A kind of water-based ink for printing and its preparation method and application
Through the simplified preparation method, the dispersion and friction resistance of water-based inks are improved, the complex problems of existing water-based ink processes are solved, and better printing effect and performance optimization are achieved.
Patent Information
- Application Number
- CN202410101960.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-01-25
AI Technical Summary
The process steps of existing water-based inks are cumbersome and complex, and their performance needs to be further improved and optimized.
A preparation method is adopted, including the preparation of aqueous acrylic copolymer resin, the preparation of functional additives of aqueous inks and the preparation of aqueous inks, by ethanolizing acrylic acid, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate. In the reaction, azodiisobutyronitrile was added and vacuum distilled, followed by dropping ammonia water to adjust the pH, combining NN-dimethacrylamide, dimethylaminoethyl methacrylate, vinyl tris(2-methoxyb) The oxy)silane is refluxed in ethanol and finally stirred with the pigment and dispersant to grind and prepare.
The preparation process is simplified, the dispersion, friction resistance, and crust resistance of water-based inks are improved, and it has good viscosity and storage stability. It is suitable for printing a variety of substrates and has excellent printing effect.
Smart Images

Figure CN117925005B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a water-based ink for printing and a preparation method thereof, and in particular to an application of the water-based ink for printing. Background Art
[0002] Paper and plastic film are currently one of the main packaging materials. In traditional printing, most of them use organic solvent inks for printing, especially in food packaging printing. The use of organic solvent inks will emit hydrocarbons and residual solvents, pollute the air and packaging items, and harm health. With the continuous improvement of people's environmental awareness, green environmental protection has become the development theme of the 21st century.
[0003] Water-based ink is a uniform paste composed of binders, pigments, additives and other substances. It is widely used in printing products such as paper cups, cartons, paper bags, newspapers, textbooks, woven bags, etc. As an emerging green and environmentally friendly printing material, water-based ink is gradually replacing solvent-based ink. Water-based ink has the characteristics of being non-flammable and non-explosive. Flexographic printing and gravure printing using water-based ink are gradually becoming the mainstream printing methods.
[0004] CN108070294A discloses a highly wear-resistant water-based plastic ink and a preparation method thereof, which includes a water-soluble acrylic resin, a water-based acrylic emulsion, a pigment, a cosolvent, an additive, and water, wherein the raw materials of the water-soluble acrylic resin include acrylic monomers, styrene monomers, acrylate monomers, monomers of carboxylic acids or anhydrides with double bonds, and modified maleic anhydride grafted polyolefin wax. The water-soluble acrylic resin can not only improve the wear resistance of the water-based ink and increase the life of the ink, but also improve its solubility in water, so that it is more evenly dispersed in the aqueous solution system, reduce the capacity of the emulsifier, and will not cause printing defects and bubbles, and the printing effect is better.
[0005] CN104693889A discloses a low-odor water-based ink, which is composed of the following raw materials in weight percentage: 10-90% of neutral varnish and 10-90% of neutral color paste; wherein the neutral varnish is composed of the following raw materials in weight percentage: 20-80% of neutral emulsion, 0-20% of neutral resin liquid, 1-8% of anti-wear agent, 0-1% of leveling agent, 0.1-0.5% of defoaming agent, and the rest is deionized water; the neutral color paste is composed of the following raw materials in weight percentage: 20-40% of neutral resin liquid, 25-45% of toner, 0-10% of dispersant, 20-40% of deionized water, and 0.05-0.5% of defoaming agent.
[0006] CN101705030A discloses a method for preparing a gravure water-based ink. First, acrylic acid, styrene, vinyl acetate, water, an emulsifier, and an initiator are mixed and stirred evenly to obtain an acrylic acid-styrene-vinyl acetate ternary copolymer emulsion interpenetrating network type water-soluble resin; then the acrylic acid-styrene-vinyl acetate ternary copolymer emulsion interpenetrating network type water-soluble resin and pigment, water, isopropyl alcohol, ethanol, defoamer, wetting agent, leveling agent, dispersant, coupling agent, and antibacterial agent are placed in an ink mixing barrel for stirring to form a paste ink material; the paste ink material is placed in a three-roll ink press for rolling ink, so that the particles of the pigment are completely crushed and evenly dispersed in the liquid binder, and a gravure water-based ink is prepared. The method is simple in process, and the prepared ink has good printability, wet friction resistance, high gloss, and good adhesion, and can be used for different types of paper.
[0007] However, the solution disclosed in the above patent has complicated and cumbersome process steps, and the performance of the water-based ink needs to be further improved and optimized. Summary of the invention
[0008] Based on this, it is necessary to provide a water-based ink for printing and a preparation method and application thereof to address the above problems.
[0009] A method for preparing a water-based ink for printing, characterized in that it comprises the following steps:
[0010] (1) Preparation of waterborne acrylic copolymer resin
[0011] A mixture of acrylic acid, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate is dissolved in a certain amount of ethanol, and then an appropriate amount of azobisisobutyronitrile is added, and the mixture is reacted at a certain temperature for a period of time in an inert gas. After the reaction is completed, the mixture is cooled to a certain temperature, unreacted monomers and solvents are removed by vacuum distillation, and ammonia water is added dropwise to adjust the pH to obtain a water-based acrylic copolymer resin;
[0012] (2) Preparation of functional additives for water-based inks
[0013] A certain amount of NN-dimethylacrylamide, dimethylaminoethyl methacrylate, vinyl tris(2-methoxyethoxy)silane and organosilicon are dispersed in a certain amount of ethanol, and refluxed for a certain period of time under an inert atmosphere to obtain a functional additive for water-based ink;
[0014] (3) Preparation of water-based ink
[0015] The aqueous acrylic copolymer resin obtained in step (1), the aqueous ink functional additive, pigment, dispersant and solvent obtained in step (2) are added into a reaction kettle and stirred evenly; the temperature is increased and kept warm for a period of time; after the reaction is completed, the mixture is stirred evenly and added into a grinding device for grinding to prepare a slurry, which is filtered to obtain an aqueous ink.
[0016] Preferably, in step (1), the weight proportions of acrylic acid, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate are 5-10, 15-25, 15-20 and 5-10.
[0017] Preferably, in step (1), the amount of ethanol used is 50-100 mL.
[0018] Preferably, in step (1), the reaction temperature is 70-90° C. and the reaction time is 3-5 hours.
[0019] Preferably, in step (1), the inert atmosphere is argon, nitrogen or helium.
[0020] Preferably, in step (1), the temperature is cooled to 30-50°C.
[0021] Preferably, in step (1), the pH is 7.5-8.0
[0022] Preferably, in step (2), the weight proportions of NN-dimethylacrylamide, dimethylaminoethyl methacrylate, vinyl tris(2-methoxyethoxy)silane, and silicone are 10-15, 10-15, 10-15, and 5-10.
[0023] Preferably, in step (2), the reflux time is 3-5 hours.
[0024] Preferably, in step (3), the weight proportions of the aqueous acrylic copolymer resin, aqueous ink functional additive, silicon oxide, pigment, dispersant and solvent are 5-10, 5-10, 3-5, 5-15, 5-10 and 10-50.
[0025] Preferably, in step (3), the pigment is one of transparent yellow pigment, pink pigment, carbon black pigment and phthalocyanine blue pigment; the dispersant is polyamide hyperbranched polymer; and the solvent is water, ethanol or a mixture thereof.
[0026] Preferably, in step (3), the temperature rise range is between 75°C and 90°C, and the insulation time is 1-5 hours.
[0027] Preferably, a water-based ink for printing is characterized by a method for preparing the water-based ink for printing.
[0028] Preferably, the invention relates to an aqueous ink for printing, characterized by its application in aqueous ink, aqueous resin, aqueous slurry and printing slurry.
[0029] The beneficial effects of the present invention are:
[0030] 1. The preparation process of the present invention is relatively simple, easy to operate, and suitable for industrial production.
[0031] 2. The water-based acrylic copolymer resin prepared by the present invention has good water solubility, which is beneficial to improving the dispersibility of ink.
[0032] 3. The functional additives of the water-based ink of the present invention make the ink have excellent properties of friction resistance, non-skinning, corrosion resistance and mildew resistance.
[0033] 4. The water-based ink prepared by the present invention has a smaller particle size, better viscosity, uniform dispersion, ink thickness, required surface energy and good storage stability.
[0034] 5. The PVC and PET films printed with the water-based ink prepared by the present invention have fast drying speed, good color strength, high adhesion due to surface energy difference and excellent friction resistance. The water-based ink can be used for printing on various substrates such as polypropylene (PP), polyethylene (PE), and biaxially oriented polypropylene (BOPP). BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is the mechanism of the waterborne acrylic copolymer resin prepared in Example 1. DETAILED DESCRIPTION
[0036] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0037] Example 1
[0038] like Figure 1 As shown, a method for preparing a water-based ink for printing comprises the following steps:
[0039] (1) Preparation of waterborne acrylic copolymer resin
[0040] A mixture of acrylic acid, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate (the weight proportions of acrylic acid, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate are 5, 15, 15, and 5) is dissolved in 50 mL of ethanol, and then an appropriate amount of azobisisobutyronitrile is added, and the mixture is reacted at 70° C. for 3 hours in a nitrogen atmosphere. After the reaction is completed, the mixture is cooled to 30° C., unreacted monomers and solvents are removed by vacuum distillation, and aqueous ammonia is added dropwise to adjust the pH to 7.5 to obtain a water-based acrylic copolymer resin.
[0041] (2) Preparation of functional additives for water-based inks
[0042] A certain amount of NN-dimethylacrylamide, dimethylaminoethyl methacrylate, and silicone (the weight proportions of NN-dimethylacrylamide, dimethylaminoethyl methacrylate, vinyl tri(2-methoxyethoxy)silane, and silicone are 10, 10, 10, and 5) are dispersed in 50 mL of ethanol and refluxed under a nitrogen atmosphere for 3 hours to obtain a functional additive for water-based ink.
[0043] (3) Preparation of water-based ink
[0044] Add the water-based acrylic copolymer resin obtained in step (1), the water-based ink functional additive obtained in step (2), transparent yellow pigment, polyamide hyperbranched polymer and water into a reaction kettle and stir evenly (the weight proportions are 5, 3, 5, 5 and 10 respectively); heat to 75° C. and keep warm for 1 hour; after the reaction is completed, stir evenly, add into a grinding equipment for grinding to prepare a slurry, filter and obtain a water-based ink.
[0045] Example 2
[0046] A method for preparing a water-based ink for printing comprises the following steps:
[0047] (1) Preparation of waterborne acrylic copolymer resin
[0048] A mixture of acrylic acid, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate (the weight proportions of acrylic acid, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate are 10, 25, 20 and 10) was dissolved in 100 mL of ethanol, and then an appropriate amount of azobisisobutyronitrile was added, and the mixture was reacted at 90° C. for 5 hours in an argon atmosphere. After the reaction was completed, the mixture was cooled to 50° C., unreacted monomers and solvents were removed by vacuum distillation, and aqueous ammonia was added dropwise to adjust the pH to 8 to obtain a water-based acrylic copolymer resin.
[0049] (2) Preparation of functional additives for water-based inks
[0050] A certain amount of NN-dimethylacrylamide, dimethylaminoethyl methacrylate, and silicone (the weight proportions of NN-dimethylacrylamide, dimethylaminoethyl methacrylate, vinyl tri(2-methoxyethoxy)silane, and silicone are 15, 15, 15, and 10) are dispersed in 100 mL of ethanol and refluxed under argon atmosphere for 3 hours to obtain a functional additive for water-based ink.
[0051] (3) Preparation of water-based ink
[0052] Add the water-based acrylic copolymer resin obtained in step (1), the water-based ink functional additive obtained in step (2), pink pigment, sodium naphthalenesulfonate and water into a reaction kettle and stir evenly (the weight proportions are 10, 5, 15, 10 and 50 respectively); heat to 90° C. and keep warm for 5 hours; after the reaction is completed, stir evenly, add into a grinding device for grinding to prepare a slurry, filter and obtain a water-based ink.
[0053] Example 3
[0054] A method for preparing a water-based ink for printing comprises the following steps:
[0055] (1) Preparation of waterborne acrylic copolymer resin
[0056] A mixture of acrylic acid, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate (the weight proportions of acrylic acid, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate are 8, 18, 18 and 7) was dissolved in 75 mL of ethanol, and then an appropriate amount of azobisisobutyronitrile was added, and the mixture was reacted at 80° C. for 4 hours in a nitrogen atmosphere. After the reaction was completed, the mixture was cooled to 30° C., unreacted monomers and solvents were removed by vacuum distillation, and aqueous ammonia was added dropwise to adjust the pH to 7.5 to obtain a water-based acrylic copolymer resin.
[0057] (2) Preparation of functional additives for water-based inks
[0058] A certain amount of NN-dimethylacrylamide, dimethylaminoethyl methacrylate, and silicone (the weight proportions of NN-dimethylacrylamide, dimethylaminoethyl methacrylate, vinyltri(2-methoxyethoxy)silane, and silicone are 12, 12, 12, and 8) are dispersed in 75 mL of ethanol and refluxed under a nitrogen atmosphere for 3 hours to obtain a functional additive for water-based ink.
[0059] (3) Preparation of water-based ink
[0060] Add the water-based acrylic copolymer resin obtained in step (1), the water-based ink functional additive obtained in step (2), phthalocyanine blue pigment, polyamide hyperbranched polymer and water into a reaction kettle and stir evenly (the weight proportions are 8, 8, 3, 8, 8 and 30 respectively); heat to 80° C. and keep warm for 2 hours; after the reaction is completed, stir evenly, add into a grinding equipment for grinding to prepare a slurry, filter and obtain a water-based ink.
[0061] Comparative Example 1
[0062] A method for preparing a water-based ink for printing comprises the following steps:
[0063] (1) Prepare a water-based acrylic resin.
[0064] (2) Preparation of water-based ink
[0065] Add the water-based acrylic copolymer resin, transparent yellow pigment, polyamide hyperbranched polymer and water obtained in step (1) into a reaction kettle and stir evenly (the weight proportions are 5, 5, 5 and 10 respectively); heat to 75° C. and keep warm for 1 hour; after the reaction is completed, stir evenly, add into a grinding equipment to grind to prepare a slurry, filter and obtain a water-based ink.
[0066] Comparative Example 2
[0067] A method for preparing a water-based ink for printing comprises the following steps:
[0068] (1) Prepare a water-based acrylic resin.
[0069] (2) Preparation of functional additives for water-based inks
[0070] A certain amount of NN-dimethylacrylamide, dimethylaminoethyl methacrylate, and silicone (the weight proportions of NN-dimethylacrylamide, dimethylaminoethyl methacrylate, vinyl tri(2-methoxyethoxy)silane, and silicone are 10, 10, 10, and 5) are dispersed in 50 mL of ethanol and refluxed under a nitrogen atmosphere for 3 hours to obtain a functional additive for water-based ink.
[0071] (3) Preparation of water-based ink
[0072] Add the aqueous acrylic resin prepared in step (1), the aqueous ink functional additive obtained in step (2), transparent yellow pigment, polyamide hyperbranched polymer and water into a reaction kettle and stir evenly (the weight proportions are 5, 5, 3, 5, 5 and 10 respectively); heat to 75° C. and keep warm for 1 hour; after the reaction is completed, stir evenly, add into a grinding equipment for grinding to prepare a slurry, filter and obtain aqueous ink.
[0073] Comparative Example 3
[0074] A method for preparing a water-based ink for printing comprises the following steps:
[0075] (1) Preparation of waterborne acrylic copolymer resin
[0076] A mixture of acrylic acid, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate (the weight proportions of acrylic acid, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate are 5, 15, 15, and 5) is dissolved in 50 mL of ethanol, and then an appropriate amount of azobisisobutyronitrile is added, and the mixture is reacted at 70° C. for 3 hours in a nitrogen atmosphere. After the reaction is completed, the mixture is cooled to 30° C., unreacted monomers and solvents are removed by vacuum distillation, and aqueous ammonia is added dropwise to adjust the pH to 7.5 to obtain a water-based acrylic copolymer resin.
[0077] (2) Preparation of water-based ink
[0078] Add the water-based acrylic copolymer resin, transparent yellow pigment, polyamide hyperbranched polymer and water obtained in step (1) into a reaction kettle and stir evenly (the weight proportions are 5, 5, 5 and 10 respectively); heat to 75° C. and keep warm for 1 hour; after the reaction is completed, stir evenly, add into a grinding equipment to grind to prepare a slurry, filter and obtain a water-based ink.
[0079] Characterization Tests:
[0080] The dispersibility and friction resistance tests were performed on Examples 1-3 and Comparative Examples 1-3 respectively.
[0081] Dispersion test: The ink was stored under certain conditions (storage temperature was 25°C) for 3 months, and its stratification and precipitation were observed.
[0082] Friction resistance test: The printed strips were subjected to the same friction treatment (85 rpm, 21b weight block, 50 frictions) using a printing friction tester, and the friction resistance of the strips after friction was evaluated using the density attenuation rate:
[0083] Case Dispersibility Friction resistance Example 1 No precipitation, no stratification Rarely falls off Example 2 No precipitation, no stratification Rarely falls off Example 3 No precipitation, no stratification Rarely falls off Comparative Example 1 Slight precipitation and stratification More shedding Comparative Example 2 Slight precipitation and stratification More shedding Comparative Example 3 Slight precipitation and stratification More shedding
[0084] Table 1
[0085] As can be seen from Table 1, the dispersibility of the water-based inks of Examples 1-3 is no precipitation and no stratification, while Comparative Examples 1-3 have slight precipitation and stratification. The friction resistance of the water-based inks of Examples 1-3 is very little shedding, while Comparative Examples 1-3 have more shedding. The reason may be that the water-based acrylic copolymer resin prepared in the present invention has good water solubility, and then the functional additives for water-based inks are prepared. The functional additives for water-based inks prepared help the ink to have excellent friction resistance and not easy to form skins.
[0086] The above-mentioned embodiments and the description in the specification only express the principle and several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be understood that for ordinary technicians in this field, the present invention can make several variations and improvements based on the above description and embodiments without departing from the concept and scope of the present invention, and these changes and improvements all fall within the scope of the present invention claimed for protection.
Claims
1. A method for preparing a water-based ink for printing, It is characterized in that The steps include: (1) Preparation of water-based acrylic copolymer resin A mixture of acrylic acid, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate is dissolved in a certain amount of ethanol, and then an appropriate amount of azobisisobutyronitrile is added, and the mixture is reacted at a certain temperature for a period of time in an inert atmosphere. After the reaction is completed, the mixture is cooled to a certain temperature, unreacted monomers and solvents are removed by vacuum distillation, and ammonia water is added dropwise to adjust the pH to obtain a water-based acrylic copolymer resin; (2) Preparation of functional additives for water-based inks A certain amount of N,N'-dimethylacrylamide, dimethylaminoethyl methacrylate, vinyl tris(2-methoxyethoxy)silane and organosilicon are dispersed in a certain amount of ethanol, and refluxed for a certain period of time under an inert atmosphere to obtain a functional additive for water-based ink; (3) Preparation of water-based ink Add the water-based acrylic copolymer resin obtained in step (1), the water-based ink functional additive, pigment, dispersant and solvent obtained in step (2) into a reaction kettle and stir evenly; The temperature is raised and kept for a period of time; after the reaction is completed, the mixture is stirred evenly and added into a grinding device for grinding to prepare a slurry, which is filtered to obtain a water-based ink; wherein the pigment is one of a transparent yellow pigment, a pink pigment, a carbon black pigment, and a phthalocyanine blue pigment; In the step (1), the weight proportions of acrylic acid, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate are 5-10, 15-25, 15-20 and 5-10 respectively; the water-based ink has good dispersibility and friction resistance; In the step (2), the weight proportions of N,N'-dimethylacrylamide, dimethylaminoethyl methacrylate, vinyl tris(2-methoxyethoxy)silane, and silicone are 10-15, 10-15, 10-15, and 5-10; In the step (2), the reflux time is 3-5 hours.
2. A method for preparing a water-based ink for printing as claimed in claim 1, Features: In the step (1), the amount of ethanol used is 50-100 mL.
3. A method for preparing a water-based ink for printing as claimed in claim 1, Features: In the step (1), the reaction temperature is 70-90° C. and the reaction time is 3-5 hours; in the step (1), the inert atmosphere is argon, nitrogen or helium.
4. A method for preparing a water-based ink for printing as claimed in claim 1, Features: In the step (1), the mixture is cooled to 30-50° C.; in the step (1), the pH value is 7.5-8.
0.
5. A method for preparing a water-based ink for printing as claimed in claim 1, Features: In the step (3), the weight proportions of the aqueous acrylic copolymer resin, aqueous ink functional additive, pigment, dispersant, and solvent are 5-10, 5-10, 5-15, 5-10, and 10-50; the dispersant is a polyamide hyperbranched polymer; and the solvent is water, ethanol, or a mixture thereof.
6. A method for preparing a water-based ink for printing as claimed in claim 1, Features: In the step (3), the temperature is raised to between 75°C and 90°C, and the insulation time is 1-5 hours.
7. A water-based ink for printing, Features: The invention is prepared by the method for preparing a water-based ink for printing as described in any one of claims 1 to 6.
8. A use of the aqueous ink for printing as claimed in claim 7, Features: Used for printing on polypropylene (PP), polyethylene (PE), and biaxially oriented polypropylene (BOPP) substrates.