A method for suppressing skin concavity during creep aging forming of external grid wall panels
By obtaining the skin thickness distribution characteristics of the outer grid wall panel, adding fillers and auxiliary plates, and using vacuum and bolt fixation, the problem of skin dents is solved, the forming accuracy and service life are improved, and a low residual stress forming effect is achieved .
Patent Information
- Application Number
- CN202410815873.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2044-06-24
AI Technical Summary
In the existing creep aging forming technology of large-scale aluminum alloy outer grid wall panels, the skin is easily dented during the forming process, affecting the forming accuracy and service life.
By obtaining the skin thickness distribution characteristics of different areas of the outer grid wall panel, add filler and use auxiliary boards, breathable felts and vacuum bags to cover them, ensuring that the auxiliary boards are closely attached to the smooth surface of the wall panels, and are fixed with vacuum and bolts. Prevent skin from denting.
Effectively suppress skin dents, improve forming accuracy and service life, reduce residual stress, and meet post-forming performance standards.
Smart Images

Figure CN118371594B
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of creep aging forming, and in particular to a method for suppressing skin depression during creep aging forming of an outer grid wall panel. Background Art
[0002] Creep aging forming technology is a new type of sheet metal forming technology that can simultaneously achieve forming and performance improvement of components. It is widely used in the integral forming and manufacturing of large aerospace components.
[0003] The outer grid wall of the interstage has an important impact on the flight performance and safety of the rocket. The existing creep aging forming technology of large aluminum alloy outer grid wall generally uses a concave die. During the forming process of the outer grid wall, the skin is very likely to be dented, and the forming accuracy and service life of the component are challenged.
[0004] In response to the above problems, scholars in the industry have conducted some relevant research. For example, the invention patent with the authorization announcement number CN111774814B discloses a method for processing the inner and outer grids of rocket short shell wall panels. In conjunction with the outer grid wall thickness control processing, the method uses a composite processing method of chemical milling and mechanical milling to ensure the accuracy of grid processing, but the method does not consider the influence of work hardening of the grid wall panels on material properties during the milling process. For another example, the invention patent with the authorization announcement number CN113000682B discloses a method for mechanical loading of outer grid wall panels. In this method, different card plates are used to form a punch suitable for forming the outer grid wall panels. The outer grid wall panels are gradually loaded through a movable mechanical loading system. However, the outer chord height at both ends of the outer grid wall panels formed by the punch is too high, and it is difficult to fix the wall panels during the actual loading process. Problems such as skin dents still exist.
[0005] Therefore, it is urgent to propose a method that can suppress the skin depression during creep aging forming of the outer grid wall panel. Summary of the invention
[0006] The purpose of the present invention is to provide a method for suppressing the skin depression during the creep aging forming process of the outer grid wall panel, so as to improve the forming accuracy and service life of the outer grid wall panel formed by the creep aging forming technology.
[0007] To achieve the above object, the present invention provides a method for suppressing the skin depression during the creep aging forming process of an outer grid wall panel, comprising the following steps:
[0008] Step S1, obtaining the distribution characteristics of the skin thickness of different areas of the outer grid wall panel; wherein the four corners of the surplus reserved area of the outer grid wall panel are provided with first through holes;
[0009] Step S2, adding fillers to the grid area corresponding to the thinner skin area according to the skin thickness distribution characteristics;
[0010] Step S3, first placing the auxiliary plate in contact with the smooth surface of the outer grid wall panel, then coating the surface of the outer grid wall panel and the auxiliary plate with a layer of breathable felt, then wrapping the breathable felt with a heat-resistant tape to obtain a whole wall panel; then using a first vacuum bag to seal the whole wall panel, and evacuating the first vacuum bag so that the auxiliary plate and the smooth surface of the outer grid wall panel are tightly fitted to obtain a vacuum-coated part;
[0011] Step S4, wrapping the surface of the vacuum-coated part with a layer of breathable felt, and then placing the vacuum-coated part wrapped with the breathable felt on the molding surface of the molding mold, and installing and positioning it;
[0012] Step S5, using a second vacuum bag to completely cover and seal the mold surface and the vacuum covering member wrapped with the breathable felt to obtain an integrally formed wall panel tooling;
[0013] Step S6, placing the integrally formed wall panel in a hot press, evacuating the outside of the tank, keeping the inside of the tank warm and loaded, and obtaining the formed outer grid wall panel after creep aging.
[0014] Furthermore, in step S2, the thinner skin area has a thickness of t <15% h of the region, h is the rib height of the outer grid wall panel.
[0015] Furthermore, in step S2, the size of the filler is 0.9-0.97 times the size of the grid area corresponding to the thinner skin area; the material of the filler is silicone or high-resistant rubber.
[0016] Furthermore, in step S3, the thickness of the auxiliary plate is selected according to the average thickness of the skin; wherein the average thickness of the skin T The calculation of is as follows:
[0017]
[0018] in, i is the skin thickness type, t i For different skin thicknesses, S i for t i The corresponding skin area.
[0019] Furthermore, the thickness of the auxiliary plate is 0.8 to 1.4 times the average thickness of the skin; the length and width of the auxiliary plate are consistent with the length and width of the outer grid wall panel.
[0020] Furthermore, second through holes corresponding to the first through holes are provided at four corners of the auxiliary plate.
[0021] Furthermore, two parallel baffles are provided on the molding mold surface, and the horizontal distance between the two baffles is greater than the width of the outer grid wall panel; the bottom arc radius of the baffle is adapted to the radius of the mold surface, and the height of the baffle is greater than the sum of the chord height of the outer grid wall panel and the thickness of the outer grid wall panel.
[0022] Furthermore, the horizontal distance between the two baffles is 10-20 mm greater than the width of the outer grid wall panel; the height of the baffle is 50-100 mm greater than the sum of the flat plate chord height of the outer grid wall panel and the thickness of the outer grid wall panel.
[0023] Furthermore, a reinforcing rib is provided on the outward side of the baffle, a first mounting hole is provided at the bottom of the baffle, and a second mounting hole corresponding to the first mounting hole is provided on the mold surface.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The present invention discloses a method for suppressing the depression of the skin during the creep aging forming process of the outer grid wall panel, by adding fillers to the corresponding grid of the thinner skin, adding auxiliary plates to the smooth surface of the outer grid wall panel, and then covering the whole with breathable felt and vacuum bags, and using vacuum to make the auxiliary plates and the smooth surface of the outer grid wall panel always keep in contact, and then the above-mentioned whole is sealed with the mold surface, and the formed outer grid wall panel is obtained after creep aging in the tank. The method of the present invention adds auxiliary plates and fillers, and uses the auxiliary plates and fillers to suppress the depression of the skin area together, wherein the auxiliary plates can be always in contact with the smooth surface of the outer grid wall panel by vacuuming, and can also be fixed by bolts to make the two fit. The method of the present invention can effectively suppress the depression of the skin, improve the forming accuracy of the outer grid wall panel formed by creep aging forming technology, and can effectively extend the service life of the formed outer grid wall panel.
[0026] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings are used to provide a further understanding of the embodiments of the present invention and constitute a part of the specification. Together with the following specific implementations, they are used to explain the embodiments of the present invention, but do not constitute a limitation on the embodiments of the present invention. In the accompanying drawings:
[0028] Figure 1 It is a flow chart of a method for suppressing skin depression during creep aging forming of an outer grid wall panel according to the present invention;
[0029] Figure 2 It is a schematic diagram of the three-dimensional structure of the outer grid wall panels of the present invention;
[0030] Figure 3 It is a schematic diagram of the top view structure of the outer grid wall panels of the present invention;
[0031] Figure 4 is a schematic diagram of the top view of the auxiliary plate in the present invention;
[0032] Figure 5 It is a structural schematic diagram of the baffle in the present invention;
[0033] Figure 6 It is a schematic diagram of the structure of the outer grid wall panels (assembled with fillers and auxiliary panels, etc.) in the present invention in cooperation with the forming mold;
[0034] Among them, 1-external grid wall panel; 1.1-remaining reserved area; 1.2-first through hole; 2-molding mold; 3-filler; 4-auxiliary plate; 4.1-second through hole; 5-baffle; 5.1-reinforcement rib; 5.2-first mounting hole. DETAILED DESCRIPTION
[0035] The present invention will be described in detail below in conjunction with the various embodiments shown in the accompanying drawings, but it should be noted that these embodiments are not limitations of the present invention, and any equivalent transformations or substitutions in functions, methods, or structures made by ordinary technicians in the field based on these embodiments are all within the scope of protection of the present invention.
[0036] See also Figures 1 to 6 This embodiment provides a method for suppressing the skin depression during the creep aging forming process of the outer grid wall panel, wherein the material of the outer grid wall panel 1 is 7050-T7451, and the specific process parameters of creep are: loading pressure 1.5MPa, aging time 1.3h, aging temperature 180℃; comprising the following steps:
[0037] 1. Obtain the distribution characteristics of the skin thickness of different regions of the outer grid wall panel 1; wherein, the four corners of the margin reserved area 1.1 of the outer grid wall panel 1 are respectively provided with first through holes 1.2; specifically, the width of the margin reserved area is 0.3-0.5 times the width of a single grid, and the diameter of the first through hole 1.2 is 5-8 mm. In this step, the thickness of the skin of different regions of the outer grid wall panel can be actually measured by an ultrasonic thickness gauge, or the thickness of the skin of different regions of the outer grid wall panel can be obtained by using the thickness analysis function of computer software.
[0038] 2. Select appropriate auxiliary plate 4 according to the average thickness of the skin. The thickness of the auxiliary plate 4 is selected according to the average thickness of the skin; wherein, the average thickness of the skin T The calculation of is as follows:
[0039]
[0040] in, i is the skin thickness type, t i For different skin thicknesses, S i for t i Corresponding skin area. Specifically, the thickness of the auxiliary plate 4 is 0.8 to 1.4 times the average thickness of the skin; the length and width of the auxiliary plate 4 are consistent with the length and width of the outer grid wall panel 1; the auxiliary plate can be a steel plate, an aluminum plate, etc.
[0041] 3. Add filler 3 to the mesh area corresponding to the thinner skin area. The size of filler 3 is 0.9-0.97 times the size of the mesh area corresponding to the thinner skin area. The material of filler 3 is silicone or high-temperature resistant rubber. The filler and the skin surface are attached with high-temperature resistant double-sided tape. The thinner skin area is thicker. t <15% h of the region, h is the rib height of the outer grid wall panel.
[0042] 4. Fasten the outer grid wall plate 1 and the auxiliary plate 4 with four sets of bolts and nuts, and keep the bolts, the first through hole 1.2 and the second through hole 4.1 coaxially aligned.
[0043] 5. Wrap the whole with a layer of breathable felt and wrap the breathable felt with heat-resistant tape to tighten it; then wrap the whole with a first vacuum bag, seal it and evacuate it to ensure that the auxiliary plate fits the smooth surface of the outer grid wall panel; obtain a vacuum-wrapped part.
[0044] 6. Wrap a layer of breathable felt on the surface of the vacuum-coated part; then place the vacuum-coated part wrapped with the breathable felt on the molding surface of the molding mold 2 and accurately position it.
[0045] 7. Use a second vacuum bag to completely cover and seal the mold surface and the vacuum covering member wrapped with the breathable felt to obtain an integral wall panel forming tooling.
[0046] 8. The integral forming device of the wall panel is placed in a hot press tank, the outside of the tank is vacuumed, the inside of the tank is kept warm and loaded, and the formed outer grid wall panel can be obtained after creep aging.
[0047] In a specific embodiment of the present invention, if the chord height of the flat plate state of the outer grid wall panel 1 is too high, in order to prevent the vacuum bag from being pulled during vacuuming and being sucked into the bottom of the wall panel and breaking, a baffle 5 can be added to the mold surface, and the outer grid wall panel 1, the baffle 5 and the mold surface are sealed together during vacuum sealing. Specifically, two parallel baffles 5 are provided on the surface of the molding mold 2, and the horizontal distance between the two baffles 5 is 10~20mm larger than the width of the outer grid wall panel 1; the height of the baffle 5 is 50~100mm greater than the sum of the flat chord height of the outer grid wall panel 1 and the thickness of the outer grid wall panel 1. A reinforcing rib 5.1 is provided on the outward side of the baffle 5, and the bottom arc radius of the baffle 5 is adapted to the radius of the mold surface. A first mounting hole 5.2 is opened at the bottom of the baffle 5, and a second mounting hole corresponding to the first mounting hole 5.2 is opened on the mold surface. In this structural setting, reinforcing ribs are provided on the outer side of the baffle, which can increase the structural rigidity and reduce weight. The bottom of the baffle plate is opened with holes on the mold surface and fixed with bolts to achieve disassembly and movement. At the same time, the bottom of the mold surface needs to be welded with a pad to ensure the depth and air tightness of the screw hole.
[0048] The external grid wall panel formed by the method of the embodiment of the present invention has a residual stress between -33MPa and 90MPa, which is generally low; the change in film adhesion and straightness before and after process allowance milling is ≤0.4mm; samples are taken from the process allowance skin and ribs to measure performance, which meets the standard requirements.
[0049] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for suppressing the skin depression during the creep aging forming process of the outer grid wall panel, It is characterized in that include: Step S1, obtaining the distribution characteristics of the skin thickness of different areas of the outer grid wall panel (1); wherein the four corners of the surplus reserved area (1.1) of the outer grid wall panel (1) are provided with first through holes (1.2); Step S2: according to the distribution characteristics of the skin thickness, filler (3) is added to the grid area corresponding to the thinner skin area, wherein the thinner skin area is the thickness t <15% h of the region, h is the rib height of the outer grid wall panel (1); the size of the filler (3) is 0.9-0.97 times the size of the grid area corresponding to the thinner area of the skin; the material of the filler (3) is silicone or high-resistant rubber; the thickness of the auxiliary plate (4) is selected according to the average thickness of the skin; wherein the average thickness of the skin T The calculation of is as follows: in, i is the skin thickness type, t i For different skin thicknesses, S i for t i The corresponding skin area; The thickness of the auxiliary plate (4) is 0.8 to 1.4 times the average thickness of the skin; the length and width of the auxiliary plate (4) are consistent with the length and width of the outer grid wall panel (1); Step S3, first placing the auxiliary plate (4) in contact with the smooth surface of the outer grid wall panel (1), then coating the surface of the outer grid wall panel (1) and the auxiliary plate (4) with a layer of breathable felt, then wrapping the breathable felt with a heat-resistant tape to obtain a whole wall panel; then sealing the whole wall panel with a first vacuum bag, and evacuating the first vacuum bag so that the auxiliary plate (4) and the smooth surface of the outer grid wall panel (1) are tightly fitted to obtain a vacuum-coated part; Step S4, wrapping the surface of the vacuum-coated part with a layer of air-permeable felt, and then placing the vacuum-coated part wrapped with the air-permeable felt on the molding surface of the molding mold (2), and installing and positioning it; Step S5, using a second vacuum bag to completely cover and seal the mold surface and the vacuum covering member wrapped with the breathable felt to obtain an integrally formed wall panel tooling; Step S6, placing the integrally formed wall panel in a hot press, evacuating the outside of the tank, keeping the inside of the tank warm and loaded, and obtaining the formed outer grid wall panel after creep aging.
2. The method according to claim 1, It is characterized in that Second through holes (4.1) corresponding to the first through holes (1.2) are arranged at four corners of the auxiliary plate (4).
3. The method according to claim 1, It is characterized in that Two parallel baffles (5) are provided on the molding surface of the molding die (2); the horizontal distance between the two baffles (5) is greater than the width of the outer grid wall panel (1); the bottom arc radius of the baffle (5) is matched to the radius of the molding surface; the height of the baffle (5) is greater than the sum of the flat plate chord height of the outer grid wall panel (1) and the thickness of the outer grid wall panel (1).
4. The method according to claim 3, It is characterized in that The horizontal distance between the two baffles (5) is 10-20 mm greater than the width of the outer grid wall panel (1); the height of the baffle (5) is 50-100 mm greater than the sum of the flat plate chord height of the outer grid wall panel (1) and the thickness of the outer grid wall panel (1).
5. The method according to claim 3, It is characterized in that A reinforcing rib (5.1) is provided on the outward side of the baffle (5), a first mounting hole (5.2) is provided at the bottom of the baffle (5), and a second mounting hole corresponding to the first mounting hole (5.2) is provided on the mold surface.
Citation Information
Patent Citations
A method for processing internal and external meshes of rocket short shell panels
CN111774814B
A mechanical loading fixture and loading method for external mesh wall panels
CN113000682B
Creep age forming method for large thin-wall component
CN111195677A
Economical creep aging forming method of large thin-wall component
CN111195678A
Male die vacuum loading tool and manufacturing and forming method of outer grid wallboard
CN113000683A
Cited By
Creep age forming method for variable-thickness high-rib component
CN119346703A
Creep aging forming method for variable thickness high-rib components
CN119346703B