table that the purity of iron oxide of this product is not improved much and the amount of impurities removed is very small.
[0163] Comparative Example 2
[0164] Except that only pure water was used to prepare the slurry without using acid, other conditions were the same as those in Example 2. The content of each element of the obtained red iron oxide product was detected as follows:
[0165] <![CDATA[Fe2O3,%]]> K Na Ca Mg Cu Mn Al Ti Zn Cl 98.11 6ppm 217ppm 275ppm 59ppm 62ppm 1948ppm 1193ppm 945ppm 88ppm 654ppm
[0166] It can be seen from the data in the table that the purity of iron oxide of this product is not improved much and the amount of impurities removed is very small.
[0167] Comparative Example 3
[0168] Except that only pure water was used to prepare the slurry without using acid, other conditions were the same as those in Example 3. The content of each element of the obtained red iron oxide product was detected as follows:
[0169] <![CDATA[Fe2O3,%]]> K Na Ca Mg Cu Mn Al Ti Zn Cl 96.19 8ppm 129ppm 378ppm 141ppm 44ppm 34ppm 697ppm 1643ppm 643ppm 12ppm
[0170] It can be seen from the data in the table that the iron oxide purity of this product not only did not increase, but also decreased, and the amount of impurities removed was very small.
[0171] Comparing Comparative Examples 1 to 3 with Examples 1 to 3, it can be seen that using only pure water without using acid cannot effectively remove impurities.
[0172] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
[0173] Industrial Applicability
[0174] Compared with the red iron oxide produced by existing steel mills or pigment factories, the invention has the advantages of higher purity, lower impurity content, smaller particle size, high sphericity and large specific surface area. In addition, the preparation method of the invention has simple process, low cost, low energy consumption and high output, and is suitable for industrial large-scale production.
Claims
1. A method for preparing red iron oxide powder, wherein the red iron oxide powder contains 98.0% by mass or more of Fe2O3 and contains K, Na, Ca, Mg, Zn, Cu and Ti each in an amount of 0.01% by mass or less, the red iron oxide having a substantially spherical shape and a median particle size D50 of 0.2 μm to 1.0 μm, The preparation method comprises the following steps: A suspension preparation step of mixing a dilute acid solution, a dispersant and red iron oxide powder to obtain a red iron oxide suspension; The obtained suspension is ground to obtain a grinding slurry, and then demagnetized to obtain a demagnetized grinding slurry; The step of filtering, washing and drying the demagnetized grinding slurry to obtain a crude iron oxide red product; and The crude red iron oxide product is crushed by a hammer mill and then crushed by a disc jet mill to obtain a spherical red iron oxide powder as a product. The dilute acid is sulfuric acid and oxalic acid, nitric acid and oxalic acid, or sulfuric acid and glacial acetic acid, and the dispersant is a nonionic surfactant. The concentration of the dilute acid solution is 0.2-2.0 mass %.
2. preparation method according to claim 1, wherein said nonionic surfactant comprises one or more in polyoxyethylene ether, polyols, polyol esters, amide type; said polyoxyethylene ether comprises one or more in alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ether; said polyols comprises one or more in Macrogol 200, Macrogol 400, Macrogol 600, polypropylene glycol, polybutylene glycol; said polyol esters comprises one or more in Tween 20, Tween 40, Tween 60, Tween 80; said amide type comprises one or more in stearic acid diethanolamide, coconut oil diethanolamide, coconut oil monoethanolamide.
3. The preparation method according to claim 1 or 2, wherein the proportion of the dispersant in the red iron oxide suspension is 0.2-2.0% by mass; and / or the proportion of the red iron oxide powder in the red iron oxide suspension is 40-80% by mass.
4. The preparation method according to claim 1 or 2, wherein the demagnetization is performed by passing the grinding slurry through a pipeline demagnetizer during the process of sending the grinding slurry to the filtering device; and / or, the cleaning is performed by using pure water with a conductivity of 10 megohms.