Flame retardant antistatic polyurethane elastomer and preparation method thereof

The conductive network and flame retardant protective layer are formed by introducing N-(β-aminoethyl)-γ-aminopropyltriethoxysilane and elolite nanotube-ammonium polyphosphate composites into the cast polyurethane elastomer. , solves the flammable and static problems of polyurethane elastomers, and achieves efficient flame retardant and antistatic performance improvements.

CN118222085BActive Publication Date: 2024-11-15SHENZHEN LIXIN LUNAN RUBBER & PLASTIC HARDWARE
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410435617.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-11
Publication Date
2024-11-15
Estimated Expiration
2044-04-11

AI Technical Summary

Technical Problem

Cast polyurethane elastomers are flammable and prone to static electricity, resulting in fire and explosion risks, and cannot meet the requirements of flame retardant and antistatic properties.

Method used

Using raw materials such as N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, carbon black, Elosite nanotube-ammonium polyphosphate composites, etc., to form a conductive network and flame retardant through specific preparation processes Protective layer to improve the flame retardancy and antistatic properties of the material.

Benefits of technology

It significantly improves the flame retardant and antistatic properties of the material, reduces the risk of static accumulation and discharge, meets the requirements of flame retardant and antistatic properties, and has environmentally friendly preparation process, simple operation, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004787104760000102
    Figure BDA0004787104760000102
  • Figure BDA0004787104760000111
    Figure BDA0004787104760000111
  • Figure BDA0004787104760000122
    Figure BDA0004787104760000122
Patent Text Reader

Abstract

The present application discloses a flame retardant antistatic polyurethane elastomer and a preparation method. The flame retardant antistatic polyurethane elastomer includes the following raw materials by weight: 100135 parts of cast polyurethane elastomer, 35 parts of N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, 918 parts of carbon black, 612 parts of halloysite nanotube-ammonium polyphosphate complex, 25-30 parts of ethyl acetate, 5-8 parts of diethylene glycol dibenzoate, 1.5-3 parts of dilauryl thiodipropionate, and 0.5-2 parts of lubricant. The flame retardant antistatic polyurethane elastomer provided in the present application has the advantages of good flame retardancy and good antistatic performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer materials, and in particular to a flame retardant and antistatic polyurethane elastomer and a preparation method thereof. Background Art

[0002] Cast polyurethane elastomers have shown a wide range of application potential due to their flexible and adaptable raw material formulas. By fine-tuning the original formula, various physical properties can be customized in different application scenarios. For example, they can be transformed from a soft sponge to an elastic solid. They can also be used in coatings, sealants, sole composite materials and even stretch fibers, significantly improving their commercial application value.

[0003] However, it is worth noting that unmodified cast polyurethane elastomer materials have flammable characteristics, and their limiting oxygen index value is about 18%, which is far below the standard threshold required for flame retardant materials. Both international and domestic regulations clearly stipulate that polyurethane products used in public facilities or places must meet strict flame retardant performance requirements. In view of this, the research and development and production of polyurethane composite materials with flame retardant properties have great practical value and social significance in actual production and life.

[0004] In addition, due to its insulating properties, cast polyurethane elastomers are prone to generate static electricity due to friction during actual operation, and static electricity is not easy to release on its own. The accumulated static electricity can easily cause short circuits in electrical equipment and even cause fire accidents. In extreme cases, it may also cause explosion risks. Summary of the invention

[0005] In order to solve at least one of the above technical problems, a flame retardant and antistatic polyurethane elastomer with good flame retardancy and antistatic performance is developed. The present application provides a flame retardant and antistatic polyurethane elastomer and a preparation method thereof.

[0006] In a first aspect, the present application provides a flame retardant antistatic polyurethane elastomer, which comprises the following raw materials in parts by weight: 100135 parts of cast polyurethane elastomer, 35 parts of N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, 918 parts of carbon black, 612 parts of halloysite nanotube-ammonium polyphosphate composite, 25-30 parts of ethyl acetate, 5-8 parts of diethylene glycol dibenzoate, 1.5-3 parts of dilauryl thiodipropionate, and 0.5-2 parts of lubricant;

[0007] The preparation method of the halloysite nanotube-ammonium polyphosphate composite comprises the following steps:

[0008] A1. Add a hydrochloric acid solution with a concentration of (3-5) mol / L to the halloysite nanotubes, heat and stir in a water bath for 6-8 hours, centrifuge to separate the solid matter, and wash and grind the solid matter to obtain the halloysite nanotubes after hydrochloric acid etching;

[0009] A2, mixing the hydrochloric acid-etched halloysite nanotubes obtained in step A1, ammonium polyphosphate and water, and ultrasonically dispersing them for 40-60 minutes in an ice bath, and then vacuum-treating the obtained suspension, wherein the vacuum treatment is as follows: when the vacuum degree reaches -0.1 MPa, maintain it for 30-45 minutes, and then return to normal pressure;

[0010] A3. After the vacuum treatment, centrifuge to separate the solid phase, wash the solid phase, vacuum dry for 24-30 hours, and grind into powder to obtain the hydrochloric acid-etched halloysite nanotubes loaded with ammonium polyphosphate;

[0011] A4, mixing a polyethyleneimine solution having a concentration of (3-5) mg / mL and the ammonium polyphosphate loaded on the halloysite nanotubes after hydrochloric acid etching obtained in step A3, stirring for 20-30 min, centrifuging to separate the solid phase, and washing the solid phase to complete the first layer of encapsulation;

[0012] A5. After the first layer of encapsulation is completed, add a sodium polystyrene sulfonate solution with a concentration of (3-5) mg / mL, stir for 10-15 minutes, centrifuge, separate the solid phase, and wash the solid phase to complete the second layer of encapsulation;

[0013] A6. After the second layer of encapsulation is completed, the mixture is dried for 24-26 hours and ground into powder to obtain the halloysite nanotube-ammonium polyphosphate composite.

[0014] By adopting the above technical scheme, the flame retardant and antistatic polyurethane elastomer in the present application combines the advantages of multiple raw materials to achieve the improvement of flame retardancy and antistatic properties. Specifically, the cast polyurethane elastomer provides basic mechanical properties and processing properties. The cast polyurethane elastomer has good elasticity and wear resistance, which is the basis for the flame retardant and antistatic polyurethane elastomer. N-(β-aminoethyl)-γ-aminopropyltriethoxysilane can form a chemical bond with the cast polyurethane elastomer. The introduction of silane can also improve the surface properties of the cast polyurethane elastomer, reduce surface resistance, reduce the accumulation and discharge of static electricity, thereby enhancing the antistatic properties of the elastomer. Carbon black is a nanomaterial with a high specific surface area and conductive properties. In the cast polyurethane elastomer, carbon black is modified by N-(β-aminoethyl)-γ-aminopropyltriethoxysilane and can be evenly dispersed in the cast polyurethane elastomer, thereby being closely combined with the cast polyurethane elastomer, forming a conductive network in the cast polyurethane elastomer, and improving the conductivity of the material. At the same time, carbon black and halloysite nanotube-ammonium polyphosphate composite are compounded and used in halloysite nanotubes, which will further improve the flame retardancy of cast polyurethane elastomer. In the present application, the preparation process of halloysite nanotube-ammonium polyphosphate composite is unique and fine, and the etching of the inner wall of halloysite nanotube, the loading of ammonium polyphosphate and the encapsulation of the composite are realized through a series of steps, thereby significantly improving the flame retardancy and stability of halloysite nanotube-ammonium polyphosphate composite. First, hydrochloric acid is selected to etch the aluminum layer of the inner wall of halloysite nanotube, which increases the specific surface area of ​​halloysite nanotube, so that more ammonium polyphosphate can be loaded. The reason is that, by the etching effect of hydrochloric acid, part of the aluminum layer of the inner wall of halloysite nanotube can be effectively removed, thereby increasing the roughness and activity of its surface, and improving its adsorption capacity for ammonium polyphosphate. Secondly, the present application uses vacuum loading method to encapsulate ammonium polyphosphate in the halloysite nanotube after hydrochloric acid etching. The present application uses vacuum loading method to make ammonium polyphosphate fully penetrate into the inside of halloysite nanotube, and realize efficient loading. At the same time, since the halloysite nanotubes have a larger specific surface area after hydrochloric acid etching, more ammonium polyphosphate can be loaded, thereby improving the flame retardant properties of the composite. In addition, the present application encapsulates the halloysite nanotube-ammonium polyphosphate composite by adsorbing positive and negative polyelectrolytes, and the adsorption of positive and negative polyelectrolytes can form a stable coating layer on the surface of the composite, effectively preventing the rapid release of ammonium polyphosphate in the early stage. In this way, not only can the service life of the composite be extended, but also its performance fluctuations during use can be reduced. Thereby, the initial release rate of ammonium polyphosphate can be reduced well, and its controlled release effect can be achieved. The present application successfully prepared the halloysite nanotube-ammonium polyphosphate composite through the above-mentioned preparation process, and significantly improved its flame retardant properties and stability. This composite can play an excellent flame retardant role during the combustion process, effectively preventing the spread of flames and the entry of oxygen.At the same time, its controlled release effect also makes the release of ammonium polyphosphate more uniform and lasting, further improving the flame retardant effect. In addition, the preparation process of the present application also has the advantages of environmental friendliness and easy operation. The raw materials used are all non-toxic or low-toxic substances, and no harmful chemicals need to be used in the preparation process. At the same time, the preparation steps are relatively simple and easy to achieve large-scale production. In summary, the present application successfully prepared a halloysite nanotube-ammonium polyphosphate complex with excellent flame retardant performance and stability by selecting hydrochloric acid to etch the halloysite nanotubes, using the vacuum loading method to load ammonium polyphosphate, and encapsulating by adsorbing positive and negative polyelectrolytes. Diethylene glycol dibenzoate can improve the processing performance and flexibility of cast polyurethane elastomers. By adding an appropriate amount of diethylene glycol dibenzoate, the viscosity of the elastomer can be reduced, and its fluidity during processing can be improved while maintaining its good physical properties. Dilauryl thiodipropionate improves its thermal stability and antioxidant properties. By reducing the occurrence of thermal oxidative degradation, dilauryl thiodipropionate can extend the service life of flame retardant antistatic polyurethane elastomers. Lubricants improve the processing of cast polyurethane elastomers. They reduce friction between the elastomer and the mold, making demolding more efficient without negatively affecting the properties of the elastomer.

[0015] Optionally, the weight ratio of the halloysite nanotubes to the hydrochloric acid solution in step A1 is (5-8): (80-100);

[0016] The weight ratio of the ammonium polyphosphate and water in step A2 to the halloysite nanotubes in step A1 is (8-10): (50-100): 1;

[0017] The weight ratio of the polyethyleneimine solution, the halloysite nanotubes loaded with ammonium polyphosphate after hydrochloric acid etching and the sodium polystyrene sulfonate solution in step A4 is (4-6):1:(4-6).

[0018] Optionally, the weight ratio of the carbon black to the halloysite nanotube-ammonium polyphosphate composite is (1.2-1.7):1.

[0019] By adopting the above technical scheme, when the weight ratio of carbon black and halloysite nanotube-ammonium polyphosphate complex is (1.2-1.7): 1, the comprehensive performance of the obtained urethane elastomer is better. First, carbon black is connected with N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, which can form a dense and uniform conductive network in the cast polyurethane elastomer, thereby improving the antistatic properties of the material. However, too high a carbon black content may cause agglomeration and affect the uniformity and stability of the conductive network. On the other hand, as a flame retardant, the content of the halloysite nanotube-ammonium polyphosphate complex has an important influence on the flame retardant properties of the elastomer. An appropriate amount of halloysite nanotube-ammonium polyphosphate complex can effectively improve the flame retardant properties of the elastomer, so that it can form a dense protective layer during the combustion process to prevent the spread of flames. In addition, the halloysite nanotube-ammonium polyphosphate complex is a highly effective flame retardant. When ammonium polyphosphate burns, it can decompose to produce compounds such as phosphoric acid. These compounds can cover the surface of the material to form a dense protective layer, effectively isolating the transfer of heat and preventing the spread of flames. As a carrier, halloysite nanotubes can load more ammonium polyphosphate and evenly disperse the flame retardant in the material through its unique tubular structure. When carbon black is compounded with the halloysite nanotube-ammonium polyphosphate complex, carbon black can form a stable carbon layer structure at high temperatures. This carbon layer structure is denser and can better isolate oxygen and heat, thereby further improving the flame retardant properties of the material and improving the material's ability to resist the spread of flames when burning.

[0020] Optionally, the weight ratio of the carbon black to the halloysite nanotube-ammonium polyphosphate composite is 1.5:1.

[0021] Preferably, the total weight of the carbon black and the halloysite nanotube-ammonium polyphosphate composite accounts for (14.91-17.96)% of the flame retardant antistatic polyurethane elastomer.

[0022] By adopting the above technical solution, when carbon black and halloysite nanotube-ammonium polyphosphate composite are used as important additives for flame retardant and antistatic polyurethane elastomer, their content has a significant effect on the flame retardant and antistatic properties of the material. When their total weight accounts for (14.91-17.96)% of the elastomer, it can ensure that the material forms an effective protective layer during combustion to prevent the spread of flames, while maintaining excellent antistatic properties to prevent the accumulation and discharge of static electricity.

[0023] Optionally, the vacuum drying in step A2 is performed twice.

[0024] By adopting the above technical solution, the present application can significantly improve the loading amount and distribution uniformity of ammonium polyphosphate on the inner wall of halloysite nanotubes by performing vacuum drying in step A2 twice, thereby achieving a better flame retardant effect.

[0025] Optionally, the centrifugation conditions in step A3 are as follows: centrifugal speed is 4000-5000 r / min, and centrifugal time is 5-10 min.

[0026] Optionally, the lubricant is selected from zinc stearate.

[0027] In a second aspect, the present application provides a method for preparing a flame retardant and antistatic polyurethane elastomer, the preparation method comprising the following steps:

[0028] S1, dissolving N-(β-aminoethyl)-γ-aminopropyltriethoxysilane in ethyl acetate, adding carbon black, ultrasonicating for 30-45 min, removing the remaining ethyl acetate, and obtaining N-(β-aminoethyl)-γ-aminopropyltriethoxysilane modified carbon black;

[0029] S2. Add the remaining raw materials to the N-(β-aminoethyl)-γ-aminopropyltriethoxysilane modified carbon black obtained in step S1, mix and stir for (130-150) min, extrude and granulate to obtain the flame retardant antistatic polyurethane elastomer.

[0030] By adopting the above technical scheme, the preparation method of the flame retardant and antistatic polyurethane elastomer provided by the present application can achieve uniform mixing and effective dispersion of raw materials, ensuring that the elastomer has excellent flame retardant and antistatic properties. At the same time, the method is simple to operate and has strong controllability, and is suitable for industrial production. The flame retardant and antistatic polyurethane elastomer obtained significantly improves the flame retardant and antistatic properties while maintaining the original mechanical properties and processing properties, and has broad application prospects.

[0031] Optionally, the temperature of each zone in the extrusion granulation is 180° C. to 200° C., and the rotation speed is 500 to 800 r / min.

[0032] In summary, the present invention includes at least one of the following beneficial technical effects:

[0033] 1. The flame retardant and antistatic polyurethane elastomer in this application combines the advantages of multiple raw materials to achieve the improvement of flame retardancy and antistatic properties. Specifically, the cast polyurethane elastomer provides basic mechanical properties and processing properties. The cast polyurethane elastomer has good elasticity and wear resistance, and is the basis for the flame retardant and antistatic polyurethane elastomer. N-(β-aminoethyl)-γ-aminopropyltriethoxysilane can form a chemical bond with the cast polyurethane elastomer. The introduction of silane can also improve the surface properties of the cast polyurethane elastomer, reduce surface resistance, reduce the accumulation and discharge of static electricity, and thus enhance the antistatic properties of the elastomer. Carbon black is a nanomaterial with a high specific surface area and conductive properties. In the cast polyurethane elastomer, carbon black is modified by N-(β-aminoethyl)-γ-aminopropyltriethoxysilane and can be evenly dispersed in the cast polyurethane elastomer, thereby being closely combined with the cast polyurethane elastomer, forming a conductive network in the cast polyurethane elastomer, and improving the conductivity of the material. At the same time, carbon black and halloysite nanotube-ammonium polyphosphate composite are combined with halloysite nanotubes for compounding and use, which will further improve the flame retardancy of cast polyurethane elastomer. In the present application, the preparation process of halloysite nanotube-ammonium polyphosphate composite is unique and fine, and the etching of the inner wall of halloysite nanotube, the loading of ammonium polyphosphate and the encapsulation of the composite are realized through a series of steps, thereby significantly improving the flame retardancy and stability of the composite. First, hydrochloric acid is selected to etch the aluminum layer of the inner wall of halloysite nanotube, which increases the specific surface area of ​​halloysite nanotube, so that more ammonium polyphosphate can be loaded. The reason is that, by the etching effect of hydrochloric acid, part of the aluminum layer of the inner wall of halloysite nanotube can be effectively removed, thereby increasing the roughness and activity of its surface, and improving its adsorption capacity for ammonium polyphosphate. Secondly, the present application uses vacuum loading method to encapsulate ammonium polyphosphate in the halloysite nanotube after hydrochloric acid etching. The present application uses vacuum loading method to make ammonium polyphosphate fully penetrate into the inside of halloysite nanotube, and realize efficient loading. At the same time, since the halloysite nanotubes have a larger specific surface area after hydrochloric acid etching, more ammonium polyphosphate can be loaded, thereby improving the flame retardant properties of the composite. In addition, the present application encapsulates the halloysite nanotube-ammonium polyphosphate composite by adsorbing positive and negative polyelectrolytes, and the adsorption of positive and negative polyelectrolytes can form a stable coating layer on the surface of the composite, effectively preventing the rapid release of ammonium polyphosphate in the early stage. In this way, not only can the service life of the composite be extended, but also its performance fluctuations during use can be reduced. Thereby, the initial release rate of ammonium polyphosphate can be reduced well, and its controlled release effect can be achieved. The present application successfully prepared the halloysite nanotube-ammonium polyphosphate composite through the above-mentioned preparation process, and significantly improved its flame retardant properties and stability. This composite can play an excellent flame retardant role during the combustion process, effectively preventing the spread of flames and the entry of oxygen.At the same time, its controlled release effect also makes the release of ammonium polyphosphate more uniform and lasting, further improving the flame retardant effect. In addition, the preparation process of the present application also has the advantages of environmental friendliness and easy operation. The raw materials used are all non-toxic or low-toxic substances, and no harmful chemicals need to be used in the preparation process. At the same time, the preparation steps are relatively simple and easy to achieve large-scale production. In summary, the present application successfully prepares the halloysite nanotube-ammonium polyphosphate complex with excellent flame retardant performance and stability by selecting hydrochloric acid to etch halloysite nanotubes, utilizing vacuum loading method to load ammonium polyphosphate, and encapsulating by adsorbing positive and negative polyelectrolytes.

[0034] Diethylene glycol dibenzoate improves the processing properties and flexibility of cast polyurethane elastomers. By adding the right amount of diethylene glycol dibenzoate, the viscosity of the elastomer can be reduced, improving its fluidity during processing while maintaining its good physical properties. Dilauryl thiodipropionate improves its thermal stability and antioxidant properties. Dilauryl thiodipropionate can extend the service life of flame retardant and antistatic polyurethane elastomers by reducing the occurrence of thermo-oxidative degradation. Lubricants can improve the processing properties of cast polyurethane elastomers. It can reduce the friction between the elastomer and the mold and improve the demolding efficiency without negatively affecting the properties of the elastomer.

[0035] 2. When the weight ratio of carbon black and halloysite nanotube-ammonium polyphosphate complex is (1.2-1.7):1, the comprehensive performance of the obtained urethane elastomer is better. Halloysite nanotube-ammonium polyphosphate complex is a highly efficient flame retardant. Ammonium polyphosphate can decompose to produce compounds such as phosphoric acid when burning. These compounds can cover the surface of the material to form a dense protective layer, effectively isolating the transfer of heat and preventing the spread of flames. As a carrier, halloysite nanotubes can load more ammonium polyphosphate and evenly disperse the flame retardant in the material through its unique tubular structure. When carbon black is compounded with halloysite nanotube-ammonium polyphosphate complex, carbon black can form a stable carbon layer structure at high temperature. This carbon layer structure is denser and can better isolate oxygen and heat, thereby further improving the flame retardant properties of the material and improving the material's ability to resist the spread of flames when burning.

[0036] 3. When carbon black and halloysite nanotube-ammonium polyphosphate composite are used as important additives for flame retardant and antistatic polyurethane elastomer, their content has a significant effect on the flame retardant and antistatic properties of the material. When their total weight accounts for (8.5-10)% of the elastomer, it can ensure that the material forms an effective protective layer during combustion to prevent the spread of flames, while maintaining excellent antistatic properties to prevent the accumulation and discharge of static electricity.

[0037] 4. The preparation method of the flame-retardant and antistatic polyurethane elastomer provided in the present application can achieve uniform mixing and effective dispersion of raw materials, ensuring that the elastomer has excellent flame retardant and antistatic properties. At the same time, the method is simple to operate and has strong controllability, and is suitable for industrial production. The flame-retardant and antistatic polyurethane elastomer prepared significantly improves the flame retardant and antistatic properties while maintaining the original mechanical properties and processing properties, and has broad application prospects. DETAILED DESCRIPTION

[0038] The present application is further described in detail below with reference to the embodiments.

[0039] Casting polyurethane elastomer: Shanghai Xuchun Chemical Technology Co., Ltd.

[0040] N-(β-aminoethyl)-γ-aminopropyltriethoxysilane: CAS number is 5089-72-5, and the active ingredient content is 99%.

[0041] Carbon black: CAS number is 10279-57-9, purity is 99%.

[0042] Halloysite nanotubes: Shijiazhuang Dinglei Mineral Products Trading Co., Ltd., item number 081265.

[0043] Ammonium polyphosphate: CAS number is 68333-79-9, purity is 99%.

[0044] Ethyl acetate: CAS number is 141-78-6, purity is 99%.

[0045] Diethylene glycol dibenzoate: CAS number is 120-55-8, purity is 99%.

[0046] Dilauryl thiodipropionate: CAS number is 123-28-4, purity is 99%.

[0047] Zinc stearate: CAS number is 557-05-1, purity is 99%.

[0048] Hydrochloric acid: Maoming Runjing Chemical Co., Ltd.

[0049] Sodium polystyrene sulfonate: CAS number is 9080-79-9, purity is 99%.

[0050] Polyethyleneimine: CAS No. 9002-98-6, purity 99%. Hubei Jusheng Technology Co., Ltd. Specific embodiments

[0052] Preparation Example 1-3

[0053] Preparation Example 1

[0054] This preparation example provides a halloysite nanotube-ammonium polyphosphate composite, and the preparation method comprises the following steps:

[0055] A1. Add 160 g of 4 mol / L hydrochloric acid solution to 10 g of halloysite nanotubes, heat and stir for 6 h in a water bath, centrifuge to separate solid matter, and wash and grind the solid matter with deionized water to obtain halloysite nanotubes etched with hydrochloric acid;

[0056] A2, the hydrochloric acid-etched halloysite nanotubes obtained in step A1, 80 g of ammonium polyphosphate and 500 g of water were mixed, and ultrasonically dispersed for 40 min in an ice bath, and the obtained suspension was vacuum treated twice, each vacuum treatment was as follows: when the vacuum degree reached -0.1 MPa, it was maintained for 30-45 min, and then returned to normal pressure;

[0057] A3. After the vacuum treatment, centrifuge at a speed of 4000 r / min for 5 min to separate the solid phase, wash the solid phase (using ethanol for 2 times), vacuum dry for 24 h and grind into powder to obtain hydrochloric acid-etched halloysite nanotubes loaded with ammonium polyphosphate;

[0058] A4, 40 g of a 3 mg / mL polyethyleneimine solution and 10 g of the hydrochloric acid-etched halloysite nanotube-loaded ammonium polyphosphate obtained in step A3 were mixed, stirred for 20 min, centrifuged, the solid phase was separated, and the solid phase was washed (with deionized water) to complete the first layer of encapsulation;

[0059] A5. After the first layer of encapsulation is completed, 40 g of a 3 mg / mL sodium polystyrene sulfonate solution is added, stirred for 10 min, centrifuged, the solid phase is separated, and the solid phase is washed (washed with deionized water) to complete the second layer of encapsulation;

[0060] A6. After the second layer of encapsulation is completed, the mixture is dried for 24 hours and ground into powder to obtain the halloysite nanotube-ammonium polyphosphate composite;

[0061] Preparation Example 2

[0062] The difference between this preparation example and preparation example 1 is that the preparation method of the halloysite nanotube-ammonium polyphosphate composite in this preparation example comprises the following steps:

[0063] A1. Add 129 g of 4 mol / L hydrochloric acid solution to 10 g of halloysite nanotubes, heat and stir for 7 h in a water bath, centrifuge to separate solid matter, and wash and grind the solid matter with deionized water to obtain halloysite nanotubes etched with hydrochloric acid;

[0064] A2, the hydrochloric acid-etched halloysite nanotubes obtained in step A1, 90 g of ammonium polyphosphate and 800 g of water were mixed, and ultrasonically dispersed for 50 min in an ice bath, and the obtained suspension was vacuum treated twice, each vacuum treatment was as follows: when the vacuum degree reached -0.1 MPa, it was maintained for 30-45 min, and then returned to normal pressure;

[0065] A3. After vacuum drying, centrifuge at a speed of 4500 r / min for 8 min to separate the solid phase, wash the solid phase (using ethanol for 2 times), vacuum dry for 26 h, and grind into powder to obtain hydrochloric acid-etched halloysite nanotubes loaded with ammonium polyphosphate;

[0066] A4, 50 g of a 4 mg / mL polyethyleneimine solution and 10 g of the hydrochloric acid-etched halloysite nanotube-loaded ammonium polyphosphate obtained in step A3 were mixed, stirred for 25 min, centrifuged, the solid phase was separated, and the solid phase was washed (with deionized water) to complete the first layer of encapsulation;

[0067] A5. After the first layer of encapsulation is completed, 50 g of a sodium polystyrene sulfonate solution with a concentration of 4 mg / mL is added, stirred for 12 min, centrifuged, the solid phase is separated, and the solid phase is washed (using deionized water) to complete the second layer of encapsulation to obtain a composite;

[0068] A6. After the second layer of encapsulation is completed, the mixture is dried for 25 hours and ground into powder to obtain the halloysite nanotube-ammonium polyphosphate composite;

[0069] Preparation Example 3

[0070] A1. Add 125 g of 4 mol / L hydrochloric acid solution to 10 g of halloysite nanotubes, heat and stir for 8 h in a water bath, centrifuge to separate solid matter, and wash and grind the solid matter with deionized water to obtain halloysite nanotubes etched with hydrochloric acid;

[0071] A2, the hydrochloric acid-etched halloysite nanotubes obtained in step A1, 100 g of ammonium polyphosphate and 1000 g of water were mixed, and ultrasonically dispersed for 60 min in an ice bath, and the obtained suspension was vacuum treated twice, each vacuum treatment was as follows: when the vacuum degree reached -0.1 MPa, it was maintained for 30-45 min, and then returned to normal pressure;

[0072] A3. After vacuum drying, centrifuge at a speed of 5000 r / min for 10 min to separate the solid phase, wash the solid phase (using ethanol for 2 times), vacuum dry for 30 h, and grind into powder to obtain hydrochloric acid-etched halloysite nanotubes loaded with ammonium polyphosphate;

[0073] A4, 60 g of a 5 mg / mL polyethyleneimine solution and the hydrochloric acid-etched halloysite nanotube-loaded ammonium polyphosphate obtained in step A3 were mixed, stirred for 30 min, centrifuged, the solid phase was separated, and the solid phase was washed (using deionized water) to complete the first layer of encapsulation;

[0074] A5. After the first layer of encapsulation is completed, 60 g of a sodium polystyrene sulfonate solution with a concentration of 5 mg / mL is added, stirred for 15 min, centrifuged, the solid phase is separated, and the solid phase is washed (using deionized water) to complete the second layer of encapsulation to obtain a composite;

[0075] A6. After the second layer of encapsulation is completed, the mixture is dried for 26 hours and ground into powder to obtain the halloysite nanotube-ammonium polyphosphate composite;

[0076] Example 1

[0077] The present embodiment provides a flame retardant and antistatic polyurethane elastomer, which includes the following raw materials by weight: 100 g of cast polyurethane elastomer, 3 g of N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, 14 g of carbon black, 10 g of halloysite nanotube-ammonium polyphosphate composite, 110 g of ethyl acetate, 5 g of diethylene glycol dibenzoate, 1.5 g of dilauryl thiodipropionate, and 0.5 g of lubricant.

[0078] The preparation method of the flame retardant antistatic polyurethane elastomer in this preparation example comprises the following steps:

[0079] S1, dissolving N-(β-aminoethyl)-γ-aminopropyltriethoxysilane in ethyl acetate, adding carbon black, ultrasonicating for 30 minutes, and then adding a casting polyurethane elastomer at 80° C. to dissolve the elastomer to obtain a first mixture;

[0080] S2, mixing the halloysite nanotube-ammonium polyphosphate complex, diethylene glycol dibenzoate, zinc stearate and dilauryl thiodipropionate to obtain a second mixture;

[0081] S3, adding the second mixed material to the first mixed material, mixing and stirring for 145 minutes, evaporating and removing the remaining ethyl acetate, extruding and granulating, and obtaining the flame retardant antistatic polyurethane elastomer.

[0082] The temperature of each zone in the extrusion granulation was 195°C and the rotation speed was 700r / min.

[0083] The halloysite nanotube-ammonium polyphosphate composite used in this example is prepared in Preparation Example 1.

[0084] The lubricant in this embodiment is zinc stearate.

[0085] The flame retardant and antistatic polyurethane elastomer in this embodiment is a cast polyurethane elastomer.

[0086] Embodiment 2-4

[0087] Example 2

[0088] The difference between this embodiment and embodiment 1 is that when preparing the flame retardant antistatic polyurethane elastomer, the total weight of carbon black and halloysite nanotube-ammonium polyphosphate composite is 24 parts, and the weight ratio of carbon black and halloysite nanotube-ammonium polyphosphate composite is 1.2:1.

[0089] Example 3

[0090] The difference between this embodiment and embodiment 1 is that when preparing the flame retardant antistatic polyurethane elastomer, the total weight of carbon black and halloysite nanotube-ammonium polyphosphate composite is 24 parts, and the weight ratio of carbon black and halloysite nanotube-ammonium polyphosphate composite is 1.5:1.

[0091] Example 4

[0092] The difference between this embodiment and embodiment 1 is that when preparing the flame retardant antistatic polyurethane elastomer, the total weight of carbon black and halloysite nanotube-ammonium polyphosphate composite is 24 parts, and the weight ratio of carbon black and halloysite nanotube-ammonium polyphosphate composite is 1.7:1.

[0093] Comparative Examples 1-3

[0094] Comparative Example 1

[0095] The difference between this comparative example and Example 3 is that the halloysite nanotube-ammonium polyphosphate composite is not added when preparing the flame retardant antistatic polyurethane elastomer.

[0096] Comparative Example 2

[0097] The difference between this comparative example and Example 3 is that no carbon black is added when preparing the flame retardant antistatic polyurethane elastomer.

[0098] Comparative Example 3

[0099] The difference between this comparative example and Example 3 is that when preparing the flame retardant antistatic polyurethane elastomer, no carbon black and halloysite nanotube-ammonium polyphosphate composite were added.

[0100] Experimental testing:

[0101] UL-94 vertical combustion test: CZF-2 integrated vertical combustion tester was used to test 5 specimens of each formulation (sample size 125×13×0.8mm) and the average value was taken.

[0102] Surface resistivity: Tested in accordance with GBT 14102006, sample specification 100*100*3.0mm rectangular plate.

[0103] Tensile strength test: Tested in accordance with GB / T 1040.22006 standard; tensile speed is 10mm / min.

[0104] Oxygen index test: Test the oxygen index according to GBT24093.

[0105] The experimental test results of Examples 1-4 and Comparative Examples 1-3 are shown in Table 1.

[0106] Table 1 - Experimental test results of Examples 1-4 and Comparative Examples 1-3

[0107]

[0108] Result analysis: The difference between Examples 2-4 and Example 1 is that when preparing the flame retardant antistatic polyurethane elastomer, the total weight of carbon black and halloysite nanotube-ammonium polyphosphate complex is 24 parts, and the weight ratio of carbon black and halloysite nanotube-ammonium polyphosphate complex is different. Combined with the experimental test results in Table 1, it can be seen that when the weight ratio of carbon black and halloysite nanotube-ammonium polyphosphate complex is 1.5:1, the flame retardant and antistatic properties of the flame retardant antistatic polyurethane elastomer prepared are good. The difference between Comparative Example 1 and Example 3 is that when preparing the flame retardant antistatic polyurethane elastomer, the halloysite nanotube-ammonium polyphosphate complex is not added. The difference between Comparative Example 2 and Example 3 is that when preparing the flame retardant antistatic polyurethane elastomer, carbon black is not added. The difference between Comparative Example 3 and Example 3 is that when preparing the flame retardant antistatic polyurethane elastomer, carbon black and halloysite nanotube-ammonium polyphosphate complex are not added. Combined with the experimental test results in Table 1, it can be seen that when preparing flame-retardant antistatic polyurethane elastomer, the compound use of carbon black and halloysite nanotube-ammonium polyphosphate composite can improve the comprehensive performance of the flame-retardant antistatic polyurethane elastomer. The reason may be that carbon black can fill the gaps in the cast polyurethane elastomer to improve the density and mechanical properties of the material; on the other hand, the halloysite nanotube-ammonium polyphosphate composite can give the material excellent flame retardant properties. This effect enables the flame-retardant antistatic polyurethane elastomer to have excellent flame retardant and antistatic properties while maintaining excellent mechanical properties.

[0109] Embodiment 5-6

[0110] Example 5

[0111] The difference between Example 5-6 and Example 3 is that the weight fractions of some components are changed when preparing the flame retardant antistatic polyurethane elastomer. See Table 2 for the differences.

[0112] Table 2 - Differences between Examples 5-6 and Example 3

[0113] Ingredients (g) Example 3 Example 5 Example 6 Casting polyurethane elastomer 100 122 135 N-(β-aminoethyl)-γ-aminopropyltriethoxysilane 3 4.7 5 Carbon Black 14.4 14.4 14.4 Halloysite nanotube-ammonium polyphosphate composite 9.6 9.6 9.6 Ethyl acetate 110 120 130 Diethylene glycol dibenzoate 5 6.5 8 Dilauryl thiodipropionate 1.5 2.2 3 Zinc stearate 0.5 1.6 2

[0114] The experimental test results of Examples 5-6 are shown in Table 3.

[0115] Table 3 - Experimental test results of Examples 5-6

[0116]

[0117]

[0118] Result analysis: The difference between Example 5-6 and Example 3 is that when preparing the flame retardant antistatic polyurethane elastomer, the weight proportions of some components are different. Combined with the experimental test results in Table 3, it can be seen that when preparing the flame retardant antistatic polyurethane elastomer, the flame retardant antistatic polyurethane elastomer prepared in Example 5 has better comprehensive performance.

[0119] Embodiment 7-11

[0120] The difference between Examples 7-11 and Example 5 is that when preparing the flame retardant antistatic polyurethane elastomer, on the premise that the weight ratio of carbon black and halloysite nanotube-ammonium polyphosphate composite is 1.5:1, the total weight ratio of carbon black and halloysite nanotube-ammonium polyphosphate composite in the flame retardant antistatic polyurethane elastomer is changed, and the optimal weight ratio is selected.

[0121] In Example 5, the total weight of carbon black and halloysite nanotube-ammonium polyphosphate is 24 parts, and the total weight of the flame retardant and antistatic polyurethane elastomer is 161 parts (because ethyl acetate acts as a solvent in this application, when examining the effect of the total weight of carbon black and halloysite nanotube-ammonium polyphosphate on the properties of the flame retardant and antistatic polyurethane elastomer, the total weight does not include ethyl acetate).

[0122] Therefore, it is not difficult to conclude that in Example 5, the proportion of carbon black (referred to as variable 1) and halloysite nanotube-ammonium polyphosphate composite (referred to as variable 2) in the flame retardant antistatic polyurethane elastomer (referred to as the matrix) is 14.91%.

[0123] The differences between Examples 7-11 and Example 5 are shown in Table 4.

[0124] Proportion = (variable 1 + variable 2) / total weight of matrix * 100%.

[0125] Table 4 - Differences between Examples 7-11 and Example 5

[0126]

[0127] The experimental test results of Examples 7-11 are shown in Table 5.

[0128] Table 5 - Experimental test results of Examples 7-11

[0129]

[0130]

[0131] Result analysis: The difference between Examples 7-11 and Example 5 is that when preparing the flame retardant antistatic polyurethane elastomer, when the proportion of carbon black (referred to as variable 1) and halloysite nanotube-ammonium polyphosphate composite (referred to as variable 2) in the flame retardant antistatic polyurethane elastomer (referred to as the matrix) is between (14.91-17.96)%, the comprehensive performance of the flame retardant antistatic polyurethane elastomer obtained is better. When the proportion of carbon black (referred to as variable 1) and halloysite nanotube-ammonium polyphosphate composite (referred to as variable 2) in the flame retardant antistatic polyurethane elastomer (referred to as the matrix) is 17.12%, the comprehensive performance of the flame retardant antistatic polyurethane elastomer obtained is better.

[0132] Examples 12-13

[0133] Example 12

[0134] The difference between this embodiment and embodiment 10 is that different preparation parameters of the halloysite nanotube-ammonium polyphosphate composite are used in preparing the flame-retardant antistatic polyurethane elastomer. The halloysite nanotube-ammonium polyphosphate composite in this embodiment is prepared by Preparation Example 2.

[0135] Example 13

[0136] The difference between this embodiment and embodiment 10 is that different preparation parameters of the halloysite nanotube-ammonium polyphosphate composite are used in preparing the flame-retardant antistatic polyurethane elastomer. The halloysite nanotube-ammonium polyphosphate composite in this embodiment is prepared by Preparation Example 3.

[0137] The experimental test results of Examples 12-13 are shown in Table 6.

[0138] Table 6 - Experimental test results of Examples 12-13

[0139]

[0140] Result analysis: The difference between Examples 12-13 and Example 10 is that, when preparing the flame retardant and antistatic polyurethane elastomer, the halloysite nanotube-ammonium polyphosphate composite prepared in Preparation Example 2 can better improve the comprehensive performance of the flame retardant and antistatic polyurethane elastomer.

[0141] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A flame retardant and antistatic polyurethane elastomer, characterized in that: The flame retardant antistatic polyurethane elastomer comprises the following raw materials by weight: 100-135 parts of cast polyurethane elastomer, 3-5 parts of N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, 9-18 parts of carbon black, 6-12 parts of halloysite nanotube-ammonium polyphosphate complex, 25-30 parts of ethyl acetate, 5-8 parts of diethylene glycol dibenzoate, 1.5-3 parts of dilauryl thiodipropionate, and 0.5-2 parts of lubricant; The preparation method of the halloysite nanotube-ammonium polyphosphate composite comprises the following steps: A1. Add a hydrochloric acid solution with a concentration of (3-5) mol / L to the halloysite nanotubes, heat and stir in a water bath for 6-8 hours, centrifuge to separate the solid matter, and wash and grind the solid matter to obtain the halloysite nanotubes etched with hydrochloric acid; A2, mixing the hydrochloric acid-etched halloysite nanotubes obtained in step A1, ammonium polyphosphate and water, and ultrasonically dispersing them for 40-60 minutes in an ice bath, and then vacuum-treating the obtained suspension, wherein the vacuum treatment is as follows: when the vacuum degree reaches -0.1 MPa, maintain it for 30-45 minutes, and then return to normal pressure; A3. After the vacuum treatment, centrifuge to separate the solid phase, wash the solid phase, vacuum dry for 24-30 hours, and grind into powder to obtain the hydrochloric acid-etched halloysite nanotubes loaded with ammonium polyphosphate; A4, mixing a polyethyleneimine solution having a concentration of (3-5) mg / mL and the ammonium polyphosphate loaded on the halloysite nanotubes after hydrochloric acid etching obtained in step A3, stirring for 20-30 minutes, centrifuging to separate the solid phase, and washing the solid phase to complete the first layer of encapsulation; A5. After the first layer of encapsulation is completed, add a sodium polystyrene sulfonate solution with a concentration of (3-5) mg / mL, stir for 10-15 minutes, centrifuge to separate the solid phase, and wash the solid phase to complete the second layer of encapsulation; A6. After the second layer of encapsulation is completed, the mixture is dried for 24-26 hours and ground into powder to obtain the halloysite nanotube-ammonium polyphosphate composite.

2. The flame retardant and antistatic polyurethane elastomer according to claim 1, characterized in that: The weight ratio of the halloysite nanotubes to the hydrochloric acid solution in step A1 is (5-8): (80-100); The weight ratio of the ammonium polyphosphate and water in step A2 to the halloysite nanotubes in step A1 is (8-10): (50-100): 1; The weight ratio of the polyethyleneimine solution, the ammonium polyphosphate loaded halloysite nanotubes after hydrochloric acid etching and the sodium polystyrene sulfonate solution in step A4 is (4-6):1:(4-6).

3. The flame retardant and antistatic polyurethane elastomer according to claim 1, characterized in that: The weight ratio of the carbon black to the halloysite nanotube-ammonium polyphosphate composite is (1.2-1.7):

1.

4. The flame retardant and antistatic polyurethane elastomer according to claim 3, characterized in that: The weight ratio of the carbon black to the halloysite nanotube-ammonium polyphosphate composite is 1.5:

1.

5. The flame retardant and antistatic polyurethane elastomer according to claim 1, characterized in that: The total weight of the carbon black and the halloysite nanotube-ammonium polyphosphate composite accounts for (14.91-17.96)% of the flame retardant antistatic polyurethane elastomer.

6. The flame retardant and antistatic polyurethane elastomer according to claim 1, characterized in that: The vacuum treatment in step A2 was performed twice.

7. The flame retardant and antistatic polyurethane elastomer according to claim 1, characterized in that: The centrifugation conditions in step A3 are as follows: centrifugal speed is 4000-5000 r / min, and centrifugal time is 5-10 min.

8. The flame retardant and antistatic polyurethane elastomer according to claim 1, characterized in that: The lubricant is selected from zinc stearate.

9. A method for preparing the flame retardant and antistatic polyurethane elastomer according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: S1, dissolving N-(β-aminoethyl)-γ-aminopropyltriethoxysilane in ethyl acetate, adding carbon black, ultrasonicating for 30-45 min, removing the remaining ethyl acetate, and obtaining N-(β-aminoethyl)-γ-aminopropyltriethoxysilane modified carbon black; S2. Add the remaining raw materials to the N-(β-aminoethyl)-γ-aminopropyltriethoxysilane modified carbon black obtained in step S1, mix and stir for (130-150) minutes, extrude and granulate to obtain the flame retardant antistatic polyurethane elastomer.

10. The method for preparing a flame retardant and antistatic polyurethane elastomer according to claim 9, characterized in that: The temperature of each zone in the extrusion granulation is 180°C-200°C, and the rotation speed is 500-800r / min.

Citation Information

Patent Citations

  • Weather-resistant single-component polyurethane black sealant and preparation method thereof

    CN116042163A

  • Alkali response self-healing agent as well as preparation method and application thereof

    CN116425445A

  • Modified phosphorus-containing flame retardant, flame-retardant polyamide, flame-retardant polyurethane and flame-retardant polyolefin

    CN116444860A

  • Aqueous Polyelectrolyte Complex as One Pot Nanocoating Solution to Impart Antiflammable Behavior to Various Substrates

    US20160280933A1

  • Waterborne Complex, Coating Procedure and Use as a Flame Retardant

    US20180022939A1