Flame retardant and high temperature resistant release film and preparation method thereof
Silicone polyurethane is prepared by reacting a silicone oligomer with toluene-2,4-diisocyanate and connecting it to 9,10-dihydro-9-oxa-10-phosphine-10-oxa to prepare a silicone polyurethane ionization method The shaped film solves the flammability and adhesive coiling problems of polyurethane release film, and achieves the improvement of flame retardancy and high temperature resistance.
Patent Information
- Application Number
- CN202311419970.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-30
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-10-30
AI Technical Summary
The existing polyurethane release film is prone to combustion during use, has poor high temperature resistance, and solvent-based silicone release agents cause sticking and coiling, which cannot effectively prevent sticking and protect.
Silicone polyurethane is prepared by reacting silicone oligomer with toluene-2,4-diisocyanate, and 9,10-dihydro-9-oxa-10-phosphine-10-oxygen-10-oxygen under the action of a catalyst Miscellaneous, combining 1-allyl-1,1,3,3-tetramethyldisiloxane and chloroplatinic acid to form a silicone polyurethane release agent, which is made of flame retardant by coating, curing, washing and drying High temperature resistant polyurethane release film.
It improves the comprehensive performance of polyurethane release film, enhances its flame retardancy, high temperature resistance and anti-stickness, avoids sticking and curling, and broadens its application range.
Smart Images

Figure BDA0004520767440000031 
Figure BDA0004520767440000041 
Figure BDA0004520767440000042
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of release films, in particular to a flame retardant and high temperature resistant polyurethane release film and a preparation method thereof. Background Art
[0002] Release film is a film with anti-adhesion and protective effects. It is made by coating a release agent with a special molecular structure on the surface of a substrate. It is usually a low-adhesion-strength auxiliary coating used to protect pressure-sensitive adhesives. The reason why release film has low surface adhesion strength is that its special molecular structure has low surface free energy and critical surface tension, and it is difficult for pressure-sensitive adhesives, adhesive dirt and other substances with high surface energy to adhere to it. The application market of release film is mainly concentrated in the production fields of roll-type transparent adhesives, label-type pressure-sensitive adhesives, dry film photoresists, etc.
[0003] The common release agents on the market are mainly solvent-based silicone release agents. If the release film made of this type of release agent is left for a long time during use, different degrees of silicon transfer will occur, which is easy to cause sticking and rolling, and cannot achieve the desired anti-sticking and protective effects. Polyurethane release film is a release film material with high strength, high transparency and high wear resistance, but it is easy to burn and has poor high temperature resistance. The present invention proposes a flame retardant and high temperature resistant polyurethane release film and a preparation method thereof, which improves the comprehensive performance of the polyurethane release film and broadens the application range of the polyurethane release film. Summary of the invention
[0004] The object of the present invention is to provide a flame retardant and high temperature resistant polyurethane release film and a preparation method thereof, so as to solve the problems existing in the prior art.
[0005] A flame retardant and high temperature resistant polyurethane release agent, characterized in that the flame retardant and high temperature resistant polyurethane release film is prepared by reacting siloxane oligomers with toluene-2,4-diisocyanate to obtain silicone polyurethane, inserting 9,10-dihydro-9-oxa-10-phosphophanol-10-oxa into the side chain of silicone polyurethane under the action of a catalyst, and then mixing with 1-allyl-1,1,3,3-tetramethyldisiloxane, chloroplatinic acid and a diluent to obtain the silicone polyurethane release agent, and then coating, curing, washing and drying the release agent to obtain the release agent.
[0006] As an optimization, the siloxane oligomer is prepared by ring-opening polymerization of 1,3,5,7-tetramethylcyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane.
[0007] As an optimization, the catalyst is azobisisobutyronitrile.
[0008] As an optimization, the diluent is toluene.
[0009] As an optimization, the coating is to coat the silicone polyurethane release agent on the surface of the polytetrafluoroethylene flat plate.
[0010] As an optimization, a flame retardant and high temperature resistant polyurethane release film mainly includes the following preparation steps:
[0011] (1) Preparation of siloxane oligomers;
[0012] (2) Preparation of silicone polyurethane;
[0013] (3) Preparation of flame retardant and high temperature resistant polyurethane release film.
[0014] The preparation method for optimizing the flame retardant and high temperature resistant polyurethane release film mainly includes the following preparation steps:
[0015] (1) 1,3,5,7-tetramethylcyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane are added into a reactor in a molar ratio of 1:1-1.2, and then 0.02-0.03 times the mass of tetramethylammonium hydroxide and 0.01-0.02 times the mass of dimethyl sulfoxide are added. After stirring at 60-70°C and 500-1000 r / min for 10-20 minutes, 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane is added to terminate the reaction. The temperature is lowered to 40-50°C and stirring is continued for 10-12 minutes before stopping the reaction. After the system is cooled to room temperature, it is washed with a mixture of water and toluene, allowed to stand for stratification, and the washing is repeated 3-5 times. The organic phase is placed in a vacuum drying oven at 70-80°C for 4-5 hours to obtain a siloxane oligomer.
[0016] (2) adding siloxane oligomer, toluene-2,4-diisocyanate and dimethylformamide in a mass ratio of 1:4-5:20-30 into a reactor, stirring and reacting at 70-80° C. and 500-1000 r / min under a nitrogen atmosphere, adding siloxane oligomer of 5% by mass of toluene-2,4-diisocyanate to the reaction system every half an hour, and detecting the -NCO group concentration of the reaction system by dibutyl amine-hydrochloric acid titration method, stopping the addition of siloxane oligomer when the -NCO group concentration is less than 10%, and then adding anhydrous ethanol of 2 times the mass of toluene-2,4-diisocyanate to the reaction system to quench the remaining -NCO groups, cooling to room temperature, and drying in a vacuum drying oven at 70-80° C. for 4-5 hours to obtain silicone polyurethane;
[0017] (3) Azobisisobutyronitrile, 9,10-dihydro-9-oxa-10-phosphophanyl-10-oxa, silicone polyurethane, and dimethylformamide are added into a reactor in a mass ratio of 1 to 1.5:40 to 50:100:300 to 400, stirred at 70 to 80° C. and 500 to 1000 r / min for 5 to 6 hours, cooled to room temperature, and vacuum dried at 80 to 90° C. for 5 to 6 hours to obtain a modified silicone polyurethane, and then the modified silicone polyurethane, chloroplatinic acid, 1-allyl-1,1,3,3-tetramethyldisiloxane, and toluene are added in a mass ratio of 1 to 1.5:40 to 50:100:300 to 400. The amount ratio is 100:2-3:10-20:300-400, and the mixture is evenly mixed. The mixture is stirred at 500-1000 r / min for 10-12 min to obtain a silicone polyurethane release agent. The silicone polyurethane release agent is coated on the surface of a polytetrafluoroethylene flat plate with a coating thickness of 200-300 μm. The polyurethane release layer coated on the polytetrafluoroethylene flat plate is peeled off from the polytetrafluoroethylene flat plate, washed with deionized water for 3-5 times, and dried at 70-80°C for 3-4 h to obtain a flame retardant and high temperature resistant polyurethane release film.
[0018] As an optimization, the reaction process of 1,3,5,7-tetramethylcyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane in step (1) is:
[0019]
[0020] As an optimization, the reaction process of the siloxane oligomer and toluene-2,4-diisocyanate in step (2) is:
[0021]
[0022] As an optimization, the reaction process of 9,10-dihydro-9-oxa-10-phosphophanol-10-oxa and silicone polyurethane in step (3) is:
[0023]
[0024] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0025] When preparing a flame retardant and high temperature resistant polyurethane release film, the present invention comprises the following steps: reacting a siloxane oligomer with toluene-2,4-diisocyanate to obtain an organosilicon polyurethane; inserting 9,10-dihydro-9-oxa-10-phosphophanol-10-oxa into a side chain of the organosilicon polyurethane under the action of a catalyst; and then mixing the mixture with 1-allyl-1,1,3,3-tetramethyldisiloxane, chloroplatinic acid and a diluent to obtain an organosilicon polyurethane release agent; and then coating, curing, washing and drying the release agent to obtain the release film.
[0026] First, 1,3,5,7-tetramethylcyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane are ring-opening polymerized, and then end-capped with 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane. By controlling the reaction conditions, siloxane oligomers are obtained. The siloxane oligomers are reacted with toluene-2,4-diisocyanate to obtain a block copolymer of silicone and polyurethane. The -Si-O-Si- segment introduced into the polyurethane has high and low temperature resistance, low surface energy, low surface tension, weather resistance and air permeability, and is firmly combined together by chemical bonds.
[0027] Secondly, 9,10-dihydro-9-oxa-10-phosphophanol-10-oxa is connected to the side chain of the silicone polyurethane in the form of a chemical bond through an addition reaction under the action of azobisisobutyronitrile, which improves the problem of easy precipitation of the flame retardant in the matrix caused by the traditional addition method of the flame retardant; then it is evenly mixed with 1-allyl-1,1,3,3-tetramethyldisiloxane, catalyst chloroplatinic acid, and diluent toluene to obtain a silicone polyurethane release agent. In the previous step of reaction, part of the double bonds in the system are consumed, and the addition of 1-allyl-1,1,3,3-tetramethyldisiloxane supplements the double bonds in the system. When the release agent is cured, under the action of heating and catalyst, the double bonds and silicon-hydrogen bonds in the system form a cross-linked structure through an addition reaction, and then it is peeled off from the plate. After washing and drying, a flame-retardant and high-temperature resistant polyurethane release film can be obtained. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0029] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the flame retardant and high temperature resistant polyurethane release films prepared in the following examples are as follows:
[0030] Flame retardancy: The embodiments and comparative examples were prepared into standard specimens according to GB / T 2406.2-2009. The limiting oxygen index of the specimens was tested according to GB / T2406.2-2009. The standard specimens were immersed in pure water for 7 days, taken out, and dried at 70°C for 6 hours. The limiting oxygen index of the treated specimens was then tested according to GB / T 2406.2-2009, and the rate of change of the oxygen index before and after the specimen treatment was calculated.
[0031] High temperature resistance: Place the sample in a heat aging box at 10Pa and 200℃ for 36h, measure the mass and tensile strength of the sample before and after treatment, and calculate the mass change rate and tensile strength change rate of the sample before and after treatment.
[0032] Example 1
[0033] A method for preparing a flame retardant and high temperature resistant polyurethane release film, the method for preparing the flame retardant and high temperature resistant polyurethane release film mainly comprises the following preparation steps:
[0034] (1) 1,3,5,7-tetramethylcyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane are added to a reactor in a molar ratio of 1:1, and then 0.02 times the mass of tetramethylammonium hydroxide and 0.01 times the mass of dimethyl sulfoxide are added. After stirring at 60°C and 500 r / min for 20 minutes, 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane is added to terminate the reaction. The temperature is lowered to 40°C and stirring is continued for 12 minutes before stopping the reaction. After the system is cooled to room temperature, it is washed with a mixture of water and toluene, allowed to stand for stratification, and the washing is repeated 3 times. The organic phase is placed in a vacuum drying oven at 70°C and dried for 5 hours to obtain a siloxane oligomer.
[0035] (2) Adding siloxane oligomer, toluene-2,4-diisocyanate and dimethylformamide in a mass ratio of 1:4:20 into a reactor, stirring and reacting at 70°C and 500 r / min under a nitrogen atmosphere, adding siloxane oligomer of 5% by mass of toluene-2,4-diisocyanate to the reaction system every half an hour, and detecting the -NCO group concentration of the reaction system by dibutylamine-hydrochloric acid titration method, stopping the addition of siloxane oligomer when the -NCO group concentration is less than 10%, and then adding anhydrous ethanol of 2 times the mass of toluene-2,4-diisocyanate to the reaction system to quench the remaining -NCO groups, cooling to room temperature, and drying in a vacuum drying oven at 70°C for 5 hours to obtain silicone polyurethane;
[0036] (3) Azobisisobutyronitrile, 9,10-dihydro-9-oxa-10-phosphophanol-10-oxa, silicone polyurethane, and dimethylformamide were added into a reactor at a mass ratio of 1:40:100:300, stirred at 70°C and 500 r / min for 6 hours, cooled to room temperature, and vacuum dried at 80°C for 6 hours to obtain a modified silicone polyurethane. The modified silicone polyurethane, chloroplatinic acid, 1-allyl-1,1,3,3-tetramethyldisiloxane, Toluene was mixed evenly in a mass ratio of 100:2:10:300, stirred at 500r / min for 12min to obtain a silicone polyurethane release agent, which was coated on the surface of a polytetrafluoroethylene flat plate with a coating thickness of 200μm and cured at 70°C for 6h. The polyurethane release layer coated on the polytetrafluoroethylene flat plate was peeled off from the polytetrafluoroethylene flat plate, washed with deionized water for 3 times, and dried at 70°C for 4h to obtain a flame retardant and high temperature resistant polyurethane release film.
[0037] Example 2
[0038] A method for preparing a flame retardant and high temperature resistant polyurethane release film, the method for preparing the flame retardant and high temperature resistant polyurethane release film mainly comprises the following preparation steps:
[0039] (1) 1,3,5,7-tetramethylcyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane are added into a reactor in a molar ratio of 1:1.1, and then 0.025 times the mass of tetramethylammonium hydroxide and 0.015 times the mass of dimethyl sulfoxide are added. After stirring at 65°C and 750 r / min for 15 minutes, 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane is added to terminate the reaction. The temperature is lowered to 45°C and stirring is continued for 11 minutes before stopping the reaction. After the system is cooled to room temperature, it is washed with a mixture of water and toluene, allowed to stand for stratification, and the washing is repeated 4 times. The organic phase is placed in a vacuum drying oven at 75°C and dried for 4.5 hours to obtain a siloxane oligomer.
[0040] (2) Adding siloxane oligomer, toluene-2,4-diisocyanate and dimethylformamide in a mass ratio of 1:4:25 into a reactor, stirring and reacting at 75°C and 750 r / min under a nitrogen atmosphere, adding siloxane oligomer of 5% by mass of toluene-2,4-diisocyanate to the reaction system every half an hour, and detecting the -NCO group concentration of the reaction system by dibutyl amine-hydrochloric acid titration method, stopping the addition of siloxane oligomer when the -NCO group concentration is less than 10%, and then adding anhydrous ethanol of 2 times the mass of toluene-2,4-diisocyanate to the reaction system to quench the remaining -NCO groups, cooling to room temperature, and drying in a vacuum drying oven at 75°C for 4.5 hours to obtain silicone polyurethane;
[0041] (3) Azobisisobutyronitrile, 9,10-dihydro-9-oxa-10-phosphophanol-10-oxa, silicone polyurethane, and dimethylformamide were added into a reactor at a mass ratio of 1.2:45:100:350, stirred at 75°C and 750 r / min for 5 h, cooled to room temperature, and vacuum dried at 85°C for 5 h to obtain a modified silicone polyurethane. The modified silicone polyurethane, chloroplatinic acid, 1-allyl-1,1,3,3-tetramethyldisiloxane, and methylformamide were then added to the reactor. Benzene was mixed evenly in a mass ratio of 100:2.5:15:350, stirred at 750 r / min for 11 min to obtain a silicone polyurethane release agent, which was coated on the surface of a polytetrafluoroethylene flat plate with a coating thickness of 250 μm and cured at 75°C for 5 h. The polyurethane release layer coated on the polytetrafluoroethylene flat plate was peeled off from the polytetrafluoroethylene flat plate, washed 4 times with deionized water, and dried at 75°C for 3.5 h to obtain a flame retardant and high temperature resistant polyurethane release film.
[0042] Example 3
[0043] A method for preparing a flame retardant and high temperature resistant polyurethane release film, the method for preparing the flame retardant and high temperature resistant polyurethane release film mainly comprises the following preparation steps:
[0044] (1) 1,3,5,7-tetramethylcyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane are added into a reactor in a molar ratio of 1:1.2, and then 0.03 times the mass of tetramethylammonium hydroxide and 0.02 times the mass of dimethyl sulfoxide are added. After stirring at 70°C and 1000 r / min for 10 minutes, 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane is added to terminate the reaction. The temperature is lowered to 50°C and stirring is continued for 10 minutes before stopping the reaction. After the system is cooled to room temperature, it is washed with a mixture of water and toluene, allowed to stand for stratification, and the washing is repeated 5 times. The organic phase is placed in a vacuum drying oven at 80°C for 4 hours to obtain a siloxane oligomer.
[0045] (2) Adding siloxane oligomer, toluene-2,4-diisocyanate and dimethylformamide in a mass ratio of 1:5:30 into a reactor, stirring and reacting at 80°C and 1000 r / min under a nitrogen atmosphere, adding siloxane oligomer of 5% by mass of toluene-2,4-diisocyanate to the reaction system every half an hour, and detecting the -NCO group concentration of the reaction system by dibutyl amine-hydrochloric acid titration method, stopping the addition of siloxane oligomer when the -NCO group concentration is less than 10%, and then adding anhydrous ethanol of 2 times the mass of toluene-2,4-diisocyanate to the reaction system to quench the remaining -NCO groups, cooling to room temperature, and drying in a vacuum drying oven at 80°C for 5 hours to obtain silicone polyurethane;
[0046] (3) Azobisisobutyronitrile, 9,10-dihydro-9-oxa-10-phosphophanyl-10-oxa, silicone polyurethane, and dimethylformamide were added into a reactor at a mass ratio of 1.5:50:100:400, stirred at 80°C and 1000 r / min for 5 h, cooled to room temperature, and vacuum dried at 90°C for 5 h to obtain a modified silicone polyurethane. The modified silicone polyurethane, chloroplatinic acid, and 1-allyl-1,1,3,3-tetramethyldisiloxane were then added to the reactor. and toluene in a mass ratio of 100:3:20:400, stirred at 1000r / min for 10min to obtain a silicone polyurethane release agent, coated the silicone polyurethane release agent on the surface of a polytetrafluoroethylene flat plate with a coating thickness of 300μm, and cured at 80°C for 5h, peeled off the polyurethane release layer coated on the polytetrafluoroethylene flat plate, washed with deionized water for 5 times, and dried at 80°C for 3h to obtain a flame retardant and high temperature resistant polyurethane release film.
[0047] Comparative Example 1
[0048] A method for preparing a flame retardant and high temperature resistant polyurethane release film, the method for preparing the flame retardant and high temperature resistant polyurethane release film mainly comprises the following preparation steps:
[0049] (1) Add octamethylcyclotetrasiloxane to a reactor, then add tetramethylammonium hydroxide (0.025 times the mass of octamethylcyclotetrasiloxane) and dimethyl sulfoxide (0.015 times the mass of octamethylcyclotetrasiloxane), stir and react at 65°C and 750 r / min for 15 minutes, then add 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane to terminate the reaction, cool to 45°C and continue stirring for 11 minutes before stopping the reaction, wait until the system cools to room temperature, then wash with a mixture of water and toluene, stand and separate, repeat washing 4 times, take the organic phase, place it in a vacuum drying oven at 75°C and dry it for 4.5 hours to obtain a siloxane oligomer;
[0050] (2) Adding siloxane oligomer, toluene-2,4-diisocyanate and dimethylformamide in a mass ratio of 1:4:25 into a reactor, stirring and reacting at 75°C and 750 r / min under a nitrogen atmosphere, adding siloxane oligomer of 5% by mass of toluene-2,4-diisocyanate to the reaction system every half an hour, and detecting the -NCO group concentration of the reaction system by dibutyl amine-hydrochloric acid titration method, stopping the addition of siloxane oligomer when the -NCO group concentration is less than 10%, and then adding anhydrous ethanol of 2 times the mass of toluene-2,4-diisocyanate to the reaction system to quench the remaining -NCO groups, cooling to room temperature, and drying in a vacuum drying oven at 75°C for 4.5 hours to obtain silicone polyurethane;
[0051] (3) Azobisisobutyronitrile, 9,10-dihydro-9-oxa-10-phosphophanol-10-oxa, silicone polyurethane, and dimethylformamide were added into a reactor at a mass ratio of 1.2:45:100:350, stirred at 75°C and 750 r / min for 5 h, cooled to room temperature, and vacuum dried at 85°C for 5 h to obtain a modified silicone polyurethane. The modified silicone polyurethane, chloroplatinic acid, 1-allyl-1,1,3,3-tetramethyldisiloxane, and methylformamide were then added to the reactor. Benzene was mixed evenly in a mass ratio of 100:2.5:15:350, stirred at 750 r / min for 11 min to obtain a silicone polyurethane release agent, which was coated on the surface of a polytetrafluoroethylene flat plate with a coating thickness of 250 μm and cured at 75°C for 5 h. The polyurethane release layer coated on the polytetrafluoroethylene flat plate was peeled off from the polytetrafluoroethylene flat plate, washed 4 times with deionized water, and dried at 75°C for 3.5 h to obtain a flame retardant and high temperature resistant polyurethane release film.
[0052] Comparative Example 2
[0053] A method for preparing a flame retardant and high temperature resistant polyurethane release film, the method for preparing the flame retardant and high temperature resistant polyurethane release film mainly comprises the following preparation steps:
[0054] (1) 1,3,5,7-tetramethylcyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane are added into a reactor in a molar ratio of 1:1.1, and then 0.025 times the mass of tetramethylammonium hydroxide and 0.015 times the mass of dimethyl sulfoxide are added. After stirring at 65°C and 750 r / min for 15 minutes, 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane is added to terminate the reaction. The temperature is lowered to 45°C and stirring is continued for 11 minutes before stopping the reaction. After the system is cooled to room temperature, it is washed with a mixture of water and toluene, allowed to stand for stratification, and the washing is repeated 4 times. The organic phase is placed in a vacuum drying oven at 75°C and dried for 4.5 hours to obtain a siloxane oligomer.
[0055] (2) Adding siloxane oligomer, toluene-2,4-diisocyanate and dimethylformamide in a mass ratio of 1:4:25 into a reactor, stirring and reacting at 75°C and 750 r / min under a nitrogen atmosphere, adding siloxane oligomer of 5% by mass of toluene-2,4-diisocyanate to the reaction system every half an hour, and detecting the -NCO group concentration of the reaction system by dibutyl amine-hydrochloric acid titration method, stopping the addition of siloxane oligomer when the -NCO group concentration is less than 10%, and then adding anhydrous ethanol of 2 times the mass of toluene-2,4-diisocyanate to the reaction system to quench the remaining -NCO groups, cooling to room temperature, and drying in a vacuum drying oven at 75°C for 4.5 hours to obtain silicone polyurethane;
[0056] (3) Organic silicon polyurethane, chloroplatinic acid, 1-allyl-1,1,3,3-tetramethyldisiloxane and toluene were mixed evenly in a mass ratio of 100:2.5:15:350, and then 10-dihydro-9-oxa-10-phosphophanol-10-oxa in an amount of 0.02 times the mass of organic silicon polyurethane was added, and stirred at 750 r / min for 11 minutes to obtain an organic silicon polyurethane release agent. The organic silicon polyurethane release agent was coated on the surface of a polytetrafluoroethylene plate with a coating thickness of 250 μm, and cured at 75° C. for 5 hours. The polyurethane release layer coated on the polytetrafluoroethylene plate was peeled off from the polytetrafluoroethylene plate, washed with deionized water 4 times, and dried at 75° C. for 3.5 hours to obtain a flame retardant and high temperature resistant polyurethane release film.
[0057] Comparative Example 3
[0058] A method for preparing a flame retardant and high temperature resistant polyurethane release film, the method for preparing the flame retardant and high temperature resistant polyurethane release film mainly comprises the following preparation steps:
[0059] (1) The German Ken-Tian release agent PU-17092 was coated on the surface of a polytetrafluoroethylene flat plate with a coating thickness of 250 μm and cured at 75°C for 5 h. The polyurethane release layer coated on the polytetrafluoroethylene flat plate was peeled off from the polytetrafluoroethylene flat plate, washed with deionized water for 4 times, and dried at 75°C for 3.5 h to obtain a flame retardant and high temperature resistant polyurethane release film.
[0060] Effect example
[0061] Table 1 below shows the performance analysis results of the flame retardant and high temperature resistant polyurethane release films of Examples 1 to 3 of the present invention and Comparative Examples 1 to 3.
[0062] Table 1
[0063]
[0064]
[0065] It can be seen from the data in Table 1 that the oxygen index change rate of Examples 1, 2, and 3 is less than that of Comparative Examples 1 and 2, indicating that the flame retardant is grafted onto the silicone polyurethane copolymer segment in the form of a chemical bond through phosphorus-hydrogen addition, which can effectively reduce the precipitation of the flame retardant, and the flame retardant effect is better than the flame retardant effect of directly adding the flame retardant; the initial tensile strength of Examples 1, 2, 3 and Comparative Example 2 is greater than that of Comparative Example 1 and Comparative Example 3, indicating that the introduction of double bonds and hydrogen bonds for silicon hydrogen addition increases the cross-linking sites during curing, thereby improving the mechanical strength of the release film; the tensile strength change rate and mass change rate of Examples 1, 2, 3 and Comparative Examples 1 and 2 are both less than that of Comparative Example 3, indicating that the polysiloxane segment is introduced into the polyurethane segment through copolymerization to form a block copolymer, thereby improving the high temperature resistance of the polyurethane release film.
[0066] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a flame retardant and high temperature resistant polyurethane release film, characterized in that: The preparation method of the flame retardant and high temperature resistant polyurethane release film comprises the following preparation steps: (1) 1,3,5,7-tetramethylcyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane are added into a reactor in a molar ratio of 1:1-1.2, and then 0.02-0.03 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane of tetramethylammonium hydroxide and 0.01-0.02 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane of dimethyl sulfoxide are added. Stir the reaction at 60-70°C and 500-1000 r / min for 10-20 min, then add 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane to terminate the reaction. Cool the temperature to 40-50°C and continue stirring for 10-12 min before stopping the reaction. After the system cools to room temperature, wash it with a mixture of pure water and toluene, let it stand to separate, repeat the washing 3-5 times, take the organic phase and place it in a vacuum drying oven at 70-80°C to dry for 4-5 h to obtain a siloxane oligomer. (2) Add siloxane oligomer, toluene-2,4-diisocyanate and dimethylformamide in a mass ratio of 1:4~5:20~30 into a reactor, stir and react at 70~80°C and 500~1000r / min under a nitrogen atmosphere, add siloxane oligomer of 5% by mass of toluene-2,4-diisocyanate to the reaction system every half an hour, and detect the -NCO group concentration of the reaction system by dibutylamine-hydrochloric acid titration method. When the -NCO group concentration is less than 10%, stop adding siloxane oligomer, then add anhydrous ethanol of 2 times the mass of toluene-2,4-diisocyanate to the reaction system to quench the remaining -NCO groups, cool to room temperature, and dry in a vacuum drying oven at 70~80°C for 4~5h to obtain silicone polyurethane; (3) Azobisisobutyronitrile, 9,10-dihydro-9-oxa-10-phosphophanyl-10-oxa, silicone polyurethane, and dimethylformamide are added into a reactor in a mass ratio of 1-1.5:40-50:100:300-400, stirred at 70-80°C and 500-1000 r / min for 5-6 hours, cooled to room temperature, and vacuum dried at 80-90°C for 5-6 hours to obtain a modified silicone polyurethane. Then, the modified silicone polyurethane, chloroplatinic acid, 1-allyl-1,1,3,3-tetramethyldisiloxane, and toluene are added in a mass ratio of 1-1.5:40-50:100:300-400. The amount ratio is 100:2~3:10~20:300~400, and the mixture is evenly mixed, and stirred at 500~1000r / min for 10~12min to obtain a silicone polyurethane release agent, and the silicone polyurethane release agent is coated on the surface of the polytetrafluoroethylene flat plate, and the coating thickness is controlled to be 200~300μm, and cured at 70~80℃ for 5~6h, and the polyurethane release layer coated on the polytetrafluoroethylene flat plate is peeled off from the polytetrafluoroethylene flat plate, washed with deionized water for 3~5 times, and dried at 70~80℃ for 3~4h to obtain a flame-retardant and high-temperature resistant polyurethane release film; The reaction process of 1,3,5,7-tetramethylcyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane in step (1) is as follows: The reaction process of the siloxane oligomer and toluene-2,4-diisocyanate in step (2) is as follows: ; The reaction process of 9,10-dihydro-9-oxa-10-phosphophanol-10-oxa and silicone polyurethane in step (3) is as follows: 。 2. A flame retardant and high temperature resistant polyurethane release film prepared according to the method for preparing a flame retardant and high temperature resistant polyurethane release film according to claim 1.
Citation Information
Patent Citations
Silane modified polymer and preparation method thereof
CN107522864A
Preparation method of ultraviolet light polymerization fluorosilicone release film for optical display
CN108676189A
Organic silicon modified flame-retardant polyurethane and preparation
CN108864399A
Smooth and elastic organic silicon release agent
CN109385207A
Organo polysiloxane composition forming peelable cured film, sheet like substrate material having peelable cured film and method for producing the same
JP2007211186A