Mg(OH)2 / carbon nanofiber membrane and its preparation method and application in heavy metal ion adsorption
By electrophoresis deposition of magnesium hydroxide on carbon nanofiber membranes, a three-dimensional network structure Mg(OH)2/carbon nanofiber membrane was formed, which solved the problem of poor adsorption effect of nanofiber membranes and achieved efficient and low-cost heavy metal ions Adsorption, suitable for large-scale industrial applications.
Patent Information
- Application Number
- CN202311301796.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-10-09
AI Technical Summary
The existing nanofiber membranes have problems such as few active adsorption sites, low interception and poor adsorption effects in the adsorption of heavy metal ions. The traditional methods are costly, have high energy consumption, and are prone to secondary pollution, making them difficult to be suitable for large-scale applications.
Electrophoretic deposition method is used to load magnesium hydroxide on the carbon nanofiber membrane, disperse magnesium ions through graphene oxide material to form a three-dimensional network structure Mg(OH)2/carbon nanofiber membrane, and use the hydroxyl group on the surface of Mg(OH)2 The synergistic effect of structure and π-electrons of carbon nanofibers improves the adsorption effect of heavy metal ions.
It improves the mechanical properties and adsorption properties of carbon nanofiber membranes, and achieves efficient adsorption of heavy metal ions. It has simple process, low cost, suitable for large-scale industrial production, and low secondary pollution.
Smart Images

Figure CN117504817B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water treatment, and in particular to a Mg(OH)2 / carbon nanofiber membrane and a preparation method thereof and application thereof in heavy metal ion adsorption. Background Art
[0002] Heavy metal pollution in water bodies refers to the pollution caused by pollutants containing heavy metal ions entering the water body. Heavy metal pollution in water bodies mainly comes from wastewater discharge from mining, metallurgy, chemical industry, electronics and other industries. Heavy metals are difficult to degrade in the environment, and with the long-term enrichment and accumulation in the food chain, exceeding the threshold can cause damage to the nervous system and functional lesions of the body, seriously threatening water ecological security and human health. On the other hand, a large amount of heavy metal ions in wastewater are directly discharged, resulting in a waste of resources. Therefore, the efficient disposal of heavy metal wastewater has become a major problem in the field of water pollution control.
[0003] For the disposal of heavy metals, the relevant technologies mainly use chemical precipitation, ion exchange, electrochemical method, membrane technology and adsorption method. Among them, although the chemical precipitation method is mature in technology and has a stable treatment effect, the pH for the best precipitation of most heavy metal ions is around 10, which will lead to excessive consumption of alkali and the production of a large amount of waste residue, causing huge negative effects on the environment and ecology. However, the ion exchange method, electrochemical method, and membrane technology have high costs, high energy consumption, low water production rate, and are very likely to cause secondary pollution, and are not suitable for large-scale applications. As for the adsorption method, it has the advantages of low cost, high efficiency, simple operation, and mature technology, and has attracted widespread attention. It includes nanofiber membrane adsorption and nanoparticle adsorption, but the existing nanofiber membranes and nanoparticles have the problems of few active adsorption sites, low interception rate, and poor adsorption effect. Summary of the invention
[0004] In order to solve or partially solve the problems existing in the related art, the present invention provides a Mg(OH)2 / carbon nanofiber membrane and a preparation method thereof.
[0005] The present invention provides a method for preparing a Mg(OH)2 / carbon nanofiber membrane, which comprises:
[0006] Using electrophoretic deposition, graphene oxide material-Mg 2+ In the colloidal suspension, two carbon nanofiber membranes were used as cathode and anode respectively, Ag / AgCl was used as reference electrode, and graphene oxide material-Mg 2+ Mg(OH)2 / carbon nanofiber film is deposited on the cathode surface; the graphene oxide material is graphene oxide and / or reduced graphene oxide; the diameter of the carbon nanofiber in the carbon nanofiber film is 100-300nm; the graphene oxide material-Mg 2+The particle size of the graphene oxide material in the colloidal suspension is smaller than the diameter of the carbon nanofiber membrane.
[0007] Furthermore, the graphene oxide material-Mg 2+ The colloidal suspension is GO-Mg 2+ The colloidal suspension is prepared according to the following method:
[0008] Add GO dispersion to the solution containing magnesium ions and mix well to form GO-Mg 2+ Colloidal suspension; the GO particle size in the GO dispersion is 10 to 100 nm.
[0009] Furthermore, the GO-Mg 2+ The concentration of GO in the colloidal suspension is 0.5-5 g / L, and the concentration of magnesium ions is 0.5-5 mol / L.
[0010] Furthermore, the solution containing magnesium ions is one or more of magnesium nitrate solution, magnesium chloride solution and magnesium sulfate solution.
[0011] Furthermore, during the electrodeposition process, a DC voltage of 3 to 9 V was applied to adjust the graphene oxide material-Mg 2+ The pH value of the colloidal suspension is 5 to 9, and the sedimentation time is 10 to 60 seconds.
[0012] Furthermore, the carbon nanofiber membrane is prepared according to the following method:
[0013] Polyacrylonitrile (PAN) was dissolved in N,N-dimethylformamide (DMF) and polyacrylonitrile nanofiber membrane was prepared by electrospinning.
[0014] The polyacrylonitrile nanofiber membrane is subjected to pre-oxidation and high-temperature carbonization treatment to obtain a carbon nanofiber membrane.
[0015] Furthermore, the pre-oxidation treatment is specifically as follows: the polyacrylonitrile nanofiber membrane is placed in a muffle furnace and pre-oxidized at 200-300° C.;
[0016] The high temperature carbonization treatment is specifically as follows: placing the pre-oxidized polyacrylonitrile nanofiber membrane into a tubular furnace under argon conditions and performing a high temperature carbonization treatment at 700-1000°C.
[0017] Furthermore, the method also includes the following steps: cleaning and drying the prepared Mg(OH)2 / carbon nanofiber membrane.
[0018] The present invention also provides a Mg(OH)2 / carbon nanofiber membrane, which comprises: carbon nanofibers, and Mg(OH)2 uniformly loaded on the surface of the carbon nanofibers and between the carbon nanofibers.
[0019] The present invention also provides an application of the above Mg(OH)2 / carbon nanofiber membrane in heavy metal ion adsorption, which allows water containing heavy metal ions to pass through the Mg(OH)2 / carbon nanofiber membrane in a dead-end filtration manner.
[0020] The Mg(OH)2 / carbon nanofiber membrane preparation method provided by the present invention may have the following beneficial effects:
[0021] 1. This method uses carbon nanofiber membrane as a substrate and loads magnesium hydroxide to form Mg(OH)2 / carbon nanofiber membrane. On the one hand, it can improve the mechanical properties of the carbon nanofiber membrane; on the other hand, the electrostatic adsorption of the hydroxyl structure on the surface of Mg(OH)2 and the electronic complexation of the conjugated structure π electrons of the carbon nanofiber synergistically enhance the adsorption effect of heavy metal ions.
[0022] 2. Electrodeposition is used, and graphene oxide material is used as a dispersion liquid to disperse magnesium ions and reduce the stacking density of magnesium ions at the cathode. In addition, the graphene oxide material is reduced at the cathode to form an rGO sheet structure, which is interspersed on the surface of the Mg(OH)2 layer, thereby greatly destroying the interlayer flatness of the Mg(OH)2 layer, making it difficult to stack multiple layers, and finally making the Mg(OH)2 uniformly dispersed and deposited. At the same time, the size of the carbon nanofibers and graphene oxide materials is controlled to achieve that magnesium hydroxide can not only be deposited on the surface of the carbon nanofibers, but also between the carbon nanofibers, thereby forming a Mg(OH)2 / carbon nanofiber membrane with a microscopic three-dimensional network structure. The advantages of the three-dimensional network structure, such as large specific surface area and high interception ratio, further improve the adsorption performance.
[0023] 3. This method has the advantages of simple preparation process, high production efficiency, short process and low cost. The prepared Mg(OH)2 / carbon nanofiber membrane has high adsorption efficiency for heavy metal ions in wastewater. In addition, the heavy metal ions can be easily separated and the secondary pollution is low, which is suitable for large-scale industrial production and promotion.
[0024] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention in conjunction with the accompanying drawings, wherein like reference numerals generally represent like components throughout the exemplary embodiments of the present invention.
[0026] Figure 1are scanning electron microscope images of the carbon nanofiber membrane, Mg(OH)2 / carbon nanofiber membrane 6-Mg-GC-10, Mg(OH)2 / carbon nanofiber membrane 6-Mg-GC-30, and Mg(OH)2 / carbon nanofiber membrane 6-Mg-GC-60 prepared in the embodiments of the present invention;
[0027] Figure 2 are scanning electron microscope images of Mg(OH)2 / carbon nanofiber membrane 3-Mg-GC-30 and Mg(OH)2 / carbon nanofiber membrane 9-Mg-GC-30 prepared in the examples of the present invention;
[0028] Figure 3 These are scanning electron microscope images of Mg(OH)2 / carbon nanofiber membrane Mg-GC-2 / 1, Mg(OH)2 / carbon nanofiber membrane Mg-GC-1 / 2 and Mg(OH)2 / carbon nanofiber membrane Mg-GC-1 / 0 prepared in accordance with the embodiments of the present invention. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] The terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The singular forms "a", "the" and "the" used in the present invention and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.
[0031] It should be understood that although the terms "first", "second", "third", etc. may be used to describe various information in the present invention, such information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of the present invention, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0032] The inventors of the present application have found through research that one of the main reasons for the above-mentioned problems of the adsorption material is that the commonly used nanofiber membrane adsorption material has a relatively coarse fiber diameter (about 1 μm), which leads to a large pore size, a lack of active adsorption sites, a low interception rate, and a poor adsorption effect. In response to this problem, the inventors of the present application first considered using nanomaterials with smaller diameters as substrates to increase the adsorption sites. Furthermore, the inventors of the present application considered using carbon nanofiber membranes, which are obtained by carbonizing polymer nanofiber membranes. Carbon nanofiber membranes have the advantages of small pore size, high porosity, and high specific surface area. In addition, carbon nanofibers have conjugated structure π electrons, which have a strong complexing ability with heavy metal ions, so the use of carbon nanofiber membranes helps to improve the adsorption effect.
[0033] Furthermore, the inventors of the present application have found that although the use of carbon nanofiber membranes can improve the adsorption effect of heavy metal ions to a certain extent, their mechanical properties are poor, which imposes certain limitations on their application. In order to improve the mechanical properties of the adsorption membrane, the inventors of the present application considered loading other materials that can adsorb heavy metal ions on the surface of the carbon nanofiber membrane, on the one hand to improve the mechanical properties, and on the other hand to further optimize the adsorption performance. Furthermore, compounds with hydroxyl groups are first considered, because hydroxyl groups can fix heavy metals through electrostatic adsorption; at the same time, it is considered that the hydroxyl compound should be insoluble so as not to be dissolved during the water treatment process. Taking the above into consideration, the inventors of the present application considered using magnesium hydroxide as an external support and carbon nanofiber membrane as a loading matrix.
[0034] Furthermore, in combination with the characteristics of magnesium ions and the fact that the electrophoretic deposition method has the characteristic of uniform coating, the inventors of the present application considered using the electrophoretic deposition method to deposit magnesium hydroxide on the surface of the carbon nanofiber membrane. However, the inventors of the present application found through practical research that in the process of electrophoretic deposition, since the deposited magnesium hydroxide has a lamellar structure, it is easy to perform multi-layer stacking deposition, which ultimately results in the formation of a magnesium hydroxide support having a block structure and a large size. Not only can it not achieve good adsorption of heavy metal ions, but it also densely covers the adsorption sites of the carbon nanofiber structure, affecting the adsorption performance of the carbon nanofiber membrane.
[0035] Therefore, how to reduce the stacking effect of magnesium hydroxide becomes the focus problem to be solved in this application. In order to solve this problem, the inventors of the present application consider introducing auxiliary compounds in the suspension used for electrodeposition, which can be combined with magnesium ions on the one hand, and play a dispersing effect on magnesium ions, and on the other hand, it also has good electrical conductivity, thereby reducing the aggregation density of magnesium ions on the one hand, and destroying the flatness of the surface of the magnesium hydroxide layer formed by deposition on the other hand, so that it is not easy to stack. Further, the applicant considers using graphene oxide, and the oxygen-containing groups of graphene oxide materials can be combined with magnesium ions, and it has excellent electrical conductivity and mechanical properties at the same time. Similar to graphene oxide, reduced graphene oxide also carries oxygen groups because it is not completely reduced, so it can play a role similar to graphene oxide. Taking the above into consideration, the inventors of the present application consider using graphene oxide / reduced graphene oxide to disperse magnesium ions, and use this as a suspension for electrodeposition, in order to destroy the stacking effect of magnesium hydroxide.
[0036] On this basis, the inventors of the present application have found in practice that after electrodeposition, magnesium hydroxide can not only be deposited on the surface of carbon nanofibers, but also be deposited between the carbon nanofibers, thereby forming a Mg(OH)2 / carbon nanofiber membrane with a microscopic three-dimensional network structure. The surface of the Mg(OH)2 of the fiber membrane has a hydroxyl structure, and the carbon nanofibers have conjugated structure π electrons. The two work synergistically to enhance the adsorption of heavy metal ions. In addition, the three-dimensional network structure has the advantages of large specific surface area and high retention ratio, which further improves the adsorption performance.
[0037] Therefore, the embodiment of the present invention provides a method for preparing a Mg(OH)2 / carbon nanofiber membrane, which comprises the following steps:
[0038] Using electrophoretic deposition, graphene oxide material-Mg 2+ In the colloidal suspension, two carbon nanofiber membranes were used as cathode and anode respectively, Ag / AgCl was used as reference electrode, and graphene oxide material-Mg 2+ Mg(OH)2 / carbon nanofiber film is deposited on the cathode surface; the graphene oxide material is graphene oxide and / or reduced graphene oxide; the diameter of the carbon nanofiber in the carbon nanofiber film is 100-300nm; the graphene oxide material-Mg 2+ The particle size of the graphene oxide material in the colloidal suspension is smaller than the diameter of the carbon nanofiber membrane.
[0039] In this embodiment, magnesium hydroxide is loaded on the carbon nanofiber membrane by electrophoretic deposition. During the electrodeposition process, two carbon nanofiber membranes are placed on the graphene oxide material-Mg 2+The cathode and anode are used in the colloidal suspension, and Ag / AgCl is used as the reference electrode. A DC voltage is applied to make the positively charged graphene oxide material-Mg 2+ Under the action of the electric field, it is easier to migrate and deposit toward the cathode. Graphene oxide / reduced graphene oxide is reduced at the cathode to form rGO sheet structure, which is interspersed on the surface of the Mg(OH)2 layer, thereby greatly destroying the interlayer flatness of the Mg(OH)2 layer, making it difficult to stack multiple layers, and finally making the Mg(OH)2 uniformly dispersed and deposited.
[0040] In order to achieve the above effects, the matching between the particle size of the graphene oxide material and the diameter of the carbon nanofiber is more important. If the particle size of the graphene oxide is larger than the diameter of the carbon nanofiber, it is easy to cause the deposition on the surface of the carbon nanofiber to form spheroids. For this reason, the particle size of the graphene oxide material in this embodiment is controlled to be smaller than the diameter of the carbon nanofiber membrane. For the diameter of the carbon nanofiber in the carbon nanofiber membrane, the smaller the diameter, the better the adsorption effect. However, the smaller the fiber diameter, the smaller the particle size of the graphene oxide material. Therefore, if the diameter of the carbon nanofiber is too small, the cost of the graphene oxide material will be too high or it will be difficult to obtain the raw materials that meet the requirements. For this reason, the diameter of the carbon nanofiber in the carbon nanofiber membrane used in this application is 100-300nm. The carbon nanofiber membrane of this size has good adsorption performance, and the graphene oxide material matching it is also easier to obtain. Further preferably, the particle size of the graphene oxide material is preferably 10-100nm.
[0041] The carbon nanofiber membrane is preferably prepared according to the following method:
[0042] Polyacrylonitrile (PAN) was dissolved in N,N-dimethylformamide (DMF) and polyacrylonitrile nanofiber membrane was prepared by electrospinning.
[0043] The polyacrylonitrile nanofiber membrane is subjected to pre-oxidation and high-temperature carbonization treatment to obtain a carbon nanofiber membrane.
[0044] Specifically, the pre-oxidation treatment is preferably: placing the polyacrylonitrile nanofiber membrane in a muffle furnace and pre-oxidizing it at 200-300°C; the high-temperature carbonization treatment is preferably: placing the pre-oxidized polyacrylonitrile nanofiber membrane in a tubular furnace under argon conditions and performing high-temperature carbonization treatment at 700-1000°C. Thus, a carbon nanofiber membrane can be obtained.
[0045] In order to remove impurities remaining on the surface of the obtained carbon nanofiber membrane, the obtained carbon nanofiber membrane is preferably subjected to the following post-treatment: the obtained carbon nanofiber membrane is sequentially immersed in a polyethylene glycol octyl phenyl ether solution, an acetone and a sulfuric acid solution, ultrasonically treated in ultrapure water, and then dried. More specifically, the obtained carbon nanofiber membrane is sequentially immersed in a 0.1% polyethylene glycol octyl phenyl ether solution, a 1 mol / L acetone, and a 1 mol / L sulfuric acid solution, and then ultrasonicated in ultrapure water for 2 hours. The drying temperature can specifically be below 60°C.
[0046] The suspension used for electrodeposition is graphene oxide material-Mg 2+ The colloidal suspension, wherein the graphite oxide material is graphene oxide, reduced graphene oxide, or a combination of the two. The graphene oxide material described in the present application -Mg 2+ The colloidal suspension contains graphene oxide material and -Mg 2+ The graphene oxide material has an oxygen radical, which can combine with magnesium ions to form a graphene oxide material-Mg 2+ The purpose of using this suspension is to use graphene oxide material to disperse magnesium ions and reduce the stacking density of magnesium ions at the cathode. In addition, the graphene oxide material is reduced at the cathode to form an rGO sheet structure, which is interspersed on the surface of the Mg(OH)2 layer, thereby greatly destroying the interlayer flatness of the Mg(OH)2 layer, making it difficult to stack multiple layers, and finally making the Mg(OH)2 uniformly dispersed and deposited.
[0047] The graphene oxide material preferably uses graphene oxide, which has a stronger ability to bind to magnesium ions than reduced graphene oxide. 2+ The colloidal suspension is GO-Mg 2+ The colloidal suspension can be prepared as follows:
[0048] Add GO dispersion to the solution containing magnesium ions and mix well to form GO-Mg 2+ Colloidal suspension; the particle size of GO in the GO dispersion is 10 to 100 nm.
[0049] The mixing time is preferably 1 to 4 hours. The solution containing magnesium ions is preferably one or more of magnesium nitrate solution, magnesium chloride solution and magnesium sulfate solution, and magnesium nitrate solution is more preferred. 2+ The concentration of GO in the colloidal suspension is preferably 0.5 to 5 g / L, and the concentration of magnesium ions is preferably 0.5 to 5 mol / L. More preferably, GO-Mg 2+ The concentration of GO in the colloidal suspension was 0.5 g / L, and the concentration of magnesium ions was 0.5 mol / L.
[0050] The inventors of the present application have found that after electrodeposition, magnesium hydroxide can not only be deposited on the surface of carbon nanofibers, but also between carbon nanofibers, thereby forming a Mg(OH)2 / carbon nanofiber film with a microscopic three-dimensional network structure. The inventors of the present application have further found that the voltage during the electrodeposition process, the pH value of the suspension, and the deposition time have an impact on the microscopic morphology of the final product. As a preferred embodiment of this embodiment, during the electrodeposition process, a DC voltage of 3 to 9 V is applied to adjust the graphene oxide material-Mg 2+ The pH value of the colloidal suspension is 5 to 9, and the deposition time is 10 to 60 seconds. The DC voltage applied is more preferably 3 to 6 V, and the deposition time is more preferably 30 to 60 seconds. 2+ The pH value of the colloidal suspension is more preferably 7; most preferably, the applied DC voltage is 6V, and the graphene oxide material-Mg 2+ The pH value of the colloidal suspension was 7, and the sedimentation time was 30 s.
[0051] After electrodeposition, a Mg(OH)2 / carbon nanofiber membrane can be obtained. In order to remove impurities remaining on the membrane surface, the following steps are preferably also included: the Mg(OH)2 / carbon nanofiber membrane obtained after deposition is washed with deionized water and then dried naturally.
[0052] From the above content, it can be seen that the method for preparing Mg(OH)2 / carbon nanofiber membrane provided in the embodiment of the present invention has the following advantages:
[0053] 1. This method uses carbon nanofiber membrane as the substrate and loads magnesium hydroxide to form Mg(OH)2 / carbon nanofiber membrane. On the one hand, it can improve the mechanical properties of the carbon nanofiber membrane, especially the tensile resistance; on the other hand, under the synergy of the hydroxyl structure on the surface of Mg(OH)2 and the conjugated π electron structure of carbon nanofiber, the adsorption effect of heavy metal ions is enhanced through electrostatic adsorption and cationic π complexation.
[0054] 2. Electrodeposition is used, and graphene oxide material is used as a dispersion liquid to disperse magnesium ions and reduce the stacking density of magnesium ions at the cathode. In addition, the graphene oxide material is reduced at the cathode to form an rGO sheet structure, which is interspersed on the surface of the Mg(OH)2 layer, thereby greatly destroying the interlayer flatness of the Mg(OH)2 layer, making it difficult to stack multiple layers, and finally making the Mg(OH)2 uniformly dispersed and deposited. At the same time, the size of the carbon nanofibers and graphene oxide materials is controlled to achieve that magnesium hydroxide can not only be deposited on the surface of the carbon nanofibers, but also between the carbon nanofibers, thereby forming a Mg(OH)2 / carbon nanofiber membrane with a microscopic three-dimensional network structure. The advantages of the three-dimensional network structure, such as large specific surface area and high interception ratio, further improve the adsorption performance.
[0055] 3. This method has the advantages of simple preparation process, high production efficiency, short process and low cost. The prepared Mg(OH)2 / carbon nanofiber membrane has high adsorption efficiency for heavy metal ions in wastewater. In addition, the heavy metal ions can be easily separated and the secondary pollution is low, which is suitable for large-scale industrial production and promotion.
[0056] Correspondingly, another embodiment of the present invention further provides a Mg(OH)2 / carbon nanofiber membrane, which includes: carbon nanofibers, and Mg(OH)2 uniformly loaded on the surface of the carbon nanofibers and between the carbon nanofibers.
[0057] Preferably, the thickness of the carbon nanofiber membrane is 0.08-0.15 mm, the diameter of the carbon nanofiber is 100-300 nm, the mass percentage of Mg(OH)2 loaded on the carbon nanofiber membrane per unit area can reach 128%-148%, and the specific surface area is greater than 150%.
[0058] The Mg(OH)2 / carbon nanofiber membrane can be prepared according to the method of the above embodiment. The electrostatic adsorption of the hydroxyl structure on the surface of Mg(OH)2 and the electronic complexation of the conjugated structure π electrons of the carbon nanofiber synergistically enhance the adsorption effect of heavy metal ions. In addition, compared with the carbon nanofiber membrane, its mechanical properties, especially tensile strength, are more excellent. The membrane is a three-dimensional network structure, which has the advantages of large specific surface area and high interception ratio, thereby further improving the adsorption performance. Therefore, the Mg(OH)2 / carbon nanofiber membrane has a high adsorption efficiency for heavy metal ions in wastewater. The membrane has a wide range of applications and has a good adsorption effect on sewage with a heavy metal ion concentration in the range of 0.1 to 10 ppm. In addition, the Mg(OH)2 / carbon nanofiber membrane is easy to separate heavy metal ions after use, has low secondary pollution, and is suitable for large-scale industrial production and promotion.
[0059] Based on the advantages of the Mg(OH)2 / carbon nanofiber membrane having strong flexibility and high flux, another embodiment of the present invention further provides an application of the Mg(OH)2 / carbon nanofiber membrane in heavy metal ion adsorption, which specifically comprises: allowing water containing heavy metal ions to pass through the Mg(OH)2 / carbon nanofiber membrane in a dead-end filtration manner. This method can achieve rapid adsorption and retention of positively charged heavy metal ions in water.
[0060] Preferably, the Mg(OH)2 / carbon nanofiber membrane can be 2 to 10 membranes stacked together and placed in a filtering device for use.
[0061] This method can be applied to the treatment of wastewater containing one or two heavy metal ions of copper, lead, cadmium or nickel, and has a good adsorption effect for heavy metal ion concentrations of 0.1 to 100 ppm and a pH range of 5 to 9.
[0062] The technical solution of the present invention is further described below in conjunction with specific embodiments:
[0063] The graphene oxide GO in the following examples was purchased from Carbon Rich Technology, and its particle size was 100 nm.
[0064] Example 1
[0065] 1. Dissolve 1.2 g of polyacrylonitrile PAN in 10 mL of N,N-dimethylformamide DMF, stir the solution for 12 h, and synthesize polyacrylonitrile PAN nanofiber membrane using electrospinning technology; wherein: the spinning solution is loaded into a 20 mL syringe with a metal needle, the working voltage of the electrospinning machine is 20 kV (positive pressure is 18 kV, negative pressure is -2 kV), aluminum foil is used as the receiving material, the distance between the needle and the receiver is set to 12 cm, and the feeding ratio of the spinning solution is set to 1.0 mL / h;
[0066] 2. The polyacrylonitrile (PAN) nanofiber membrane obtained in step 1 was pre-oxidized in a muffle furnace at 230°C for 1 hour, and then placed in a tubular furnace for carbonization under argon for 12 hours to obtain a carbon nanofiber membrane; the obtained carbon nanofiber membrane was subsequently treated as follows: soaked in 0.1% polyethylene glycol octylphenyl ether solution, 1 mol / L acetone, 1 mol / L sulfuric acid solution and ultrapure water for 2 hours to completely remove surface residual impurities, and dried at 60°C to obtain a clean carbon nanofiber membrane. The scanning electron microscope image of the obtained carbon nanofiber membrane is as shown in FIG. Figure 1 As shown in a.
[0067] 3. Add 1g / L graphene oxide GO dispersion to 1mol / L magnesium nitrate solution in equal volume and mix thoroughly for 4h to obtain GO-Mg 2+ The colloidal suspension has a GO concentration of 0.5 g / L and a magnesium ion concentration of 0.5 mol / L.
[0068] 4. Using electrophoretic deposition, place two carbon nanofiber membranes from step 2 on the GO-Mg 2+ The cathode and anode were used in the colloidal suspension, and Ag / AgCl was used as the reference electrode. A DC voltage of 6 V was applied. The GO-Mg 2+ The pH of the colloidal suspension was 7.00, and the deposition time was 10 s, 30 s, and 60 s, respectively. The Mg(OH)2 / carbon nanofiber membranes obtained after deposition were washed with deionized water and dried naturally. The obtained Mg(OH)2 / carbon nanofiber membranes were labeled as 6-Mg-GC-10, 6-Mg-GC-30, and 6-Mg-GC-60, respectively. The scanning electron microscope images are shown in FIG. Figure 1 b. Figure 1 c. Figure 1The physical properties of the Mg(OH)2 / carbon nanofiber membrane and its adsorption capacity for heavy metals were tested respectively (using the fourth edition of the water and wastewater monitoring and analysis method and the ICP-OES instrument to determine the heavy metal ion concentration). The test results are shown in Table 1:
[0069] Table 1 Physical properties and heavy metal adsorption capacity of Mg(OH)2 / carbon nanofiber membrane prepared in Example 1
[0070]
[0071]
Adsorption performance test
[0072] Water containing heavy metal ions was filtered through three Mg(OH)2 / carbon nanofiber membranes (single layer) prepared in this embodiment in a dead-end filtration manner, and the adsorption performance of different heavy metal ions was tested in 5 minutes. The test results are shown in Table 2:
[0073] Table 2 Adsorption performance test results of Mg(OH)2 / carbon nanofiber membrane prepared in Example 1
[0074] Nanofiber membrane number 6-Mg-GC-10 6-Mg-GC-30 6-Mg-GC-60 Copper ions 1.9mg / g 15.4mg / g 11.9mg / g Lead ions 2.1mg / g 12.9mg / g 8.4mg / g Cadmium ions 3.3mg / g 19.2mg / g 14.2mg / g Nickel Ion 4.6mg / g 20.5mg / g 17.3mg / g
[0075] Example 2
[0076] Steps 1, 2 and 3 are the same as those in Example 1.
[0077] 4. Using electrophoretic deposition, place two carbon nanofiber membranes from step 2 on the GO-Mg 2+ The cathode and anode were used in the colloidal suspension, and Ag / AgCl was used as the reference electrode. DC voltages of 3 V, 6 V, and 9 V were applied respectively. The GO-Mg 2+ The pH of the colloidal suspension was 7.00, and the deposition time was 30 s. The Mg(OH)2 / carbon nanofiber membrane obtained after deposition was washed with deionized water and dried naturally. The obtained Mg(OH)2 / carbon nanofiber membranes were labeled as 3-Mg-GC-30, 6-Mg-GC-30, and 9-Mg-GC-30, respectively. The scanning electron microscope images are shown in FIG. Figure 2 a. Figure 1 c. Figure 2 The physical properties of the Mg(OH)2 / carbon nanofiber membrane and its adsorption capacity for heavy metals were tested respectively, and the test results are shown in Table 3:
[0078] Table 3 Physical properties and heavy metal adsorption capacity of Mg(OH)2 / carbon nanofiber membrane prepared in Example 2
[0079]
[0080]
Adsorption performance test
[0081] Water containing heavy metal ions was filtered through three Mg(OH)2 / carbon nanofiber membranes (single layer) prepared in this embodiment in a dead-end filtration manner, and the adsorption performance of different heavy metal ions was tested in 5 minutes. The test results are shown in Table 4:
[0082] Table 4 Adsorption performance test results of Mg(OH)2 / carbon nanofiber membrane prepared in Example 2
[0083] Nanofiber membrane number 3-Mg-GC-30 6-Mg-GC-30 9-Mg-GC-30 Copper ions 9.4mg / g 15.4mg / g 6.6mg / g Lead ions 6.8mg / g 12.9mg / g 5.9mg / g Cadmium ions 12.9mg / g 19.2mg / g 10.5mg / g Nickel Ion 15.1mg / g 20.5mg / g 8.2mg / g
[0084] Example 3
[0085] Steps 1 and 2 are the same as those in Example 1.
[0086] 3. Mix the magnesium nitrate solution and graphene oxide GO dispersion in a ratio of 2:1, 0.5:1, and 1:0, respectively, and mix them thoroughly for 4 hours to obtain GO-Mg 2+ Colloidal suspensions, the concentrations of magnesium ions and GO in the suspensions were 1 mol / L and 0.5 g / L, 0.5 mol / L and 1 g / L, and 1 mol / L and 0 g / L, respectively.
[0087] 4. Using electrophoretic deposition, place two carbon nanofiber membranes from step 2 on the GO-Mg 2+ The cathode and anode were used in the colloidal suspension, and Ag / AgCl was used as the reference electrode. A DC voltage of 6 V was applied. The GO-Mg 2+ The pH of the colloidal suspension was 7.00 and the deposition time was 30 s. The Mg(OH)2 / carbon nanofiber membrane obtained after deposition was washed with deionized water and dried naturally. The obtained Mg(OH)2 / carbon nanofiber membranes were labeled as Mg-GC-2 / 1, Mg-GC-1 / 2, and Mg-GC-1 / 0, respectively. The scanning electron microscope images were as follows: Figure 3 a. Figure 3 b. Figure 3 c. The physical properties of the Mg(OH)2 / carbon nanofiber membrane and its adsorption capacity for heavy metals were tested respectively, and the test results are shown in Table 5:
[0088] Table 5 Physical properties and heavy metal adsorption capacity of Mg(OH)2 / carbon nanofiber membrane prepared in Example 3
[0089]
[0090]
[0091]
Adsorption performance test
[0092] The water containing heavy metal ions was passed through three Mg(OH)2 / carbon nanofiber membranes (single layer) prepared in this embodiment by dead-end filtration, and the adsorption performance of different heavy metal ions was tested in 5 minutes. The test results are shown in Table 6:
[0093] Table 6 Adsorption performance test results of Mg(OH)2 / carbon nanofiber membrane prepared in Example 3
[0094] Nanofiber membrane number Mg-GC-2 / 1 Mg-GC-1 / 2 Mg-GC-1 / 0 Copper ions 6.0mg / g 11.4mg / g 1.8mg / g Lead ions 5.4mg / g 8.0mg / g 2.2mg / g Cadmium ions 6.9mg / g 10.9mg / g 3.6mg / g Nickel Ion 7.2mg / g 15.4mg / g 4.3mg / g
[0095] Depend on Figure 1 b~d, Figure 2 a and Figure 3 As shown in a-b, the method of the present invention can be used to prepare a Mg(OH)2 / carbon nanofiber membrane with a three-dimensional network structure. Figure 3 c It can be seen that adding GO to the suspension can promote the uniform dispersion of the load of magnesium hydroxide layer structure and avoid its block stacking on the electrode surface. Figure 2 b It can be seen that a deposition voltage that is too high (9 V) will cause the carbon nanofibers to break, thereby affecting the Mg(OH)2 deposition load.
[0096] It can be seen from Tables 1, 3 and 5 that the specific surface area of the Mg(OH)2 / carbon nanofiber membrane prepared in the embodiment of the present invention is greater than 150 m 2 / g, breaking strength is 1.5-3.5Mpa, breaking elongation is 2-10%, the adsorption rate of copper ions is 20-95%, the adsorption rate of lead ions is 12-92%, the adsorption rate of cadmium ions is 16-94%, and the adsorption rate of nickel ions is 10-94%.
[0097] The Mg(OH)2 / carbon nanofiber membrane prepared in the embodiment of the present invention can adsorb 1.9-15.4 mg / g of copper ions, 3-12 mg / g of lead ions, 3.3-19.2 mg / g of cadmium ions, and 4.6-20.5 mg / g of nickel ions within 5 minutes.
[0098] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
Claims
1. Application of Mg(OH)2 / carbon nanofiber membrane in heavy metal ion adsorption, characterized in that: The water containing heavy metal ions is passed through the Mg(OH)2 / carbon nanofiber membrane by dead-end filtration; The preparation method of the Mg(OH)2 / carbon nanofiber membrane comprises: Using electrophoretic deposition, graphene oxide material-Mg 2+ In the colloidal suspension, two carbon nanofiber membranes were used as cathode and anode respectively, Ag / AgCl was used as reference electrode, and graphene oxide material-Mg 2+ Mg(OH)2 / carbon nanofiber film is deposited on the cathode surface; The graphene oxide material-Mg 2+ The colloidal suspension is GO-Mg 2+ The colloidal suspension is prepared by adding GO dispersion to a solution containing magnesium ions and mixing them uniformly to form GO-Mg 2+ Colloidal suspension; the GO-Mg 2+ The concentration of GO in the colloidal suspension was 0.5~5 g / L, and the concentration of magnesium ions was 0.5~5 mol / L; The graphene oxide material-Mg 2+ The particle size of the graphene oxide material in the colloidal suspension is smaller than the diameter of the carbon nanofiber membrane; the diameter of the carbon nanofiber in the carbon nanofiber membrane is 100-300 nm; the particle size of GO in the GO dispersion is 10-100 nm; During the electrodeposition process, a DC voltage of 3 to 6 V was applied to adjust the graphene oxide material-Mg 2+ The pH value of the colloidal suspension is 5~9, and the sedimentation time is 30~60 s.
2. The use according to claim 1, characterized in that: The solution containing magnesium ions is one or more of magnesium nitrate solution, magnesium chloride solution and magnesium sulfate solution.
3. The use according to claim 1, characterized in that: The carbon nanofiber membrane is prepared according to the following method: Polyacrylonitrile was dissolved in N,N-dimethylformamide and polyacrylonitrile nanofiber membrane was prepared by electrospinning. The polyacrylonitrile nanofiber membrane is subjected to pre-oxidation and high-temperature carbonization treatment to obtain a carbon nanofiber membrane.
4. The use according to claim 3, characterized in that: The pre-oxidation treatment is specifically as follows: the polyacrylonitrile nanofiber membrane is placed in a muffle furnace and pre-oxidized at 200-300°C; The high temperature carbonization treatment is specifically as follows: placing the pre-oxidized polyacrylonitrile nanofiber membrane into a tubular furnace under argon conditions and performing a high temperature carbonization treatment at 700-1000°C.
5. The use according to claim 1, characterized in that: The method for preparing the Mg(OH)2 / carbon nanofiber membrane further comprises the following steps: The prepared Mg(OH)2 / carbon nanofiber membrane was cleaned and then dried.