A method for preparing a dispersant for high-concentration coal-water slurry
High-concentration water-coal slurry dispersant prepared by vinyl polyethylene glycol ether VPEG and other materials solves the problem of poor fluidity of water-coal slurry dispersant at high concentrations, and achieves the improvement of water-coal slurry concentration and fluidity, reducing costs The effect is cost-effective and environmentally friendly.
Patent Information
- Application Number
- CN202310982490.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-08-07
AI Technical Summary
The apparent viscosity of existing water-coal slurry dispersants increases significantly at high concentrations, and their fluidity becomes worse, which affects pumping, atomization and combustion performance. The cost of low-concentration dispersants is high, so they cannot effectively improve the performance of water-coal slurry to offset the cost. The issue of increased pulping costs.
High-concentration water-coal slurry dispersant prepared with vinyl polyethylene glycol ether VPEG and other materials, through specific formula and process steps, including configuring B and C solutions, dropping and adjusting pH values, to prepare a molecular weight of 29527~68141. The dispersant with an effective content of 78.25% to 95.87% is used to improve the fluidity and concentration of water and coal slurry.
It has achieved the significant increase in the concentration of water and coal slurry while maintaining good fluidity and apparent viscosity, improved gasification efficiency, reduced pulping costs, and has high cost performance and green environmental protection characteristics.
Smart Images

Figure QLYQS_1 
Figure BDA0004379794120000051 
Figure BDA0004379794120000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coal water slurry dispersants, in particular to a method for preparing a dispersant for high-concentration coal water slurry. Background Art
[0002] As a raw material or fuel, water-coal slurry is mainly used in gasifiers and boilers. Moreover, with the rapid development of coal chemical technologies such as coal-to-methanol, coal-to-olefins and coal-to-ethylene glycol, the market size of water-coal slurry used as a raw material for gasifiers is growing.
[0003] Coal-water slurry as a substitute for oil has the advantages of low cost and low NO x The advantages of emission are particularly favored by the boiler market. Whether used as a gasification raw material or a boiler fuel, water-coal slurry needs to have good fluidity and stability, and be easy to pump and atomize. The main factors affecting the above-mentioned properties are coal quality, particle size distribution and chemical additives. Chemical additives mainly include dispersants and stabilizers, among which dispersants are the most critical and important. This is because water-coal slurry dispersants generally have hydrophilic and hydrophobic groups. The hydrophobic groups on their molecular chains are combined with the surface of coal particles, and the hydrophilic groups are facing the water, making the coal easier to wet, thereby reducing the viscosity of the slurry and improving the fluidity of the slurry; and the dispersant can form a hydration film on the surface of the coal. Under the action of electrostatic repulsion or steric hindrance, the coal particles are better dispersed in the water, and coal powders cannot form agglomerations. Therefore, dispersants play an important role in the preparation of high-performance water-coal slurry, especially in recent years, a large number of low-rank coals with poor slurry properties, mainly lignite, non-sticky coal and long flame coal, have been used to prepare water-coal slurry.
[0004] Therefore, dispersants are required to have better viscosity reduction and stability for slurry. Although new dispersants are constantly emerging, few are actually used in industry. This is mainly due to the fact that as the concentration of water-coal slurry increases, its apparent viscosity increases significantly, and its fluidity deteriorates, which is not conducive to pumping, atomization and combustion. In addition, due to the generally high cost of new dispersants for low-concentration water-coal slurry, the benefits brought by the improved performance of water-coal slurry cannot offset the increase in pulping cost caused by the use of new dispersants. Summary of the invention
[0005] A main purpose of the present invention is to solve the problems and difficulties raised in the background technology, and provide a method for preparing a dispersant for high-concentration coal water slurry, comprising the following steps:
[0006] Step 1): prepare solution B, 50-300 parts by weight of butyl acrylate, 50-300 parts by weight of glycerophosphate, 100-500 parts by weight of acrylic acid, and 400 parts by weight of deionized water, and stir evenly;
[0007] Step 2): prepare solution C, 10-30 parts by weight of mercaptopropionic acid, 4-10 parts by weight of L-ascorbic acid, and 1000 parts by weight of deionized water, and stir evenly;
[0008] Step 3): Weigh 3300 parts by weight of vinyl polyethylene glycol ether VPEG with a molecular weight of 600 to 1600 and place it in a four-necked flask A;
[0009] Step 4): Add 2000 to 3000 parts by weight of deionized water into the four-necked flask A as bottom kettle water and stir evenly;
[0010] Step 5): Add 10 to 100 parts by weight of sodium methyl allyl sulfonate into a four-necked flask A and stir evenly;
[0011] Step 6): Add 20 to 60 parts of sodium hypophosphite into the four-necked flask A and stir evenly;
[0012] Step 7): Add 20 to 50 parts by weight of hydrogen peroxide into a four-necked flask A, wherein the concentration of hydrogen peroxide is 27.5%, and stir evenly;
[0013] Step 8): Add 0 to 50 parts by weight of a ferrous sulfate solution into a four-necked flask A, wherein the concentration of the ferrous sulfate is 0.1‰, and stir evenly;
[0014] Step 9): Add the prepared solutions B and C to the four-necked flask A dropwise, with the addition time of solutions B and C being 20-70 min and 30-80 min, respectively.
[0015] Step 10): After the dropwise addition is completed, 10 to 100 parts by weight of sodium hydroxide is added to a four-necked flask, the pH is adjusted to 6.5 to 7.5, deionized water is added, the solid content is adjusted to 40%, and the mixture is stirred evenly to obtain a dispersant for high-concentration coal water slurry.
[0016] Preferably, in step 3), the effect is better when the molecular weight of the vinyl polyethylene glycol ether VPEG is 800-1200.
[0017] Preferably, in step 4), the effect is better when the water used in the bottom kettle is 2200-2800 parts by weight.
[0018] Preferably, in step 5), the effect is better when the amount of sodium methacrylate sulfonate is 30 to 50 parts by weight.
[0019] Preferably, in step 6), the effect is better when the amount of sodium hypophosphite is 10 to 50 parts by weight.
[0020] Preferably, in step 7), the effect is better when the amount of hydrogen peroxide is 35 to 35 parts by weight.
[0021] Preferably, in step 8), the effect is better when the amount of ferrous sulfate is 5 to 20 parts by weight.
[0022] Preferably, in step 1), the effect is better when the amounts of butyl acrylate, glycerophosphate and acrylic acid are 100-200 parts by weight, 150-300 parts by weight and 300-400 parts by weight respectively.
[0023] Preferably, in step 2), the effect is better when the amounts of mercaptopropionic acid and L-ascorbic acid are 15-25 parts by weight and 5-8 parts by weight respectively.
[0024] Preferably, in step 9), the effect is better when the B solution is added dropwise for 40 to 50 minutes, and the effect is better when the C solution is added dropwise for 50 to 60 minutes.
[0025] Preferably, the conductivity of the deionized water is 2 to 20 μS / cm;
[0026] The different coal water slurry dispersants prepared were subjected to GPC test, and the corresponding coal water slurry dispersants were used to prepare coal water slurry, and the fluidity, concentration, apparent viscosity, etc. of the coal water slurry were tested.
[0027] The water-coal slurry dispersant provided by the present invention has a molecular weight of 29527-68141, an effective content of 78.25%-95.87%, a distribution coefficient of 1.85-2.30, and the water-coal slurry prepared by using the dispersant has good fluidity and a water-coal slurry concentration of 63%-75%. It can maintain the water-coal slurry at room temperature and a shear rate of 100s -1 At the same time, the apparent viscosity is 1122-1191m Pa·s, and the concentration of water-coal slurry is effectively increased on the basis of traditional water-coal slurry dispersants, which can effectively improve the gasification efficiency of water-coal slurry, and has certain positive significance for energy conservation and emission reduction, cost reduction and efficiency improvement, and low-carbon environmental protection. The preparation method of the dispersant is simple and efficient, and has good operability.
[0028] The beneficial effects of the present invention are:
[0029] (1) The polycarboxylate water-reducing agent synthesized by using vinyl polyethylene glycol ether VPEG in the present invention has a richer side chain structure than the traditional naphthalene-type dispersant, and the side chain has a larger degree of freedom of swinging, which can better wrap the water-coal slurry particles and provide higher dispersibility. On this basis, the present invention screens the molecular weight of the vinyl polyethylene glycol ether VPEG used. Compared with the molecular weight of the vinyl polyethylene glycol ether VPEG3000 currently used in concrete, the dispersant prepared by the low molecular weight vinyl polyethylene glycol ether VPEG has a shorter side chain, which can effectively reduce the viscosity of the water-coal slurry while ensuring the dispersibility.
[0030] (2) The molecular weight of the dispersant prepared by the present invention is 29527-68141, the effective content is 78.25%-95.87%, and the distribution coefficient is 1.85-2.30. The preparation method is simple and easy to operate, green and environmentally friendly, and has high cost performance.
[0031] (3) The dispersant prepared in the present invention has good fluidity for water-coal slurry and can effectively reduce the apparent viscosity of water-coal slurry. -1 When the apparent viscosity is 1122-1191 mPa·s, the coal water slurry concentration is 65%-75%, which can effectively increase the working concentration of coal water slurry compared with the traditional naphthalene-type coal water slurry dispersant. DETAILED DESCRIPTION
[0032] The present invention will be further described below in conjunction with the embodiments.
[0033] A method for preparing a dispersant for high-concentration coal water slurry, characterized in that it comprises the following steps:
[0034] Step 1): prepare solution B, 50-300 parts by weight of butyl acrylate, 50-300 parts by weight of glycerophosphate, 100-500 parts by weight of acrylic acid, and 400 parts by weight of deionized water, and stir evenly;
[0035] Step 2): prepare solution C, 10-30 parts by weight of mercaptopropionic acid, 4-10 parts by weight of L-ascorbic acid, and 1000 parts by weight of deionized water, and stir evenly;
[0036] Step 3): Weigh 3300 parts by weight of vinyl polyethylene glycol ether VPEG with a molecular weight of 600 to 1600 and place it in a four-necked flask A;
[0037] Step 4): Add 2000 to 3000 parts by weight of deionized water into the four-necked flask A as bottom kettle water and stir evenly;
[0038] Step 5): Add 10 to 100 parts by weight of sodium methyl allyl sulfonate into a four-necked flask A and stir evenly;
[0039] Step 6): Add 20 to 60 parts of sodium hypophosphite into the four-necked flask A and stir evenly;
[0040] Step 7): Add 20 to 50 parts by weight of hydrogen peroxide into a four-necked flask A, wherein the concentration of hydrogen peroxide is 27.5%, and stir evenly;
[0041] Step 8): Add 0 to 50 parts by weight of a ferrous sulfate solution into a four-necked flask A, wherein the concentration of the ferrous sulfate is 0.1‰, and stir evenly;
[0042] Step 9): Add the prepared solutions B and C to the four-necked flask A dropwise, with the addition time of solutions B and C being 20-70 min and 30-80 min, respectively.
[0043] Step 10): After the dropwise addition is completed, 10 to 100 parts by weight of sodium hydroxide is added to a four-necked flask, the pH is adjusted to 6.5 to 7.5, deionized water is added, the solid content is adjusted to 40%, and the mixture is stirred evenly to obtain a dispersant for high-concentration coal water slurry.
[0044] The coal water slurry dispersant prepared in step 10 is subjected to GPC test, and the corresponding coal water slurry dispersant is used to prepare coal water slurry, and the fluidity, concentration, apparent viscosity, etc. of the coal water slurry are tested.
[0045] Examples 1 to 6
[0046] According to the method and steps of the present invention, different water-coal slurry dispersants are prepared according to the formula and operating parameters in Table 1.
[0047] Table 1
[0048]
[0049]
[0050] The performance of the coal water slurry dispersants with different properties prepared in the above Examples 1 to 6, the commercially available traditional naphthalene-type coal water slurry dispersant of Comparative Example 1, and the comparative example 2 without adding dispersant were tested. The results are shown in Table 2.
[0051] Table 2
[0052]
[0053] Examples 1 to 6 are different coal water slurry dispersants prepared by the present invention, comparative example 1 is a commercially available traditional naphthalene type coal water slurry dispersant, and comparative example 2 does not add a dispersant. The performance of the coal water slurry is shown in Table 2. As can be seen from Table 2, the molecular weight of the coal water slurry dispersant prepared by the present invention is 30780-49842, the effective content is 86.61%-95.87%, and the distribution coefficient is 1.85-2.30. The coal water slurry prepared by the present invention has good fluidity. When the apparent viscosity is 1122-1191m Pa·s, the working concentration of the coal water slurry is 66%-75%, which is significantly improved compared with comparative examples 1 and 2.
[0054] The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, all equivalent technical solutions also belong to the scope of the present invention. The patent protection scope of the present invention should be defined by the claims.
Claims
1. Use of a dispersant for preparing high-concentration coal-water slurry, It is characterized in that The preparation method of the dispersant comprises the following steps: Step 1): prepare solution B, 100 parts by weight of butyl acrylate, 150 parts by weight of glycerophosphate, 300 parts by weight of acrylic acid, and 400 parts by weight of deionized water, and stir evenly; Step 2): prepare solution C, 20 parts by weight of mercaptopropionic acid, 6 parts by weight of L-ascorbic acid, and 1000 parts by weight of deionized water, and stir evenly; Step 3): Weigh 3300 parts by weight of vinyl polyethylene glycol ether VPEG with a molecular weight of 1000 and place it in a four-necked flask A. The molecular formula of vinyl polyethylene glycol ether VPEG is: ; Step 4): Add 2600 parts by weight of deionized water into the four-necked flask A as bottom kettle water and stir evenly; Step 5): Add 40 parts by weight of sodium methyl allyl sulfonate into the four-necked flask A and stir evenly; Step 6): Add 30 parts by weight of sodium hypophosphite into the four-necked flask A and stir evenly; Step 7): Add 30 parts by weight of hydrogen peroxide into the four-necked flask A, wherein the concentration of hydrogen peroxide is 27.5%, and stir evenly; Step 8): Add 10 parts by weight of a ferrous sulfate solution into a four-necked flask A, wherein the concentration of the ferrous sulfate is 0.1‰, and stir evenly; Step 9): Add the prepared solutions B and C to the four-necked flask A dropwise, with the addition time of solutions B and C being 40 min and 50 min respectively; Step 10): After the dropwise addition is completed, 10 to 100 parts by weight of sodium hydroxide is added to a four-necked flask, the pH is adjusted to 6.5 to 7.5, deionized water is added, the solid content is adjusted to 40%, and the mixture is stirred evenly to obtain the dispersant, which is used to prepare a high-concentration coal water slurry.