A method for resource utilization of deep-sea mining tailings cement based on thermal drying

By thermally drying the deep-sea mining tail cement and mixing it with other natural raw materials, soil improvement agents are prepared, which solves the problems of resource utilization and soil improvement of deep-sea mining tail cement, improves the nutrients and structure of the soil, and meets the islands and reefs and floats. Planting needs in cities and coastal areas.

CN118005459BActive Publication Date: 2024-11-19OCEAN UNIV OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410165301.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-05
Publication Date
2024-11-19
Estimated Expiration
2044-02-05

AI Technical Summary

Technical Problem

The resource utilization of deep-sea mining tail cement in the existing technology has not been effectively solved, resulting in stacking and environmental impact problems, and the soil improvement needs of islands, reefs, floating cities and coastal areas have not been met.

Method used

Deep-sea mining tail cement is processed by thermal drying method, and soil modification agent is prepared by combining earthworm manure, mushroom slag, corn stalk, diatomaceous earth, fly ash, microbial fungus, wood chips, shell powder and other raw materials. It is mechanically dehydrated and watered The steps of chemical reaction and aerobic fermentation can reduce quantification and harmless finish cement and improve the fertilizer supply capacity and structure of the soil.

Benefits of technology

The resource utilization of deep-sea mining tail cement has been achieved, which has significantly improved the nutrient content and fertilizer supply capacity of the soil, improved the soil structure, and is suitable for planting soil improvement in islands, reefs, floating cities and coastal areas, and promoted the growth and development of crops and Yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118005459B_ABST
    Figure CN118005459B_ABST
Patent Text Reader

Abstract

The invention discloses a method for resource utilization of deep-sea mining tailings cement based on thermal drying, and relates to the technical field of resource utilization. According to weight parts, the raw materials include: 100-150 parts of deep-sea mining tailings cement drying products, 30-40 parts of earthworm manure, 50-70 parts of mushroom residues, 10-30 parts of corn stalks, 15-20 parts of diatomaceous earth, 10-15 parts of fly ash, 1-3 parts of microbial agents, 15-25 parts of sawdust, and 10-20 parts of shell powder. The invention prepares a soil conditioner based on thermal drying by cooperating aerobic fermentation of deep-sea mining tailings cement, which can not only effectively improve soil structure, balance pH, and improve soil fertilizer supply capacity, but also can make resource utilization of deep-sea mining tailings cement, while protecting the environment, bringing economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resource utilization, and in particular to a method for resource utilization of deep-sea mining tailings cement based on thermal drying. Background Art

[0002] On the surface of the earth, the ocean occupies most of the area, and the hidden resources are rich and diverse, with huge economic value. With the increasing depletion of land resources, humans have begun to turn their attention to the depths of this blue planet. Deep-sea mining, as an important means of tapping deep-sea resources, is gradually attracting global attention. However, deep-sea mining is not a simple task. It involves a series of technical difficulties and economic benefits, and also has a profound impact on the marine environment. In order to reduce the impact of deep-sea mining activities on the marine ecology, some scholars have proposed lifting the tailings cement and nodules to the sea surface together.

[0003] At present, the resource utilization of deep-sea mining tailings is still in the exploratory stage. How to efficiently utilize deep-sea mining tailings is a difficult research problem. The present invention provides a method for resource utilization of deep-sea mining tailings based on thermal drying, which can not only solve the problems of stacking and land occupation of deep-sea mining tailings, but also promote the resource utilization of deep-sea mining tailings, creating significant economic and environmental value. Summary of the invention

[0004] In view of the above-mentioned needs in the prior art, the purpose of the present invention is to provide a method for resource utilization of deep-sea mining tailings cement based on thermal drying, and to make the deep-sea mining tailings cement into a thermal drying product, so that the deep-sea mining tailings cement is reduced, stabilized and harmless, and is made into a soil conditioner with earthworm castings, mushroom residues, corn straw, diatomaceous earth, fly ash, microbial agents, sawdust, shell powder and other raw materials for use as planting soil in islands, reefs, floating cities and coastal areas, so as to solve the existing problems of resource utilization of deep-sea mining tailings cement and soil improvement in islands, reefs, floating cities and coastal areas.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] The present invention provides a method for resource utilization of deep-sea mining tailings cement based on thermal drying, comprising the following steps:

[0007] S1: Add one or more cationic flocculants and anionic flocculants to deep-sea mining tailings cement and stir and mix at a stirring rate of 100-200 r / min for 3-5 min, and let the mixture stand for 10-30 min to destroy the colloidal stability in the tailings cement and improve the dehydration performance of the tailings cement;

[0008] S2: placing the preliminarily dehydrated tailings cement in one of a belt filter press, a plate and frame filter press, and a centrifugal dehydrator, and performing a secondary mechanical dehydration treatment on the deep-sea mining tailings cement by one of a belt filter press, a plate and frame filter press, and a centrifugal dehydrator, so as to reduce the water content of the tailings cement to 10% to 15%, and obtain sediment tailings cement;

[0009] S3: Put the large-size sediment tail cement into a soil crusher to crush it into sediment tail cement with a particle size of less than 0.1 mm, so as to increase the specific surface area of ​​the sediment tail cement and improve the drying efficiency, and then spray an appropriate amount of water into the crushed sediment tail cement to ensure the humidity and uniformity of the sediment tail cement, which is conducive to the drying process;

[0010] S4: Add quicklime to the sediment tailings cement and stir and mix at a stirring rate of 100-200 r / min for 3-5 min, and send the pretreated tailings cement to a thermal drying device to evaporate the water in the tailings cement by utilizing the heat energy and the hydration reaction of quicklime to obtain a dried tailings cement product;

[0011] S5: Send the tailings cement drying product to the cooling equipment, cool it to 10-20 ℃ to prevent the product from overheating and oxidation, send the cooled tailings cement drying product to the soil grinder for grinding, grind the tailings cement drying product to a particle size of 100-200 meshes, and facilitate resource utilization;

[0012] S6: Mix the dried cement product of deep-sea mining tailings, earthworm castings, mushroom residue, corn stalks, microbial agents and sawdust in proportion, stir at a rate of 200-300 r / min for 3-5 min, add appropriate amount of water to obtain a mixture I, wherein the water content of the mixture I is 30%-40% and the pH is 6-7;

[0013] S7: The mixture is placed in an aerobic fermentation container, and the compost is turned for the first time after the high temperature period ends. Thereafter, the compost is turned once a week. The ventilation method adopts intermittent oxygen supply. The aeration is carried out at two time periods every day, 8:00-9:00 in the morning and 20:00-21:00 in the evening. The ventilation volume is 0.5 L / min and the duration is 1 hour. After fermentation for 1-2 months, mature materials and compost liquid are obtained;

[0014] S8: Mix the decomposed matter with diatomaceous earth, fly ash and shell powder at a stirring rate of 100-200 r / min for 3-5 min to obtain a mixture II, add the compost liquid to the mixture II and stir and mix at a stirring rate of 120-150 r / min for 2-3 min to obtain a soil conditioner;

[0015] S9: Add soil conditioners to the planting soil of islands, reefs, floating cities and coastal areas to improve the planting soil, increase the nutrients in the planting soil, improve the fertilizer supply capacity of the planting soil, and improve the planting soil structure, which will ultimately be reflected in the growth, development, yield and quality of crops.

[0016] The present invention provides a method for resource utilization of deep-sea mining tailings cement based on thermal drying, which comprises the following raw materials in parts by weight:

[0017] 100-150 parts of dried cement products from deep-sea mining tailings, 30-40 parts of earthworm castings, 50-70 parts of mushroom residues, 10-30 parts of corn stalks, 1-3 parts of microbial agents, 15-25 parts of sawdust, 15-20 parts of diatomaceous earth, 10-15 parts of fly ash, and 10-20 parts of shell powder.

[0018] In the above-mentioned method for resource utilization of deep-sea mining tailings based on thermal drying, the mushroom residue is the residue after cultivation of one or more of Auricularia auricula, Flammulina velutipes, Pleurotus eryngii and Pleurotus eryngii;

[0019] In the above-mentioned method for resource utilization of deep-sea mining tailings cement based on thermal drying, the diatomaceous earth is ultrafine diatomaceous earth;

[0020] In the above-mentioned method for resource utilization of deep-sea mining tailings cement based on thermal drying, the fly ash particle size is 200-400 mesh;

[0021] In the above-mentioned method for resource utilization of deep-sea mining tailings cement based on thermal drying, the microbial agent comprises one or more of Bacillus, photosynthetic bacteria, yeast, lactic acid bacteria, and nitrogen-fixing bacteria;

[0022] In the above-mentioned method for resource utilization of deep-sea mining tailings cement based on thermal drying, the particle size of the shell powder is less than 0.1 mm, and it is ground from one or more of the shells of marine organisms such as clam shells, oyster shells, and mussel shells;

[0023] The deep-sea mining tailings cement drying product is a product that uses a series of means to "reduce and render harmless" the deep-sea mining tailings cement, which can inhibit the activity of microorganisms and eliminate pathogens.

[0024] In the above-mentioned method for resource utilization of deep-sea mining tailings cement based on thermal drying, the dried product of the sediment tailings cement is finally crushed into a particle size of less than 0.1 mm;

[0025] Deep-sea mining tailings cement is mainly composed of siliceous clay, rich in mineral elements and trace elements required by plants, but its nitrogen, phosphorus, potassium, organic matter, etc. content is not high and the microbial abundance is low. Making it into a thermal drying product can significantly reduce the volume, achieve the purpose of "reduction and harmlessness", inhibit the activity of microorganisms, and will not produce rancidity, which is convenient for storage and transportation, and is suitable for use as agricultural fertilizer and soil conditioner.

[0026] The humic acid content of earthworm manure is between 21% and 40%, and it contains a variety of digestive enzymes and bacterial substances that neutralize the pH of the soil. It can increase the activity of neutral phosphate, protease, urease and sucrase in the soil, thereby improving the soil's fertilizer supply capacity, improving soil structure and balancing pH, which is ultimately reflected in the growth, development, yield and quality of crops.

[0027] Mushroom residue is very rich in nitrogen, phosphorus, potassium and organic matter, which is a source of nutrients for plants and energy for the life activities of soil microorganisms. It can effectively improve the low fertility of deep-sea mining soil. At the same time, it can also be used to form aggregates, increase soil porosity, and enhance nutrient preservation and water holding capacity.

[0028] Corn straw is rich in nitrogen, phosphorus, potassium, calcium, magnesium and organic matter. It is a multi-purpose renewable biological resource that can reduce soil bulk density, improve soil aggregate structure, increase soil porosity, reduce soil exchangeable acidity, and increase crop yields.

[0029] Diatomaceous earth can increase the number of soil aggregates, which can not only improve the physical and biological properties of the soil, reduce soil bulk density, increase soil porosity, but also improve soil water retention and air permeability, and improve the quantity and quality of organic matter in artificial soil.

[0030] Fly ash contains a variety of chemical nutrients required by plants, which promotes microbial activity in the soil, is conducive to nutrient conversion and heat preservation, makes water, fertilizer, air and heat move in a coordinated manner, and creates a good soil environment for crop growth. At the same time, the silicon, copper, zinc, molybdenum, calcium, iron, manganese, tungsten, selenium and other nutritional trace elements contained in fly ash increase the content of these nutrients in the soil and improve the soil nutrient status. Microbial agents can increase the abundance of microorganisms in the soil, and the activity of the bacterial community can increase the soil aggregate structure, reduce soil compaction, salinization and acidification, and promote root growth, improve the soil environment, loosen the soil and retain fertilizer.

[0031] Sawdust is added as a carbon source to the deep-sea sediment tailings cement, which can significantly increase the organic carbon content of artificial soil, effectively improve the problem of soil nutrient loss, increase the ability of soil to retain water and fertilizer, and at the same time, it can significantly increase the biological activity of microorganisms and improve the humification efficiency of organic matter in artificial soil. Shell powder is used to improve soil structure and increase the air permeability of artificial soil.

[0032] Compared with the prior art, the present invention brings the following beneficial technical effects:

[0033] (1) The present invention proposes a method for resource utilization of deep-sea mining tailings cement based on thermal drying. By subjecting the deep-sea mining tailings cement to a series of thermal drying processes, a dried product of deep-sea mining tailings cement is obtained, which can significantly reduce the volume, inhibit the activity of microorganisms, and eliminate pathogens, thereby achieving the purpose of "reduction and harmlessness". It will not produce rancidity, is easy to store and transport, and is suitable for use as an agricultural fertilizer and soil conditioner.

[0034] (2) The present invention proposes a method for resource utilization of deep-sea mining tailings cement based on thermal drying. Through aerobic fermentation, the soil's fertility capacity is improved, the defect of low fertility of deep-sea mining soil is improved, the biological activity of microorganisms is significantly increased, and the humification efficiency of soil organic matter is improved;

[0035] (3) The present invention proposes a method for resource utilization of deep-sea mining tailings cement based on thermal drying. Diatomaceous earth, fly ash and shell powder are added to the soil conditioner to promote the activity of microorganisms in the soil, improve the physical and biological properties of the soil, reduce the soil bulk density, increase the soil porosity, and improve the water retention and air permeability of the soil.

[0036] (4) The present invention proposes a method for resource utilization of deep-sea mining tailings cement based on thermal drying, wherein earthworm manure having a humic acid content of between 21% and 40% and containing a variety of digestive enzymes and bacterial substances that neutralize the pH of the soil is added to the soil conditioner, which can increase the activity of neutral phosphate, protease, urease and sucrase in the soil, improve the soil structure and balance the pH, neutralize the pH of the soil for planting on islands and reefs, floating cities and coastal areas, and thus be more suitable for crop growth. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The present invention will be further described below in conjunction with the accompanying drawings:

[0038] Figure 1 This is a schematic diagram of a method for resource utilization of deep-sea mining tailings cement based on thermal drying according to the present invention. DETAILED DESCRIPTION

[0039] The present invention discloses a method for resource utilization of deep-sea mining tailings cement based on thermal drying. In order to make the advantages and technical solutions of the present invention clearer and more specific, the present invention is further described below in conjunction with specific embodiments.

[0040] The raw materials described in the present invention can be purchased through commercial channels.

[0041] The present invention mainly utilizes deep-sea mining tailings cement as a resource. The deep-sea mining tailings cement is subjected to a series of thermal drying processes to obtain a dry product of deep-sea mining tailings cement, which can significantly reduce the volume, inhibit the activity of microorganisms, and eliminate pathogens, thereby achieving the purpose of "reduction and harmlessness". It will not produce odor, is easy to store and transport, and is suitable for use as an agricultural fertilizer and soil conditioner.

[0042] A method for resource utilization of deep-sea mining tailings cement based on thermal drying, comprising the following raw materials in parts by weight:

[0043] 100-150 parts of dried cement products from deep-sea mining tailings, 30-40 parts of earthworm castings, 50-70 parts of mushroom residues, 10-30 parts of corn stalks, 1-3 parts of microbial agents, 15-25 parts of sawdust, 15-20 parts of diatomaceous earth, 10-15 parts of fly ash, and 10-20 parts of shell powder.

[0044] Under the guidance of the above raw material combinations, other combinations can be easily obtained by those skilled in the art.

[0045] The present invention will be further described below in conjunction with specific embodiments. Example

[0046] A method for resource utilization of deep-sea mining tailings cement based on thermal drying, comprising the following raw materials in parts by weight:

[0047] 150 parts of dried cement products from deep-sea mining tailings, 35 parts of earthworm castings, 70 parts of mushroom residues, 10 parts of corn stalks, 3 parts of microbial agents, 15 parts of sawdust, 15 parts of diatomaceous earth, 15 parts of fly ash, and 10 parts of shell powder.

[0048] The preparation method is:

[0049] S1: Add one or more cationic flocculants and anionic flocculants to deep-sea mining tailings cement and stir and mix at a stirring rate of 100-200 r / min for 3-5 min, and let the mixture stand for 10-30 min to destroy the colloidal stability in the tailings cement and improve the dehydration performance of the tailings cement;

[0050] S2: placing the preliminarily dehydrated tailings cement in one of a belt filter press, a plate and frame filter press, and a centrifugal dehydrator, and performing a secondary mechanical dehydration treatment on the deep-sea mining tailings cement by one of a belt filter press, a plate and frame filter press, and a centrifugal dehydrator, so as to reduce the water content of the tailings cement to 10% to 15%, and obtain sediment tailings cement;

[0051] S3: Put the large-size sediment tail cement into a soil crusher to crush it into sediment tail cement with a particle size of less than 0.1 mm, so as to increase the specific surface area of ​​the sediment tail cement and improve the drying efficiency, and then spray an appropriate amount of water into the crushed sediment tail cement to ensure the humidity and uniformity of the sediment tail cement, which is conducive to the drying process;

[0052] S4: Add quicklime to the sediment tailings cement and stir and mix at a stirring rate of 100-200 r / min for 3-5 min, and send the pretreated tailings cement to a thermal drying device to evaporate the water in the tailings cement by utilizing the heat energy and the hydration reaction of quicklime to obtain a dried tailings cement product;

[0053] S5: Send the tailings cement drying product to the cooling equipment, cool it to 10-20 ℃ to prevent the product from overheating and oxidation, send the cooled tailings cement drying product to the soil grinder for grinding, grind the tailings cement drying product to a particle size of 100-200 meshes, and facilitate resource utilization;

[0054] S6: Mix the dried cement product of deep-sea mining tailings, earthworm castings, mushroom residue, corn stalks, microbial agents and sawdust in proportion, stir at a rate of 200-300 r / min for 3-5 min, add appropriate amount of water to obtain a mixture I, wherein the water content of the mixture I is 30%-40% and the pH is 6-7;

[0055] S7: The mixture is placed in an aerobic fermentation container, and the compost is turned for the first time after the high temperature period ends. Thereafter, the compost is turned once a week. The ventilation method adopts intermittent oxygen supply. The aeration is carried out at two time periods every day, 8:00-9:00 in the morning and 20:00-21:00 in the evening. The ventilation volume is 0.5 L / min and the duration is 1 hour. After fermentation for 1-2 months, mature materials and compost liquid are obtained;

[0056] S8: Mix the decomposed matter with diatomaceous earth, fly ash and shell powder at a stirring rate of 100-200 r / min for 3-5 min to obtain a mixture II, add the compost liquid to the mixture II and stir and mix at a stirring rate of 120-150 r / min for 2-3 min to obtain a soil conditioner;

[0057] S9: Add soil conditioners to the planting soil of islands, reefs, floating cities and coastal areas to improve the planting soil, increase the nutrients in the planting soil, improve the fertilizer supply capacity of the planting soil, and improve the planting soil structure, which will ultimately be reflected in the growth, development, yield and quality of crops.

[0058] The dried product of tailings cement is finally crushed to a particle size of less than 0.1 mm; Example

[0059] A method for resource utilization of deep-sea mining tailings cement based on thermal drying, comprising the following raw materials in parts by weight:

[0060] 150 parts of dried cement products from deep-sea mining tailings, 40 parts of earthworm castings, 60 parts of mushroom residues, 10 parts of corn stalks, 2 parts of microbial agents, 20 parts of sawdust, 20 parts of diatomaceous earth, 10 parts of fly ash, and 20 parts of shell powder.

[0061] The preparation method is:

[0062] S1: Add one or more cationic flocculants and anionic flocculants to deep-sea mining tailings cement and stir and mix at a stirring rate of 100-200 r / min for 3-5 min, and let the mixture stand for 10-30 min to destroy the colloidal stability in the tailings cement and improve the dehydration performance of the tailings cement;

[0063] S2: placing the preliminarily dehydrated tailings cement in one of a belt filter press, a plate and frame filter press, and a centrifugal dehydrator, and performing a secondary mechanical dehydration treatment on the deep-sea mining tailings cement by one of a belt filter press, a plate and frame filter press, and a centrifugal dehydrator, so as to reduce the water content of the tailings cement to 10% to 15%, and obtain sediment tailings cement;

[0064] S3: Put the large-size sediment tail cement into a soil crusher to crush it into sediment tail cement with a particle size of less than 0.1 mm, so as to increase the specific surface area of ​​the sediment tail cement and improve the drying efficiency, and then spray an appropriate amount of water into the crushed sediment tail cement to ensure the humidity and uniformity of the sediment tail cement, which is conducive to the drying process;

[0065] S4: Add quicklime to the sediment tailings cement and stir and mix at a stirring rate of 100-200 r / min for 3-5 min, and send the pretreated tailings cement to a thermal drying device to evaporate the water in the tailings cement by utilizing the heat energy and the hydration reaction of quicklime to obtain a dried tailings cement product;

[0066] S5: Send the tailings cement drying product to the cooling equipment, cool it to 10-20 ℃ to prevent the product from overheating and oxidation, send the cooled tailings cement drying product to the soil grinder for grinding, grind the tailings cement drying product to a particle size of 100-200 meshes, and facilitate resource utilization;

[0067] S6: Mix the dried cement product of deep-sea mining tailings, earthworm castings, mushroom residue, corn stalks, microbial agents and sawdust in proportion, stir at a rate of 200-300 r / min for 3-5 min, add appropriate amount of water to obtain a mixture I, wherein the water content of the mixture I is 30%-40% and the pH is 6-7;

[0068] S7: The mixture is placed in an aerobic fermentation container, and the compost is turned for the first time after the high temperature period ends. Thereafter, the compost is turned once a week. The ventilation method adopts intermittent oxygen supply. The aeration is carried out at two time periods every day, 8:00-9:00 in the morning and 20:00-21:00 in the evening. The ventilation volume is 0.5 L / min and the duration is 1 hour. After fermentation for 1-2 months, mature materials and compost liquid are obtained;

[0069] S8: Mix the decomposed matter with diatomaceous earth, fly ash and shell powder at a stirring rate of 100-200 r / min for 3-5 min to obtain a mixture II, add the compost liquid to the mixture II and stir and mix at a stirring rate of 120-150 r / min for 2-3 min to obtain a soil conditioner;

[0070] S9: Add soil conditioners to the planting soil of islands, reefs, floating cities and coastal areas to improve the planting soil, increase the nutrients in the planting soil, improve the fertilizer supply capacity of the planting soil, and improve the planting soil structure, which will ultimately be reflected in the growth, development, yield and quality of crops.

[0071] The dried product of tailings cement is finally crushed to a particle size of less than 0.1 mm; Example

[0072] A method for resource utilization of deep-sea mining tailings cement based on thermal drying, comprising the following raw materials in parts by weight:

[0073] 100 parts of dried cement products from deep-sea mining tailings, 30 parts of earthworm castings, 50 parts of mushroom residues, 30 parts of corn stalks, 1 part of microbial agent, 25 parts of sawdust, 15 parts of diatomaceous earth, 10 parts of fly ash, and 10 parts of shell powder.

[0074] The preparation method is:

[0075] S1: Add one or more cationic flocculants and anionic flocculants to deep-sea mining tailings cement and stir and mix at a stirring rate of 100-200 r / min for 3-5 min, and let the mixture stand for 10-30 min to destroy the colloidal stability in the tailings cement and improve the dehydration performance of the tailings cement;

[0076] S2: placing the preliminarily dehydrated tailings cement in one of a belt filter press, a plate and frame filter press, and a centrifugal dehydrator, and performing a secondary mechanical dehydration treatment on the deep-sea mining tailings cement by one of a belt filter press, a plate and frame filter press, and a centrifugal dehydrator, so as to reduce the water content of the tailings cement to 10% to 15%, and obtain sediment tailings cement;

[0077] S3: Put the large-size sediment tail cement into a soil crusher to crush it into sediment tail cement with a particle size of less than 0.1 mm, so as to increase the specific surface area of ​​the sediment tail cement and improve the drying efficiency, and then spray an appropriate amount of water into the crushed sediment tail cement to ensure the humidity and uniformity of the sediment tail cement, which is conducive to the drying process;

[0078] S4: Add quicklime to the sediment tailings cement and stir and mix at a stirring rate of 100-200 r / min for 3-5 min, and send the pretreated tailings cement to a thermal drying device to evaporate the water in the tailings cement by utilizing the heat energy and the hydration reaction of quicklime to obtain a dried tailings cement product;

[0079] S5: Send the tailings cement drying product to the cooling equipment, cool it to 10-20 ℃ to prevent the product from overheating and oxidation, send the cooled tailings cement drying product to the soil grinder for grinding, grind the tailings cement drying product to a particle size of 100-200 meshes, and facilitate resource utilization;

[0080] S6: Mix the dried cement product of deep-sea mining tailings, earthworm castings, mushroom residue, corn stalks, microbial agents and sawdust in proportion, stir at a rate of 200-300 r / min for 3-5 min, add appropriate amount of water to obtain a mixture I, wherein the water content of the mixture I is 30%-40% and the pH is 6-7;

[0081] S7: The mixture is placed in an aerobic fermentation container, and the compost is turned for the first time after the high temperature period ends. Thereafter, the compost is turned once a week. The ventilation method adopts intermittent oxygen supply. The aeration is carried out at two time periods every day, 8:00-9:00 in the morning and 20:00-21:00 in the evening. The ventilation volume is 0.5 L / min and the duration is 1 hour. After fermentation for 1-2 months, mature materials and compost liquid are obtained;

[0082] S8: Mix the decomposed matter with diatomaceous earth, fly ash and shell powder at a stirring rate of 100-200 r / min for 3-5 min to obtain a mixture II, add the compost liquid to the mixture II and stir and mix at a stirring rate of 120-150 r / min for 2-3 min to obtain a soil conditioner;

[0083] S9: Add soil conditioners to the planting soil of islands, reefs, floating cities and coastal areas to improve the planting soil, increase the nutrients in the planting soil, improve the fertilizer supply capacity of the planting soil, and improve the planting soil structure, which will ultimately be reflected in the growth, development, yield and quality of crops.

[0084] The dried product of tailings cement is finally crushed to a particle size less than 0.1mm;

[0085] The present invention selects natural unimproved planting soil as a control group. After the soil improver prepared by using the deep-sea mining tailings cement drying product in the above Examples 1, 2, and 3 is applied to the planting soil, the effect of the present invention is illustrated by an indoor planting test:

[0086] As can be seen from Table 1, the ammonium nitrogen of the control group was 185 mg / Kkg, the available phosphorus was 241 mg / Kkg, the available potassium was 402 mg / Kkg, and the organic matter was 1.732 g / Kkg; however, the ammonium nitrogen of the improved soil of the test group 1 of the present invention was 1534 mg / Kkg, the available phosphorus was 1793 mg / Kkg, the available potassium was 2653 mg / Kkg, and the organic matter was 15.952 g / Kkg; the ammonium nitrogen of the improved soil of the test group 2 of the present invention was 1246 mg / Kkg, the available phosphorus was 1265 mg / Kkg, the available potassium was 1969 mg / Kkg, and the organic matter was 13.424 g / Kkg; the ammonium nitrogen of the improved soil of the test group 3 of the present invention was 1263 mg / Kkg, the available phosphorus was 13558 mg / Kkg, the available potassium was 2093 mg / Kkg, and the organic matter was 13.264 g / Kkg; This shows that after the soil conditioners prepared by using the dried products of deep-sea mining tailings cement in the three embodiments were applied to the planting soil, the soil nutrients were significantly increased.

[0087] Table 1 Nutrient index test table

[0088] deal with Ammonium nitrogen (mg / Kkg) Available phosphorus (mg / Kkg) Fast-acting potassium (mg / Kkg) Organic matter (g / Kkg) Control group 185 241 402 1.732 Experimental Group 1 1534 1793 2653 15.952 Experimental Group 2 1246 1265 1969 13.424 Experimental Group 3 1263 1358 2093 13.264

[0089] The present invention utilizes the dried product of deep-sea mining tailings cement in synergistic aerobic fermentation to prepare a soil conditioner, which can not only effectively improve the soil structure, balance the pH value, and increase the soil's fertilizer supply capacity, but also can utilize the deep-sea mining tailings cement as a resource, thereby protecting the environment and bringing economic benefits.

[0090] Those skilled in the art should recognize that the above embodiments are only used to illustrate the present application and are not intended to be limiting of the present application. As long as they are within the spirit and scope of the present application, appropriate changes and modifications to the above embodiments are within the scope of protection claimed in the present application.

Claims

1. A method for resource utilization of deep-sea mining tailings cement based on thermal drying, It is characterized in that The following steps are involved: S1: adding one or more cationic flocculants and anionic flocculants to deep-sea mining tailings cement and stirring and mixing, the stirring rate is 100-200r / min, the stirring time is 3-5min, and the mixture is allowed to stand for 10-30min to destroy the colloidal stability in the tailings cement and improve the dehydration performance of the tailings cement; S2: placing the preliminarily dehydrated tailings cement in one of a belt filter press, a plate and frame filter press, and a centrifugal dehydrator, and performing a secondary mechanical dehydration treatment on the deep-sea mining tailings cement by one of a belt filter press, a plate and frame filter press, and a centrifugal dehydrator to reduce the moisture content of the tailings cement to 10% to 15%, thereby obtaining deposited tailings cement; S3: Put the large-particle sediment tail cement into a soil crusher and crush it into sediment tail cement with a particle size less than 0.1mm, so as to increase the specific surface area of ​​the sediment tail cement and improve the drying efficiency, and then spray an appropriate amount of water into the crushed sediment tail cement to ensure the humidity and uniformity of the sediment tail cement, which is conducive to the drying process; S4: add quicklime to the deposited tail cement and stir and mix, the stirring speed is 100-200r / min, the stirring time is 3-5min, the pretreated tail cement is sent to the thermal drying equipment, the water in the tail cement is evaporated by the hydration reaction of heat energy and quicklime, and the tail cement drying product is obtained; S5: sending the tail cement drying product to a cooling device, cooling it to 10-20° C. to prevent the product from overheating and oxidation, sending the cooled tail cement drying product to a soil grinder for grinding, and grinding the tail cement drying product to a particle size of 100-200 meshes for easy resource utilization; S6: mixing the dried cement product of deep-sea mining tailings, earthworm castings, mushroom residue, corn stalks, microbial agents, and sawdust in proportion, stirring at a rate of 200-300 r / min for 3-5 min, adding an appropriate amount of water to obtain a mixture I, wherein the water content of the mixture I is 30%-40% and the pH is 6-7; S7: placing the mixture into an aerobic fermentation container, turning the compost for the first time after the high temperature period, and then turning the compost once a week, using intermittent oxygen supply, ventilation at 8:00-9:00 in the morning and 20:00-21:00 in the evening every day, ventilation at a rate of 0.5 L / min, duration of 1 hour, fermentation for 1-2 months to obtain mature material and compost liquid; S8: mixing the decomposed matter with diatomaceous earth, fly ash and shell powder at a stirring rate of 100-200 r / min for 3-5 min to obtain a mixture II, adding compost liquid to the mixture II and stirring and mixing at a stirring rate of 120-150 r / min for 2-3 min to obtain a soil conditioner; S9: Add soil conditioners to the planting soil of islands, reefs, floating cities and coastal areas to improve the planting soil, increase the nutrients in the planting soil, improve the fertilizer supply capacity of the planting soil, and improve the planting soil structure, which will ultimately be reflected in the growth, development, yield and quality of crops.

2. A method for resource utilization of deep-sea mining tailings cement based on thermal drying according to claim 1, It is characterized in that According to weight parts, Including the following ingredients: 100-150 parts of dried cement products from deep-sea mining tailings, 30-40 parts of earthworm manure, 50-70 parts of mushroom residue, 10-30 parts of corn stalks, 15-20 parts of diatomaceous earth, 10-15 parts of fly ash, 1-3 parts of microbial agent, 15-25 parts of sawdust, and 10-20 parts of shell powder; The mushroom residue is the residue from the cultivation of one or more of black fungus, enoki mushroom, king oyster mushroom and white enoki mushroom; The microbial agent comprises one or more of bacillus, photosynthetic bacteria, yeast, lactic acid bacteria, and nitrogen-fixing bacteria; The shell powder is prepared by grinding one or more of the shells of marine organisms such as clam shells, oyster shells and mussel shells.

3. A method for resource utilization of deep-sea mining tailings cement based on thermal drying according to claim 1, It is characterized in that The fly ash particle size is 200-400 meshes.

4. A method for resource utilization of deep-sea mining tailings cement based on thermal drying according to claim 1, It is characterized in that The particle size of the shell powder is less than 0.1 mm.

5. A method for resource utilization of deep-sea mining tailings cement based on thermal drying according to claim 1, It is characterized in that The dried product of tail cement is finally crushed into particles with a diameter less than 0.1 mm.