A nano-silicon dioxide synergistic flame retardant modified coating and preparation method thereof

By preparing the modified nano-silica with phosphorus-containing flame retardant and polyurethane emulsion, the problems of flammability and poor water resistance of solvent-based coatings are solved, and efficient flame retardant, water resistance and weather resistance are achieved, suitable for industrial and outdoor use Building paint.

CN118271957BActive Publication Date: 2024-11-29广州豫顺新材料科技有限公司 +1

Patent Information

Application Number
CN202410556431.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-07
Publication Date
2024-11-29
Estimated Expiration
2044-05-07

AI Technical Summary

Technical Problem

Solvent-based coatings are flammable, water-resistant and weather-resistant, and existing flame retardants are easily lost and cannot meet the long-term use needs.

Method used

By preparing phosphorus-containing flame retardant modified nanosilica and combining it with polyurethane emulsion, nanosilica synergistic flame retardant modified coatings are formed to enhance the flame retardant, water and weather resistance of the coatings.

Benefits of technology

It significantly improves the flame retardancy, water resistance and weather resistance of the coating, reduces the loss of flame retardant, and is suitable for industrial and outdoor building coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004826191560000081
    Figure BDA0004826191560000081
  • Figure BDA0004826191560000082
    Figure BDA0004826191560000082
  • Figure BDA0004826191560000091
    Figure BDA0004826191560000091
Patent Text Reader

Abstract

The invention provides a nano-silicon dioxide synergistic flame-retardant modified coating and a preparation method thereof, belonging to the technical field of coatings; the nano-silicon dioxide synergistic flame-retardant modified coating of the invention comprises the following components in parts by weight: 60-80 parts of polyurethane emulsion, 10-30 parts of nano-silicon dioxide, 5-60 parts of phosphorus-containing flame retardant modified nano-silicon dioxide, 5-10 parts of dispersant, 0.1-2 parts of leveling agent, and 0.1-2 parts of light stabilizer, wherein the phosphorus-containing flame retardant modified nano-silicon dioxide is prepared by the following steps: S1. surface-treating the nano-silicon dioxide with a silane coupling agent to obtain the silane coupling agent modified nano-silicon dioxide, and S2. reacting the phosphorus-containing flame retardant with the silane coupling agent modified nano-silicon dioxide in an organic solvent to obtain the phosphorus-containing flame retardant modified nano-silicon dioxide. The present invention provides a nano-silica synergistic flame retardant modified coating, which is prepared by preparing phosphorus-containing flame retardant modified nano-silica and compounding nano-silica and adding them to polyurethane coating to obtain a modified coating with good flame retardancy, good water resistance and good weather resistance, thereby overcoming the problems of solvent-based coatings being flammable, poor water resistance and poor weather resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a nano-silicon dioxide synergistic flame-retardant modified coating and a preparation method thereof. Background Art

[0002] For a long time, solvent-based coatings have been widely used for their good decorative properties, variety and low price. More than half of the solvents used in solvent-based coatings are hydrocarbons, and the rest are ketones, alcohols, ethylene glycol, ethers, esters, nitro straight-chain alkanes and a small amount of other substances. Solvents are conducive to film formation, and when the solvent evaporates, the polymers combine with each other. Historically, almost all coatings are solvent-based coatings. Currently, there are water-based coatings, powder coatings, radiation-cured coatings, etc. The main reason for the development of these coatings is to reduce fire hazards and odors and facilitate cleaning with water. However, solvent-based coatings still have advantages that other coatings cannot surpass: the cost of their construction is generally lower, especially compared with water-based coatings, because water-based coatings require stainless steel equipment for construction, and the electrostatic spraying equipment of solvent-based coatings costs less than water-based coatings; humidity has little effect on solvent volatilization; the coating film has few problems of trapped air and explosion holes. At present, most industrial coatings, special coatings and some architectural coatings are still solvent-based coatings. Combined with the current safety considerations of frequent fires in high-rise buildings, in order to solve the flammable problem of solvent-based coatings, the industry mainly uses external flame retardants to achieve flame retardant requirements. However, due to the poor water resistance, salt spray resistance, solvent resistance and other properties of the external small molecule flame retardants, they are easy to be lost from the coating, resulting in the gradual loss of flame retardant properties during use, etc., which cannot meet long-term use needs. Summary of the invention

[0003] In order to overcome the deficiencies of the above-mentioned prior art, the present invention provides a nano-silicon dioxide synergistic flame retardant modified coating, which has the characteristics of flame retardancy, good water resistance, good outdoor durability, etc.

[0004] Another object of the present invention is to provide a method for preparing a nano-silicon dioxide synergistic flame retardant modified coating.

[0005] The present invention is achieved through the following technical scheme: a nano-silicon dioxide synergistic flame retardant modified coating, characterized in that it comprises the following components by weight: 60-80 parts of polyurethane emulsion, 10-30 parts of nano-silicon dioxide, 5-60 parts of phosphorus-containing flame retardant modified nano-silicon dioxide, 5-10 parts of dispersant, 0.1-2 parts of leveling agent, and 0.1-2 parts of light stabilizer. The phosphorus-containing flame retardant modified nano-silicon dioxide is prepared by the following steps: S1. surface treatment of nano-silicon dioxide with a silane coupling agent to obtain silane coupling agent modified nano-silicon dioxide, and S2. reacting the phosphorus-containing flame retardant with the silane coupling agent modified nano-silicon dioxide in an organic solvent to obtain the phosphorus-containing flame retardant modified nano-silicon dioxide.

[0006] In a specific embodiment, the preparation method of nano-silica surface-treated with a silane coupling agent to obtain silane coupling agent-modified nano-silica can be as follows: ultrasonically dispersing the nano-silica in a 75% ethanol solution to obtain a dispersion A, ultrasonically dispersing the silane coupling agent in a 75% ethanol solution to obtain a dispersion B, then heating the dispersion A to 60-80° C., slowly adding the dispersion B, and finally stirring at 60-80° C. for 6-10 hours, cooling, filtering, and drying to obtain the silane coupling agent-modified nano-silica.

[0007] In a specific embodiment, the mass of the silane coupling agent is 0.5wt%-3wt% of the nano-silicon dioxide; preferably, the mass of the silane coupling agent is 1wt%-2wt% of the nano-silicon dioxide.

[0008] In a specific embodiment, the mass of the phosphorus-containing flame retardant is 50wt%-100wt% of the silane coupling agent modified nano-silica; preferably, the mass of the phosphorus-containing flame retardant is 60wt%-80wt% of the silane coupling agent modified nano-silica.

[0009] In a specific embodiment, the silane coupling agent is selected from at least one of an aminosilane coupling agent and an epoxysilane coupling agent. Preferably, the aminosilane coupling agent is selected from at least one of 3-aminopropyltriethoxysilane and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane; the epoxysilane coupling agent is selected from 3-glycidyloxypropyltrimethoxysilane.

[0010] In a specific embodiment, the phosphorus-containing flame retardant is selected from at least one of hexachlorocyclotriphosphazene and hexa(p-aminophenoxy)cyclotriphosphazene;

[0011] Preferably, when the silane coupling agent is selected from aminosilane coupling agent, the phosphorus-containing flame retardant is selected from hexachlorocyclotriphosphazene; when the silane coupling agent is selected from epoxysilane coupling agent, the phosphorus-containing flame retardant is selected from hexa(p-aminophenoxy)cyclotriphosphazene.

[0012] Preferably, the phosphorus-containing flame retardant reacts with the silane coupling agent-modified nano-silica in an organic solvent, wherein the organic solvent is at least one of tetrahydrofuran and N,N-dimethylformamide, the reaction temperature is controlled at 50-130° C., and the reaction time is 6-8 hours.

[0013] In a specific embodiment, the mass ratio of nano-silicon dioxide to the nano-silicon dioxide modified by the phosphorus-containing flame retardant is 1:(1-3), preferably, the mass ratio of nano-silicon dioxide to the nano-silicon dioxide modified by the phosphorus-containing flame retardant is 1:(1.5-2).

[0014] In a specific embodiment, the nano silicon dioxide is selected from fumed silicon dioxide, and the specific surface area of ​​the nano silicon dioxide is 80-400 m 2 / g; Preferably, the specific surface area of ​​nano-silicon dioxide is 150-200m 2 / g; the specific surface area of ​​the nano-silicon dioxide is measured by the nitrogen adsorption method specified in the standard GB / T 10722-2014; specifically, the nano-silicon dioxide used in the present invention and the nano-silicon dioxide in the nano-silicon dioxide modified with the phosphorus-containing flame retardant can be the same or different; preferably, the nano-silicon dioxide used in the present invention and the nano-silicon dioxide in the nano-silicon dioxide modified with the phosphorus-containing flame retardant are the same.

[0015] In a specific embodiment, the polyurethane emulsion can be purchased from the market or prepared by oneself. Optionally, the preparation method of the polyurethane emulsion is as follows: S1. Prepolymerization reaction: adding diisocyanate and a catalyst to a polymer diol, and carrying out a prepolymerization reaction at 60 to 85° C. and an inert gas atmosphere for 45 to 150 minutes to obtain a prepolymer product; S2. Chain extension reaction: adding a chain extender to the prepolymer product obtained in S1, carrying out a chain extension reaction at 60 to 80° C. for 60 to 180 minutes, and diluting with a diluent to obtain a chain extension product; S3. Neutralization reaction: adding a neutralizer to obtain the polyurethane emulsion.

[0016] Optionally, the diisocyanate is at least one of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, 1,6-hexamethylene diisocyanate and L-lysine diisocyanate;

[0017] Optionally, the polymer diol is selected from at least one of polyester alcohol, polyether alcohol, and polycarbonate diol;

[0018] Optionally, the catalyst is selected from at least one of triethylamine, dimethylcyclohexylamine, N-methylmorpholine, N,N'-dimethylpiperazine, 2-(dimethylaminoethoxy)ethanol, and diazabicyclo (2,2,2) octane (DABCO);

[0019] Optionally, the chain extender is at least one of dimethylol propionic acid, dimethylol butyric acid, 1,3-propylene glycol, 1,4-butanediol, and 1,6-hexanediol;

[0020] Optionally, the diluent is at least one of acetone or butanone;

[0021] Optionally, the neutralizing agent is at least one of triethylamine, sodium hydroxide, sodium bicarbonate and ammonia water.

[0022] In a specific embodiment, the dispersant is selected from at least one of acrylic acid copolymer and maleic acid copolymer;

[0023] Preferably, the dispersant is selected from at least one of styrene / acrylic acid copolymers, acrylic acid / maleic acid copolymers, acrylic acid / methacrylic acid copolymers, butadiene / acrylic acid copolymers, isobutylene / maleic acid copolymers, diisobutylene / maleic acid copolymers, styrene / maleic acid copolymers, and polyethylene glycol monovinyl ether / maleic acid copolymers.

[0024] In a specific embodiment, the leveling agent is selected from at least one of a nonionic surfactant, a cationic surfactant, and an anionic surfactant; preferably, the leveling agent is selected from a nonionic acetylene glycol compound

[0025] In a specific embodiment, the light stabilizer is at least one of BASF's TINUVIN 783, BASF's TINUVIN 791, and BASF's TINUVIN XT833.

[0026] In a specific embodiment, the nano-silicon dioxide synergistic flame retardant modified coating further comprises at least one of 1-30 parts of pigment, 0.1-5 parts of defoaming agent, and 0.1-5 parts of antibacterial agent by weight;

[0027] Optionally, the pigment is selected from at least one of an organic pigment and an inorganic pigment;

[0028] Optionally, the organic pigment is selected from one or more of a disazo pigment, a disazo condensation pigment, a dibenzopyrene dione pigment, anthraquinone pigment, anthraquinone pyrimidine pigment, a benzimidazolone pigment, a quinacridone pigment, a quinophthalone pigment, a diketopyrrolopyrrole pigment, a dioxazine pigment, an indanthrone pigment, an isoindoline pigment, an isoindolinone pigment, a perylene pigment, a phthalocyanine pigment, and a pyrazolequinazolinone pigment, and the inorganic pigment is selected from one or more of titanium dioxide, black iron oxide, iron manganese black, spinel black, carbon black, graphite, chromium oxide iron black, red iron oxide, brown iron oxide, yellow iron oxide, nickel titanium yellow, spinel phase, and bismuth vanadate;

[0029] Optionally, the defoaming agent is selected from at least one of polysiloxane, hydrophobic solid, polyether-modified siloxane, and polyether-siloxane copolymer;

[0030] Optionally, the antimicrobial agent is selected from at least one of isothiazolones and isothiazolinones;

[0031] Optionally, the isothiazolones are selected from methylisothiazolone, benzisothiazolone, chloromethylisothiazolone; and the isothiazolinones are selected from methylisothiazolinone.

[0032] The present invention also protects a method for preparing a carbon fiber composite material for a bicycle frame, comprising the following steps:

[0033] S1. Weigh each component by weight, add part of the solvent, polyurethane, nano-silica, dispersant, leveling agent, light stabilizer to a mixer, and stir at a speed of 400-600r / min for 15-25min to obtain a first mixture;

[0034] S2. Add the phosphorus-containing flame retardant modified nano-silica to the first mixture and stir at a speed of 600-800r / min for 30-40min;

[0035] S3. Add the remaining solvent and other additives under stirring, and continue stirring at a speed of 400-600 r / min for at least 30 min to obtain the nano-silicon dioxide synergistic flame retardant modified coating.

[0036] Beneficial Effects

[0037] The present invention provides a nano-silica synergistic flame retardant modified coating, which is prepared by preparing phosphorus-containing flame retardant modified nano-silica and nano-silica compounded and added to polyurethane coating to obtain a modified coating with good flame retardancy, good water resistance and good weather resistance, thereby overcoming the problems of flammability, poor water resistance and poor weather resistance of solvent-based coatings. The present invention grafts the phosphorus-containing flame retardant onto the nano-silica, thereby reducing the phenomenon that the flame retardant precipitates from the coating due to outdoor adverse weather conditions, thereby affecting the long-term flame retardant effect and coating effect; and the phosphorus-containing flame retardant modified nano-silica can further synergistically improve its flame retardant, water resistance and weather resistance effects with nano-silica, and is suitable for use in industrial coatings, special coatings and outdoor architectural coatings. DETAILED DESCRIPTION

[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0040] The raw materials used in the embodiments and comparative examples are described as follows:

[0041] Polyurethane emulsion: Homemade, preparation method is as follows:

[0042] S1. Prepolymerization reaction: add toluene diisocyanate and catalyst triethylamine to polyether diol, carry out prepolymerization reaction at 80°C and inert gas atmosphere for 100 minutes to obtain a prepolymer product; S2. Chain extension reaction: add chain extender 1,3-propylene glycol to the prepolymer product obtained in S1, carry out chain extension reaction at 65°C for 150 minutes, add acetone to dilute, and obtain a chain extension product; S3. Neutralization reaction: add ammonia water to obtain the polyurethane emulsion.

[0043] Nano-silicon dioxide 1: Fumed silica, HL-90, nitrogen adsorption specific surface area 100±20m 2 / g, purchased from Hubei Huifu Nanomaterials;

[0044] Nano-silicon dioxide 2: Fumed silica, HL-150, nitrogen adsorption specific surface area 150±15m 2 / g, purchased from Hubei Huifu Nanomaterials;

[0045] Nano-silicon dioxide 3: Fumed silica, HL-200, nitrogen adsorption specific surface area 200±20m 2 / g, purchased from Hubei Huifu Nanomaterials;

[0046] Nano-silicon dioxide 4: Fumed silica, HL-380, nitrogen adsorption specific surface area 380±30m 2 / g, purchased from Hubei Huifu Nanomaterials;

[0047] Phosphorus-containing flame retardant modified nano-silica (hereinafter referred to as modified silica): homemade, specific components and their weight parts are shown in Table 1, and the preparation method is as follows:

[0048] S1. Ultrasonic dispersion of nano-silica in 75% ethanol solution to obtain dispersion A, ultrasonic dispersion of silane coupling agent in 75% ethanol solution to obtain dispersion B, then heating dispersion A to 70°C, slowly adding dispersion B, stirring at 70°C for 8 hours, cooling, filtering, and drying at 100°C to obtain silane coupling agent-modified nano-silica;

[0049] S2. The phosphorus-containing flame retardant and the silane coupling agent-modified nano-silica are reacted in N,N-dimethylformamide, the reaction temperature is controlled at 60-130° C., and the reaction time is 6-8 hours to obtain the phosphorus-containing flame retardant-modified nano-silica.

[0050] Silane coupling agent 1: 3-aminopropyltriethoxysilane, purchased from Qufu Yishun Chemical;

[0051] Silane coupling agent 2: N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, purchased from Qufu Yishun Chemical;

[0052] Silane coupling agent 3: 3-glycidyloxypropyltrimethoxysilane, purchased from Qufu Yishun Chemical;

[0053] Phosphorus-containing flame retardant 1: hexachlorocyclotriphosphazene, purchased from Hubei Chengfeng Chemical;

[0054] Phosphorus-containing flame retardant 2: hexa(p-aminophenoxy)cyclotriphosphazene, purchased from Shanghai Zhuogao New Materials;

[0055] Dispersant 1: DISPERBYK-2015, acrylic copolymer, purchased from BYK, Germany;

[0056] Dispersant 2: DISPERBYK-190, maleic acid copolymer, purchased from BYK, Germany;

[0057] Leveling agent: Surfynol 104BC, acetylenic diol nonionic surfactant, purchased from Evonik;

[0058] Light stabilizer: TINUVIN 783, TINUVIN791, purchased from BASF, mass ratio is 1:1;

[0059] Defoamer: BYK 022, polysiloxane and hydrophobic solid, purchased from BYK, Germany;

[0060] Antimicrobial agents: KathonTM LX-150 Biocide, 5-chloro-2-methyl-4-isothiazolin-3-one and 2-methyl-4-isothiazolin-3-one, purchased from Dow;

[0061] Unless otherwise specified, the components and raw materials used in the embodiments and comparative examples of the present invention are all commercially available raw materials, and the components and raw materials used in each parallel experiment are all of the same kind.

[0062] Table 1

[0063]

[0064] Table 1

[0065]

[0066] Example 1-18 A nano-silicon dioxide synergistic flame retardant modified coating and its preparation method

[0067] Example 1-18 provides a nano-silicon dioxide synergistic flame retardant modified coating and a preparation method thereof. The weight formula is shown in Table 2. The preparation method is as follows:

[0068] S1. Weigh each component by weight, add polyurethane, nano-silica, dispersant, leveling agent, light stabilizer to a mixer, and stir at a speed of 600r / min for 25min to obtain a first mixture;

[0069] S2. Add the phosphorus-containing flame retardant modified nano-silica to the first mixture and stir at a speed of 700r / min for 30min;

[0070] S3. Add other additives under stirring, and continue stirring at a speed of 600 r / min for 30 min to obtain a nano-silicon dioxide synergistic flame retardant modified coating.

[0071] Table 2

[0072]

[0073]

[0074] Table 2

[0075]

[0076]

[0077] The preparation method of Comparative Examples 1-4 is the same as that of Examples 1-18, and the weight formula is shown in Table 3.

[0078] Table 3

[0079] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Polyurethane emulsion 70 70 70 70 Nano Silica 1 Nano Silica 2 60 20 20 Nano Silica 3 Nano Silica 4 Modified silica 1 60 Modified silica 13 40 Modified silica 14 40 Phosphorus flame retardant 1 15 Dispersant 1 8 8 8 8 Leveling agent 1 1 1 1 Light Stabilizer 1 1 1 1 Defoaming agent 2 2 2 2 Antimicrobial agents 2 2 2 2

[0080] A nano-silicon dioxide synergistic flame retardant modified coating prepared in Examples 1-18 and Comparative Examples 1-4 was coated on a substrate to conduct the following performance tests. The results are shown in Table 4.

[0081] 1. Water resistance: Test the water resistance of the modified coating according to Method A of GB / T 1733-93, and record whether there is loss of gloss, discoloration, blistering, wrinkling, shedding, rust, etc. If the area of ​​gloss loss, discoloration, blistering, wrinkling, shedding and rusting accounts for 0% of the flooded area, it is recorded as level 0; if the area of ​​gloss loss, discoloration, blistering, wrinkling, shedding and rusting accounts for 1-5% of the flooded area, it is recorded as level 1; if the area of ​​gloss loss, discoloration, blistering, wrinkling, shedding and rusting accounts for 5-10% of the flooded area, it is recorded as level 2; if the area of ​​gloss loss, discoloration, blistering, wrinkling, shedding and rusting accounts for 10-20% of the flooded area, it is recorded as level 3; if the area of ​​gloss loss, discoloration, blistering, wrinkling, shedding and rusting accounts for 20-50% of the flooded area, it is recorded as level 4; if the area of ​​gloss loss, discoloration, blistering, wrinkling, shedding and rusting accounts for more than 50% of the flooded area, it is recorded as level 5;

[0082] 2. Weather resistance: According to GB / T1727-2021, select tinplate and prepare the paint film by brushing method. According to GB / T9761-2008, select artificial light source to carry out light aging test on the paint film for 500 hours, and record the color difference grade. The color difference grade is as follows: 0: no visible difference; 1: very slight, that is, just visible difference; 2: slight, with clearly visible difference; 3: medium difference; 4: considerable difference; 5: very large difference.

[0083] 3. Flame retardancy: According to Appendix A of GB 12441-2018, the modified coating was tested for flame retardancy, and its flame retardancy time and flame retardancy (average value of the remaining length of the specimen after burning) were recorded;

[0084] 4. Flame retardancy after light aging: According to GB / T 9761-2008, select artificial light source to carry out light aging test on the modified coating, and then carry out flame retardancy test on the modified coating after light aging according to Appendix A of GB 12441-2018, and record its flame retardancy time and flame retardancy (average value of the remaining length of the specimen after burning).

[0085] Table 4

[0086]

[0087]

[0088] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A nano-silicon dioxide synergistic flame retardant modified coating, It is characterized in that The invention comprises the following components by weight: 60-80 parts of polyurethane emulsion, 10-30 parts of nano silicon dioxide, 5-60 parts of nano silicon dioxide modified by phosphorus-containing flame retardant, 5-10 parts of dispersant, 0.1-2 parts of leveling agent and 0.1-2 parts of light stabilizer. The nano silicon dioxide modified by phosphorus-containing flame retardant is prepared by the following steps: S1. surface treating nano silicon dioxide with silane coupling agent to obtain nano silicon dioxide modified by silane coupling agent; S2. reacting the phosphorus-containing flame retardant with the nano silicon dioxide modified by silane coupling agent in an organic solvent to obtain nano silicon dioxide modified by phosphorus-containing flame retardant; when the silane coupling agent is selected from aminosilane coupling agent, the phosphorus-containing flame retardant is selected from hexachlorocyclotriphosphazene; the mass ratio of nano silicon dioxide to nano silicon dioxide modified by phosphorus-containing flame retardant is 1:(1.5-2); the specific surface area of ​​nano silicon dioxide is 150-200m 2 / g, the nano silicon dioxide is selected from fumed silicon dioxide.

2. The nano-silicon dioxide synergistic flame retardant modified coating according to claim 1, It is characterized in that The mass of the silane coupling agent is 0.5wt%-3wt% of the nano-silicon dioxide; the mass of the phosphorus-containing flame retardant is 50wt%-100wt% of the silane coupling agent-modified nano-silicon dioxide.

3. The nano-silicon dioxide synergistic flame retardant modified coating according to claim 1, It is characterized in that The organic solvent is at least one of tetrahydrofuran and N,N-dimethylformamide.

4. The nano-silicon dioxide synergistic flame retardant modified coating according to claim 1, It is characterized in that The dispersant is selected from at least one of acrylic acid copolymers and maleic acid copolymers; the leveling agent is selected from at least one of nonionic surfactants, cationic surfactants and anionic surfactants; the light stabilizer is at least one of BASF's TINUVIN 783, BASF's TINUVIN 791 and BASF's TINUVIN XT833.

5. The nano-silicon dioxide synergistic flame retardant modified coating according to claim 1, It is characterized in that By weight, it also includes 1-30 parts of pigment, 0.1-5 parts of defoaming agent, and 0.1-5 parts of antibacterial agent; the pigment is selected from at least one of organic pigment and inorganic pigment; the defoaming agent is selected from at least one of polysiloxane, hydrophobic solid, and polyether modified siloxane; the antibacterial agent is selected from at least one of isothiazolones and isothiazolinones.

6. A method for preparing a nano-silicon dioxide synergistic flame retardant modified coating according to any one of claims 1 to 5, It is characterized in that The following steps are involved: S1. Weigh each component by weight, add polyurethane, nano-silica, dispersant, leveling agent, light stabilizer to a mixer, and stir at a speed of 400-600r / min for 15-25min to obtain a first mixture; S2. Add the phosphorus-containing flame retardant modified nano-silica to the first mixture and stir at a speed of 600-800r / min for 30-40min; S3. Add other additives under stirring, and continue stirring at a speed of 400-600 r / min for at least 30 min to obtain a nano-silicon dioxide synergistic flame retardant modified coating.

Citation Information

Patent Citations

  • Wear-resistant flame-retardant polyurethane coating

    CN108424718A

  • Waterborne inflaming retarding damping coating

    CN108822661A

Cited By

  • SiO2 synergistic bio-based PAPP / SPI intumescent flame-retardant thermoplastic polyurethane and preparation method thereof

    CN122103868A