A method for preparing gelatin polyelectrolyte brushes via thermally initiated emulsion polymerization

The graft of 2-methacryloyloxyethylphosphate choline monomer in gelatin spherical polyelectrolyte brushes by heat-induced emulsion polymerization has solved the problem of insufficient biodegradability of traditional nanospherical polyelectrolyte brushes, and prepared good biological properties Compatible gelatin spherical polyelectrolyte brushes have expanded their application in the field of biomedical science.

CN117487094BActive Publication Date: 2024-11-19EAST CHINA UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311146995.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-07
Publication Date
2024-11-19
Estimated Expiration
2043-09-07

AI Technical Summary

Technical Problem

The application of traditional nanospherical polyelectrolyte brushes in the field of biomedical science is limited, because they are insufficient biodegradable and the materials used during the preparation process do not have good biocompatibility.

Method used

Using the heat-induced emulsion polymerization method, the reaction of methacrylic anhydride gelatin nanoparticles and 2-methacryloyloxyethylphosphate choline monomers through heat-induced reaction to form a gelatin spherical polyelectrolyte brush, realizing the connection of polyelectrolyte chains. The formation of branches and structures.

Benefits of technology

Preparation of gelatin spherical polyelectrolyte brushes with uniform particle size, controllable chain length and good biocompatibility solves the problem of insufficient biocompatibility of traditional materials and provides broad application prospects in the field of biomedical.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117487094B_ABST
    Figure CN117487094B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a gelatin polyelectrolyte brush by a thermally initiated emulsion polymerization method, wherein methacrylic anhydride-modified gelatin nanoparticles and a monomer 2-methacryloyloxyethyl phosphorylcholine (MPC) surface-modified with methacrylic anhydride are subjected to a thermally initiated emulsion polymerization reaction to prepare a gelatin spherical polyelectrolyte brush. Under the action of a thermal initiator, the MPC monomer is grafted on the surface of the gelatin sphere core to form an elongated molecular chain, and finally a structure similar to a "brush" is formed to obtain a gelatin spherical polyelectrolyte brush. The gelatin spherical polyelectrolyte brush prepared by the present invention has a regular morphology and uniform size, and the brush chain size can be regulated by the amount of the added monomer MPC, and has broad application prospects in the field of biomedicine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of functional polymer material preparation, and in particular to a method for preparing a gelatin polyelectrolyte brush by thermally initiated emulsion polymerization, and a gelatin polyelectrolyte brush prepared by the method. Background Art

[0002] Spherical Polyelectrolyte Brush (SPB) is a macromolecular assembly system formed by grafting high-density linear polyelectrolyte chains on the surface of a nanoscale spherical structure. Due to steric repulsion and electrostatic repulsion, the polyelectrolyte chains grafted on the surface of the nanosphere core will stretch outward to form a "brush"-like structure. This unique structure has opened up a new way to prepare controllable nanodevices, nano-metal composite particles, and nano-sized protein carriers. However, traditional materials for synthesizing SPB cores (such as polystyrene, polybutadiene, etc.) have potential problems in biodegradation, which limits the application of SPB in the biomedical field.

[0003] As a hydrolyzate of collagen, gelatin has good biocompatibility and degradability. Using gelatin as the core material can improve the biocompatibility of SPB. Poly(2-methacryloyloxyethyl phosphorylcholine) (PMPC) is a biocompatible amphoteric polyelectrolyte. Therefore, the nano-spherical polyelectrolyte brush obtained by grafting PMPC onto the surface of MA-modified gelatin nanoparticles can further expand its application in the biomedical field. Summary of the invention

[0004] The invention provides a method for preparing a gelatin spherical polyelectrolyte brush by a thermally initiated emulsion polymerization method, which can prepare a gelatin spherical polyelectrolyte brush with uniform particle size, controllable chain length, good biocompatibility and biodegradability.

[0005] To achieve the above object, the technical solution of the present invention is as follows:

[0006] The invention discloses a method for preparing gelatin polyelectrolyte brushes by thermally initiated emulsion polymerization. Methacrylic anhydride gelatin nanoparticles surface-modified with methacrylic anhydride (MA) and monomer 2-methacryloyloxyethyl phosphorylcholine (MPC) are subjected to thermally initiated emulsion polymerization to prepare gelatin spherical polyelectrolyte brushes.

[0007] Under the action of thermal initiator, MPC monomer will be grafted on the surface of gelatin spherical core to form a slender molecular chain, and finally form a "brush"-like structure to obtain gelatin spherical polyelectrolyte brush.

[0008] It is further preferred that the thermal initiator used in the polymerization reaction is selected from potassium persulfate (KPS), ammonium persulfate or azobisisobutyronitrile (AIBN).

[0009] It is further preferred that the polymerization reaction temperature is 50-95°C.

[0010] The present invention is further preferably that, in the polymerization reaction, the mass ratio of the MPC monomer to the methacrylic anhydride-treated gelatin nanoparticles is (1-15):1.

[0011] It is further preferred that the chain length of the prepared gelatin spherical polyelectrolyte brush is 10 to 200 nm.

[0012] The present invention is further preferably that the method for preparing the gelatin spherical polyelectrolyte brush specifically comprises the following steps:

[0013] S1: Using gelatin as raw material, gelatin self-assembles to form gelatin nanoparticles (Gel-NPs) by adding a cross-linking agent;

[0014] S2: using methacrylic anhydride to modify the surface of the prepared gelatin nanoparticles to prepare methacrylated gelatin nanoparticles (Gel-MA);

[0015] S3: preparing gelatin spherical polyelectrolyte brushes (Gel-NPs-PMPC) by thermally initiating emulsion polymerization of the methacrylated gelatin nanoparticles and monomer 2-methacryloyloxyethyl phosphorylcholine (MPC).

[0016] The present invention is further preferably that in step S1, the preparation of the gelatin nanoparticles comprises the following steps:

[0017] (1) Mix gelatin and deionized water, stir to dissolve, add concentrated hydrochloric acid, and adjust the pH value of the system to 1-3;

[0018] (2) adding excess acetone to the above reaction system until the turbidity of the reaction system increases significantly, so that the long chains of gelatin molecules curl up to form self-assembled nanoparticles;

[0019] (3) adding a cross-linking agent glutaraldehyde solution to cross-link and solidify the gelatin particles;

[0020] (4) adding guanidine hydrochloride solution to neutralize the residual glutaraldehyde in the reaction system, terminate the cross-linking reaction, and centrifuge, purify, and freeze-dry the solution to obtain the self-assembled gelatin nanoparticles.

[0021] The present invention is further preferably that in step S2, the preparation of the methacrylated gelatin nanoparticles comprises the following steps:

[0022] (1) mixing and stirring the gelatin nanoparticles and the carbonic acid-sodium bicarbonate buffer to dissolve, and adjusting the pH to 8-10;

[0023] (2) adding a certain amount of methacrylic anhydride and reacting at 50-55° C. in the dark;

[0024] (3) After the reaction is completed in a dark environment, the product is dialyzed in hot water for purification, and the molecular weight cut-off of the dialysis bag is 8-14 KDa;

[0025] (4) freeze-drying the purified solution to obtain the desired methacrylated gelatin nanoparticles.

[0026] The present invention is further preferably that in step S3, the preparation of the gelatin spherical polyelectrolyte brush comprises the following steps:

[0027] (1) mixing a certain amount of methacrylated gelatin nanoparticles and a thermal initiator, pumping nitrogen, dissolving 2-methacryloyloxyethyl phosphorylcholine monomer in deionized water, and injecting the mixture into the mixture of the gelatin nanoparticles and the thermal initiator; and mixing and stirring the reaction system at 50 to 95° C. to perform a polymerization reaction;

[0028] (2) The reaction product of step (1) is then dialyzed and purified in deionized water using an 8-14 KDa dialysis bag to obtain the gelatin spherical polyelectrolyte brush.

[0029] The monomer 2-methacryloyloxyethyl phosphorylcholine has the following structure:

[0030]

[0031] The present invention is further preferably that the method for preparing the gelatin spherical polyelectrolyte brush comprises the following steps:

[0032] S1: Add gelatin and deionized water into a three-necked flask, stir and dissolve at 35-45°C; then add concentrated hydrochloric acid dropwise to adjust the pH value of the system to 1-3;

[0033] S2: Add excess acetone until the turbidity of the reaction system increases significantly, causing the long chains of gelatin molecules to curl up to form self-assembled nanoparticles;

[0034] S3: adding cross-linking agent glutaraldehyde to cross-link and solidify the gelatin particles;

[0035] S4: After the cross-linking reaction is completed, a guanidine hydrochloride solution is added to neutralize the residual glutaraldehyde in the system to terminate the cross-linking reaction, and the solution is centrifuged, purified, and freeze-dried to obtain gelatin nanoparticles (Gel-NPs);

[0036] S5: Mix gelatin nanoparticles, CB buffer and additional deionized water in a flask to make the gelatin nanoparticle concentration reach 1-3wt%, stir well at 50-55°C, and adjust pH to 8-10;

[0037] S6: adding methacrylic anhydride, reacting for 1 hour under magnetic stirring at 500-700 rpm; after the reaction, dialysis and purification were performed in deionized water using an 8-14 KDa dialysis bag to obtain methacrylated gelatin nanoparticles (Gel-MA);

[0038] S7: Mix Gel-MA and potassium persulfate, dissolve MPC monomer in deionized water after pumping nitrogen, and inject into the flask;

[0039] S8: After reacting for 24 h at 50-95°C and 800 rpm magnetic stirring, the mixture was dialyzed and purified in deionized water using an 8-14 KDa dialysis bag to obtain a gelatin spherical polyelectrolyte brush;

[0040] The raw materials are in the following weight parts: 4-6 parts of gelatin; 0.5-1 parts of concentrated hydrochloric acid; 240-300 parts of acetone; 1-2 parts of glutaraldehyde; 70-80 parts of guanidine hydrochloride; 1-3 parts of 2-methacryloyloxyethyl phosphorylcholine (MPC); 4-10 parts of methacrylic anhydride; 50-60 parts of sodium carbonate-sodium bicarbonate (CB) buffer; 1-2 parts of potassium persulfate; and 90-120 parts of deionized water.

[0041] The present invention also provides a gelatin spherical polyelectrolyte brush prepared by any one of the above methods for preparing a gelatin polyelectrolyte brush.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] (1) The present invention adopts a thermally initiated emulsion polymerization method, which only requires simple heating to achieve the reaction, has low raw material cost, and is simple to prepare. Potassium persulfate dissolved in the aqueous phase decomposes at high temperature to generate free radicals. As the chain of free radical polymerization grows, linear PMPC chains are gradually generated on the surface of MA-modified gelatin nanoparticles to form stable gelatin spherical polyelectrolyte brushes.

[0044] (2) The present invention successfully synthesized a new type of gelatin spherical polyelectrolyte brush by thermally initiated emulsion polymerization. The material has a controllable polyelectrolyte chain length, and no toxic substances that are difficult to remove are introduced during the preparation process. It has good biocompatibility, which makes it have broad application prospects in biomedical applications.

[0045] (3) In the technical scheme of the present invention, methacrylic anhydride is used as a surface modification agent for gelatin nanoparticles, and a thermally initiated emulsion polymerization method is used to prepare gelatin spherical polyelectrolyte brushes. The method has good repeatability, low raw material cost, regular product morphology, and uniform particle size. It is an important way to industrially mass-produce gelatin spherical polyelectrolyte brushes in the future. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 The figure is a flow chart of the preparation of the gelatin spherical polyelectrolyte brush described in the present invention.

[0047] Figure 2 The particle size distribution diagram of gelatin spherical polyelectrolyte brushes with different chain lengths prepared in the embodiments of the present invention.

[0048] Figure 3 The infrared spectra of the gelatin spherical polyelectrolyte brush, PMPC, MA-modified gelatin nanoparticles, and cross-linked gelatin nanoparticles prepared by the preparation method of the present invention are shown. DETAILED DESCRIPTION

[0049] The present invention is further described below by way of examples. The following examples are only used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0050] All raw materials in the present invention can be directly purchased. In the embodiments of the present invention, dynamic light scattering, TEM electron microscope and infrared spectrum are used to characterize the products in the preparation process.

[0051] The chain length of the spherical polyelectrolyte brush in the present invention = (D (Gel-NPs-PMPC) -D (Gel-NPs) ) / 2.

[0052] Example 1

[0053] like Figure 1 As shown in FIG. 1 , in this embodiment, gelatin nanoparticles and methacrylated gelatin nanoparticles are prepared in sequence using gelatin as a raw material, and finally gelatin spherical polyelectrolyte brushes are prepared by thermally initiated emulsion polymerization. In the preparation process, TEM electron microscopy and infrared spectroscopy are used to observe and characterize the morphology of the products in the preparation process. The characterization results are shown in FIG. Figure 2 and 3 shown.

[0054] The preparation of the gelatin spherical polyelectrolyte brush specifically includes the following process:

[0055] Weigh 5g gelatin and 60mL deionized water into a three-necked flask and stir to dissolve at 40℃. Use concentrated hydrochloric acid to adjust the pH value of the reaction system to 1-3, then add excess acetone to greatly increase the turbidity of the reaction system; then add 600μL glutaraldehyde solution and cross-link overnight. After the cross-linking reaction is completed, add 100mL of 100mM guanidine hydrochloride aqueous solution, stir to react for 1-2h, centrifuge and purify, and freeze-dry to obtain gelatin nanoparticles (Gel-NPs) with a particle size of 230nm. Weigh 1g Gel-NPs and dissolve in 100mL of 1M carbonate-sodium bicarbonate buffer, and adjust the pH to about 9, then add 1-1.5mL methacrylic anhydride, react at 50-55℃ in the dark for 1h, and then dialysis and purification in hot water. The molecular weight cutoff of the dialysis bag is 8-14KDa. After freeze-drying, methacrylated gelatin nanoparticles (Gel-MA) can be obtained.

[0056] Weigh 0.1g of the prepared Gel-MA and 3mg of KPS and dissolve them in 100mL of deionized water. After pumping nitrogen for 5 times, place in a 75℃ oil bath and stir to mix. Use a syringe to add 1mL of 0.1g / mL MPC aqueous solution to react for 24h. After dialysis purification, freeze-drying can obtain Gel-NPs-PMPC. The molecular weight cutoff of the dialysis bag is 8-14Kda. The particle size of the prepared Gel-NPs-PMPC is 330nm. Therefore, the chain length of the obtained spherical polyelectrolyte brush is 50nm. Figure 2 and Figure 3 As shown, in this embodiment, TEM electron microscopy and infrared spectroscopy are used to characterize the products in the preparation process.

[0057] Example 2

[0058] The difference from Example 1 is that the thermal initiator selected is ammonium persulfate, and the process of the thermal polymerization reaction is as follows: weigh 0.1 g of the prepared Gel-MA and 3 mg of ammonium persulfate and dissolve them in 100 mL of deionized water. After pumping nitrogen for 5 times, place them in a 75°C oil bath and stir to mix. Use a syringe to add 1 mL of a 0.1 g / mL MPC aqueous solution. After reacting for 24 hours, dialyze and purify, and then freeze-dry to obtain Gel-NPs-PMPC. The chain length of the obtained spherical polyelectrolyte brush is 20 nm.

[0059] Example 3

[0060] The difference from Example 1 is that the thermal initiator selected is azobisisobutyronitrile (AIBN), and the process of the thermal polymerization reaction is as follows: 0.1 g of the prepared Gel-MA and 3 mg of AIBN are weighed and dissolved in 100 mL of deionized water. After nitrogen is pumped in and filled for 5 times, the mixture is placed in a 75°C oil bath and stirred to mix. 1 mL of a 0.1 g / mL MPC aqueous solution is added with a syringe. After reacting for 24 hours, Gel-NPs-PMPC is obtained by dialysis purification and freeze-drying. The chain length of the obtained spherical polyelectrolyte brush is 20 nm.

[0061] Example 4

[0062] The difference from Example 1 is that the reaction temperature of the thermal polymerization reaction is different. The process of the thermal polymerization reaction is as follows: 0.1 g of Gel-MA and 3 mg of KPS are weighed and dissolved in 100 mL of deionized water, and after nitrogen is pumped and filled for 5 times, the mixture is placed in a 50°C oil bath and stirred to mix, and 1 mL of a 0.1 g / mL MPC aqueous solution is added with a syringe, and after reacting for 24 hours, Gel-NPs-PMPC is obtained by dialysis purification and freeze-drying, and the chain length of the obtained spherical polyelectrolyte brush is 10 nm.

[0063] Example 5

[0064] The difference from Example 1 is that the reaction temperature of the thermal polymerization reaction is different. The process of the thermal polymerization reaction is as follows: 0.1 g of Gel-MA and 3 mg of KPS are weighed and dissolved in 100 mL of deionized water, and after pumping nitrogen for 5 times, the mixture is placed in a 70°C oil bath and stirred to mix, and 1 mL of a 0.1 g / mL MPC aqueous solution is added with a syringe, and after reacting for 24 hours, Gel-NPs-PMPC is obtained by dialysis purification and freeze-drying, and the chain length of the obtained spherical polyelectrolyte brush is 50 nm.

[0065] Example 6

[0066] The difference from Example 1 is that the reaction temperature of the thermal polymerization reaction is different. The process of the thermal polymerization reaction is as follows: 0.1 g of Gel-MA and 3 mg of KPS are weighed and dissolved in 100 mL of deionized water, and after pumping nitrogen for 5 times, the mixture is placed in an 80°C oil bath and stirred to mix, and 1 mL of a 0.1 g / mL MPC aqueous solution is added with a syringe, and after reacting for 24 hours, Gel-NPs-PMPC is obtained by dialysis purification and freeze-drying, and the chain length of the obtained spherical polyelectrolyte brush is 50 nm.

[0067] Example 7

[0068] The difference from Example 1 is that the reaction temperature of the thermal polymerization reaction is different. The process of the thermal polymerization reaction is as follows: 0.1 g of Gel-MA and 3 mg of KPS are weighed and dissolved in 100 mL of deionized water, and after pumping nitrogen for 5 times, the mixture is placed in an 85°C oil bath and stirred to mix, and 1 mL of a 0.1 g / mL MPC aqueous solution is added with a syringe, and after reacting for 24 hours, Gel-NPs-PMPC is obtained by dialysis purification and freeze-drying, and the chain length of the obtained spherical polyelectrolyte brush is 40 nm.

[0069] Example 8

[0070] The difference from Example 1 is that the reaction temperature of the thermal polymerization reaction is different. The process of the thermal polymerization reaction is as follows: 0.1 g of Gel-MA and 3 mg of KPS are weighed and dissolved in 100 mL of deionized water, and after pumping nitrogen for 5 times, the mixture is placed in a 95°C oil bath and stirred to mix, and 1 mL of a 0.1 g / mL MPC aqueous solution is added with a syringe, and after reacting for 24 hours, Gel-NPs-PMPC is obtained by dialysis purification and freeze-drying, and the chain length of the obtained spherical polyelectrolyte brush is 40 nm.

[0071] Example 9

[0072] The difference from Example 1 is that the amount of MPC monomer added is different. The process of thermal polymerization reaction is as follows: 0.1 g Gel-MA and 3 mg KPS are weighed and dissolved in 100 mL deionized water, and after pumping nitrogen for 5 times, placed in a 75°C oil bath pot and stirred to mix, 1 mL of 0.05 g / mL MPC aqueous solution is added with a syringe, and after reacting for 24 hours, Gel-NPs-PMPC is obtained after purification by dialysis and freeze-drying, and the chain length of the obtained spherical polyelectrolyte brush is 10 nm.

[0073] Example 10

[0074] The difference from Example 1 is that the amount of MPC monomer added is different. The process of thermal polymerization reaction is as follows: 0.1 g Gel-MA and 3 mg KPS are weighed and dissolved in 100 mL deionized water, and after nitrogen is pumped and filled for 5 times, the mixture is placed in a 75°C oil bath and stirred and mixed, and 1 mL of 0.5 g / mL MPC aqueous solution is added with a syringe, and after reacting for 24 hours, Gel-NPs-PMPC is obtained by dialysis purification and freeze-drying, and the chain length of the obtained spherical polyelectrolyte brush is 100 nm.

[0075] Embodiment 11

[0076] The difference from Example 1 is that the amount of MPC monomer added is different. The process of thermal polymerization reaction is as follows: 0.1 g Gel-MA and 3 mg KPS are weighed and dissolved in 100 mL deionized water, and after pumping nitrogen for 5 times, placed in a 75°C oil bath and stirred to mix, 1 mL of 1 g / mL MPC aqueous solution is added with a syringe, and after reacting for 24 hours, Gel-NPs-PMPC is obtained by dialysis purification and freeze-drying, and the chain length of the obtained spherical polyelectrolyte brush is 200 nm.

[0077] Example 12

[0078] The difference from Example 1 is that the amount of MPC monomer added is different. The process of thermal polymerization reaction is as follows: 0.1 g Gel-MA and 3 mg KPS are weighed and dissolved in 100 mL deionized water, and after nitrogen is pumped and filled for 5 times, the mixture is placed in a 75°C oil bath and stirred to mix, and 1 mL of 1.5 g / mL MPC aqueous solution is added with a syringe, and after reacting for 24 hours, Gel-NPs-PMPC is obtained by dialysis purification and freeze-drying, and the chain length of the obtained spherical polyelectrolyte brush is 150 nm.

[0079] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent transformation or modification made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing gelatin polyelectrolyte brushes by thermally initiated emulsion polymerization. It is characterized in that The specific steps include: S1: Using gelatin as raw material, gelatin self-assembles to form gelatin nanoparticles by adding a cross-linking agent; S2: using methacrylic anhydride to perform surface modification on the prepared gelatin nanoparticles to prepare methacrylated gelatin nanoparticles; S3: preparing a gelatin spherical polyelectrolyte brush by thermally initiating emulsion polymerization of the methacrylated gelatin nanoparticles and a monomer 2-methacryloyloxyethyl phosphorylcholine (MPC); In the polymerization reaction, the mass ratio of the monomer 2-methacryloyloxyethyl phosphorylcholine to the methacrylic anhydride-modified gelatin nanoparticles is (1-10):

1.

2. The method for preparing gelatin polyelectrolyte brushes by thermally initiated emulsion polymerization according to claim 1, It is characterized in that The thermal initiator used in the polymerization reaction is selected from potassium persulfate, ammonium persulfate or azobisisobutyronitrile.

3. The method for preparing gelatin polyelectrolyte brush by thermally initiated emulsion polymerization according to claim 1, It is characterized in that The polymerization temperature is 50-95°C.

4. The method for preparing gelatin polyelectrolyte brush by thermally initiated emulsion polymerization according to claim 1, It is characterized in that The chain length of the prepared gelatin spherical polyelectrolyte brush is 10-200 nm.

5. The method for preparing gelatin polyelectrolyte brush by thermally initiated emulsion polymerization according to claim 1, It is characterized in that In step S1, the preparation of the gelatin nanoparticles comprises the following steps: (1) Mix gelatin and deionized water, stir to dissolve, then add concentrated hydrochloric acid to adjust the pH value of the system to 1-3; (2) Adding excess acetone to the reaction system until the turbidity of the reaction system increases significantly, causing the long chains of gelatin molecules to curl up to form self-assembled nanoparticles; (3) adding a cross-linking agent glutaraldehyde solution to cross-link and solidify the gelatin particles; (4) adding guanidine hydrochloride solution to neutralize the residual glutaraldehyde in the reaction system and terminate the cross-linking reaction, and centrifuging, purifying, and freeze-drying the solution to obtain self-assembled gelatin nanoparticles.

6. The method for preparing gelatin polyelectrolyte brushes by thermally initiated emulsion polymerization according to claim 1, It is characterized in that In step S2, the preparation of the methacrylated gelatin nanoparticles comprises the following steps: (1) mixing and stirring the gelatin nanoparticles and the carbonic acid-sodium bicarbonate buffer to dissolve, and adjusting the pH to 8-10; (2) Add a certain amount of methacrylic anhydride and carry out the reaction at 50-55°C in the dark; (3) After the reaction is completed in a dark environment, the product is dialyzed in hot water for purification, and the molecular weight cut-off of the dialysis bag is 8-14 KDa; (4) freeze-drying the purified solution to obtain the desired methacrylated gelatin nanoparticles.

7. The method for preparing gelatin polyelectrolyte brushes by thermally initiated emulsion polymerization according to claim 1, It is characterized in that In step S3, the preparation of the gelatin spherical polyelectrolyte brush comprises the following steps: (1) A certain amount of methacrylated gelatin nanoparticles and a thermal initiator are mixed, and after nitrogen is pumped in, 2-methacryloyloxyethyl phosphorylcholine monomer is dissolved in deionized water and injected into the mixed system of gelatin nanoparticles and the thermal initiator; and the reaction system is mixed and stirred at 50-95°C to perform a polymerization reaction; (2) The reaction product of step (1) is then dialyzed and purified in deionized water using an 8-14 KDa dialysis bag to obtain the gelatin spherical polyelectrolyte brush.

8. A gelatin spherical polyelectrolyte brush prepared according to the method for preparing a gelatin polyelectrolyte brush according to any one of claims 1 to 7.