A high flame retardant flame retardant composite additive and polypropylene composite material
By combining 1/2 carboxylated silsesquioxane with hydrotalcite and modified hydrotalcite, a high flame retardant composite additive was prepared and combined with flame retardant containing nitrogen, phosphorus and silicon, the solution was solved The problems of flammability and slow crystallization speed of polypropylene materials have significantly improved their flame retardant properties and mechanical properties, achieving wider applications.
Patent Information
- Application Number
- CN202410619778.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-17
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-05-17
AI Technical Summary
The flammability and combustible dripability of polypropylene materials limit their application range, and they have slow crystallization speed and low toughness, making it difficult to widely use in more fields.
Using a high flame retardant flame retardant composite additive preparation method, the excellent ones are prepared by combining 1/2 carboxylated silsesquioxane with hydrotalcite and modified hydrotalcite, and ultrasonic dispersion and carboxylation treatment. Flame retardant composite additives with thermal stability and dispersion properties, and are used together with flame retardants containing nitrogen, phosphorus and silicon to improve the flame retardant and mechanical properties of polypropylene composite materials.
The flame retardant performance, crystallization speed and mechanical properties of polypropylene composite materials have been significantly improved, solving the problems of environmental pollution, high volatility and poor heat resistance of traditional flame retardants, and at the same time improving the dispersion performance and production efficiency.
Smart Images

Figure BDA0004846499750000071 
Figure BDA0004846499750000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame retardant composite additives, in particular to a highly flame retardant flame retardant composite additive and a polypropylene composite material. Background Art
[0002] Polypropylene (PP) is widely used in many fields such as electronics, automobiles, interior decoration, etc. due to its excellent mechanical properties, good chemical properties and low cost. However, its flammability and burning dripping properties severely limit its scope of application. In order to improve the flame retardant properties of PP, the method of adding flame retardants is usually adopted. Commonly used flame retardants include halogen, phosphorus and inorganic hydroxides. Halogen flame retardants are highly efficient but cause great environmental pollution, phosphorus flame retardants are highly volatile and have poor heat resistance, and inorganic hydroxide flame retardants are environmentally friendly but require large amounts.
[0003] At the same time, polypropylene has a relatively slow crystallization rate and low toughness, which further limits its application in more fields. Therefore, it is of great significance to invent a highly flame retardant flame retardant composite additive and a polypropylene composite material to improve the flame retardancy, crystallization rate and mechanical properties of the polypropylene composite material. Summary of the invention
[0004] The object of the present invention is to provide a highly flame retardant flame retardant composite auxiliary agent and a polypropylene composite material to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A method for preparing a highly flame retardant flame retardant composite auxiliary agent comprises the following steps:
[0007] 1 / 2 of the carboxylated silsesquioxane is added to deionized water, and hydrotalcite and modified hydrotalcite are added, and ultrasonic dispersion is performed to obtain a suspension; the suspension is added to the remaining 1 / 2 of the carboxylated silsesquioxane, and the mixture is heated to 60-65° C. and stirred for reaction for 2-2.5 hours to obtain a highly flame retardant flame retardant composite auxiliary agent.
[0008] Furthermore, the preparation method of the hydrotalcite comprises the following steps:
[0009] Aluminum nitrate nonahydrate and zinc nitrate hexahydrate are added to deionized water and stirred evenly to obtain a salt solution; the salt solution is preheated to 75-80° C., added to a sodium carbonate solution, stirred at a constant temperature for 2-2.5 hours, crystallized for 7.5-8 hours, centrifuged, washed, and freeze-dried to obtain hydrotalcite;
[0010] Furthermore, the molar ratio of zinc nitrate hexahydrate to aluminum nitrate nonahydrate is 3:1.
[0011] Furthermore, the preparation method of the modified hydrotalcite comprises the following steps:
[0012] Add 3-aminopropyltriethoxysilane to an ethanol aqueous solution, adjust the pH to 10, and hydrolyze for 2 hours to obtain a silane hydrolyzate; add aluminum nitrate nonahydrate, zinc nitrate hexahydrate, and a silane hydrolyzate to the ethanol aqueous solution, stir evenly, and obtain a salt silane solution; preheat the salt silane solution to 75-80° C., stir and react at a constant temperature for 1-1.5 hours, crystallize for 24 hours, centrifuge, wash, and vacuum dry to obtain a modified hydrotalcite;
[0013] Furthermore, in the silane hydrolyzate, the volume ratio of 3-aminopropyltriethoxysilane to ethanol aqueous solution is 1:40;
[0014] Furthermore, in the modified hydrotalcite, the molar ratio of zinc nitrate hexahydrate: aluminum nitrate nonahydrate: 3-aminopropyltriethoxysilane in the silane hydrolyzate is 1:(1-2):(1-2).
[0015] Furthermore, the method for preparing the carboxylated silsesquioxane comprises the following steps:
[0016] Vinyl trimethylsiloxane, acetone, concentrated hydrochloric acid and deionized water are stirred and reacted for 48 hours, washed and filtered to obtain vinyl silsesquioxane; vinyl silsesquioxane, 1 / 2 methacrylic acid, 1 / 2 itaconic acid and sodium dodecyl sulfate are added to deionized water, ultrasonically dispersed, 1 / 2 ammonium persulfate is added, heated to 60-65°C for reaction for 30-45 minutes, the remaining 1 / 2 ammonium persulfate, sodium bisulfate, deionized water, the remaining 1 / 2 methacrylic acid and the remaining 1 / 2 itaconic acid are added, and the reaction is kept warm for 3-3.5 hours to obtain carboxylated silsesquioxane;
[0017] Furthermore, the proportions of the components in the vinylated silsesquioxane are, by weight, 10-20 parts of vinyl trimethylsiloxane, 100-200 parts of acetone, 15-20 parts of concentrated hydrochloric acid, and 25-40 parts of deionized water;
[0018] Furthermore, the proportions of the components in the carboxylated silsesquioxane are, by mass, 0.2-0.4 parts of vinyl silsesquioxane, 6-8 parts of methacrylic acid, 6-16 parts of itaconic acid, 0.3-0.5 parts of sodium dodecyl sulfate, 2.4-3 parts of ammonium persulfate, and 0.3-0.4 parts of sodium hydrogen sulfate; wherein the mass ratio of methacrylic acid to itaconic acid is 1:(1-2).
[0019] Furthermore, in the highly flame-retardant flame-retardant composite auxiliary agent, the mass ratio of carboxylated silsesquioxane: hydrotalcite: modified hydrotalcite is (20-40): (1-2): (1-2).
[0020] Furthermore, the polypropylene composite material prepared by the highly flame retardant flame retardant composite auxiliary agent comprises the following components, measured by mass: 80-100 parts of polypropylene, 15-30 parts of the highly flame retardant flame retardant composite auxiliary agent, 12-25 parts of flame retardant, 1.2 parts of itaconic acid, 0.2-0.6 parts of nano-alumina particles, 6-8 parts of epoxy soybean oil, and 20-25 parts of ethylene acrylic acid copolymer; wherein the mass ratio of the highly flame retardant flame retardant composite auxiliary agent to the flame retardant is (5-6):(4-5).
[0021] Furthermore, the method for preparing the flame retardant comprises the following steps:
[0022] Heat DOPO to 130-135°C, add triglycidyl isocyanurate after it is completely melted, stir evenly, add N,N-dimethylacetamide, heat to 160-165°C, react for 3-3.5h, distill under reduced pressure, wash, and vacuum dry to obtain a flame retardant.
[0023] Furthermore, in the flame retardant, the molar ratio of DOPO to triglycidyl isocyanurate is 1:(1-3).
[0024] Furthermore, the preparation method of the polypropylene composite material comprises the following steps:
[0025] Preheat the mixer to 160-190°C, add 1 / 2 polypropylene, high flame retardant flame retardant composite additive, itaconic acid, nano alumina particles, stir and mix for 6-8 minutes, add flame retardant, epoxy soybean oil, ethylene acrylic acid copolymer, remaining 1 / 2 polypropylene, stir and mix for 10-15 minutes, heat to 190-210°C, extrude and granulate to obtain a polypropylene composite material.
[0026] In the above technical solutions, the concentration of the ethanol aqueous solution is 25% v / v, and the concentration of the concentrated hydrochloric acid is 12 mol / L.
[0027] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0028] The invention selects aluminum nitrate nonahydrate and zinc nitrate hexahydrate as trivalent metal nitrate and divalent metal nitrate respectively, and selects appropriate molar ratio and crystallization time to prepare zinc-aluminum hydrotalcite; compared with traditional aluminum, copper-aluminum and cobalt-aluminum hydrotalcites, the zinc-aluminum hydrotalcite prepared by the invention has excellent thermal stability and heat insulation effect in the thermal decomposition process, because the prepared zinc-aluminum hydrotalcite has regular lamella morphology and uniform thickness, and the surface is smooth without fine granular precipitation.
[0029] The invention uses 3-aminopropyltriethoxysilane as a silane hydrolysis system and prepares the modified hydrotalcite by an in-situ generation method. Compared with the traditional hydrotalcite, the edge growth of the hydrotalcite is inhibited in the in-situ generation process due to the early coating of silanol by silane hydrolysis, resulting in an incomplete lamella morphology of the hydrotalcite, which presents a partially refined particle shape and a reduced particle size, thereby greatly improving the dispersibility of the modified hydrotalcite in a polypropylene matrix. At the same time, since one silanol group of the silanol by silane hydrolysis is coupled with the lamella hydroxyl group of the hydrotalcite, and the other end hydroxyl group is coated on the surface of the hydrotalcite, the surface energy of the modified hydrotalcite is greatly reduced, and the dispersibility of the modified hydrotalcite in the polypropylene matrix is further improved.
[0030] The present invention uses carboxylated silsesquioxane to simultaneously perform carboxylation modification treatment on hydrotalcite and modified hydrotalcite to prepare a highly flame retardant flame retardant composite auxiliary agent. On the one hand, the zinc-aluminum hydrotalcite and the modified hydrotalcite are peeled off under the combined action of carboxylated silsesquioxane and ultrasound, and the combined action of the peeling and reorganization modification treatment and the low surface energy of the modified hydrotalcite further improves its dispersion performance in the matrix while retaining the regular morphology and uniform thickness characteristics of the zinc-aluminum hydrotalcite layer (i.e., excellent thermal stability and heat insulation effect during thermal decomposition). The highly flame retardant flame retardant composite auxiliary agent decomposes into silicon oxide compounds and spinel oxides during combustion, has excellent barrier effect and flame retardant and smoke suppression performance, and the alternately linked silicon oxide skeleton and spinel oxides generate a cross-linked structure through the catalytic carbonization effect to generate a dense carbon layer, which isolates the transfer and release of heat and greatly improves the flame retardant performance.
[0031] In order to further improve the flame retardant performance, the present invention uses triglycidyl isocyanurate and DOPO as raw materials to prepare a flame retardant, which together with the previously prepared high flame retardant flame retardant composite auxiliary agent, forms a flame retardant containing nitrogen, phosphorus and silicon. The high flame retardant flame retardant composite auxiliary agent and the flame retardant are added separately to the mixer, the purpose of which is to improve the mechanical properties, flame retardant properties, crystallization rate and production efficiency of the polypropylene composite material, and at the same time improve the dispersion performance of the flame retardant and the high flame retardant flame retardant composite auxiliary agent in the matrix.
[0032] The present invention first uses half of the polypropylene as a matrix, adds a highly flame-retardant flame-retardant composite auxiliary agent, itaconic acid, and nano zinc oxide particles, and uses the itaconic acid structure in the highly flame-retardant composite auxiliary agent structure and the nano zinc oxide particles to in-situ prepare zinc itaconic acid as a β-nucleating agent to modify the polypropylene composite material. Compared with the traditional method of directly adding zinc itaconic acid, when a certain amount of zinc itaconic acid is directly added, the zinc itaconic acid will agglomerate in the polypropylene matrix, thereby inhibiting the formation of β crystals. The present invention can use a highly flame-retardant composite auxiliary agent as a carrier, greatly improve the dispersion performance of zinc itaconic acid in the polypropylene matrix, solve the problem of easy agglomeration of zinc itaconic acid added directly in the traditional method, and at the same time increase the amount of itaconic acid in the polypropylene matrix, thereby improving the ability to induce polypropylene to form β crystals, and greatly improving the mechanical properties of the polypropylene composite material. If polypropylene, highly flame-retardant flame-retardant composite additives, itaconic acid, flame retardants, nano zinc oxide particles, epoxy soybean oil, and ethylene acrylic acid copolymer are heated and blended at the same time without any particular order, and melt extruded, the conversion rate of zinc itaconate will be reduced, and its proportion in the polypropylene composite material will be reduced. The reason is that the carboxylic acid group in the structure of the highly flame-retardant flame-retardant composite additive will react with the epoxy group of the reactive compatibilizer epoxy soybean oil and the epoxy group in the flame retardant, resulting in a reduction in the itaconic acid carboxylic acid structure, which affects the conversion efficiency of zinc itaconate.
[0033] The invention prepares a polypropylene composite material by adding residual polypropylene, a flame retardant, epoxy soybean oil and an ethylene acrylic acid copolymer for blending and melt extrusion; the epoxy soybean oil is used as a reactive compatibilizer, and the epoxy group in the flame retardant structure is matched with the carboxylic acid group in the ethylene acrylic acid copolymer and the structure of a highly flame retardant flame retardant composite auxiliary agent; the generated graft copolymer is distributed at the interface of each phase to form a cross-linked network structure; on the one hand, the dispersibility and compatibility of the highly flame retardant flame retardant composite auxiliary agent, the flame retardant and the ethylene acrylic acid copolymer in the polypropylene composite material are improved; on the other hand, the mechanical properties and flame retardant properties of the polypropylene composite material are enhanced. DETAILED DESCRIPTION
[0034] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] In the following examples, the polypropylene model is EPS30R, the melt flow rate is 1.2 g / 10 min, and the density is 0.905 g / cm 3, purchased from Xinjiang Dushanzi Petrochemical Co., Ltd., China; ethylene acrylic acid copolymer model 1410, purchased from Dow Chemical Company, USA; nano zinc oxide particles CAS1314-13-2, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; epoxidized soybean oil model E8088, epoxide value 6.5%, Mw = 975.399, purchased from Shanghai McLean Biochemical Technology Co., Ltd., and the remaining raw materials are commercially available.
[0036] The preparation method of the flame retardant in the following embodiment comprises the following steps: heating DOPO to 130° C., adding triglycidyl isocyanurate after it is completely melted, stirring evenly, adding N,N-dimethylacetamide, heating to 160° C. for reaction for 3 hours, distilling under reduced pressure, washing, and vacuum drying to obtain a flame retardant;
[0037] The molar ratio of DOPO to triglycidyl isocyanurate is 1:1.
[0038] Embodiment 1: A method for preparing a polypropylene composite material with a highly flame retardant flame retardant composite auxiliary agent: S1: adding aluminum nitrate nonahydrate and zinc nitrate hexahydrate to deionized water, stirring evenly to obtain a salt solution; preheating the salt solution to 80°C, adding it to a sodium carbonate solution, stirring and reacting at a constant temperature for 2 hours, crystallizing for 8 hours, centrifuging, washing, and freeze-drying to obtain hydrotalcite; wherein the molar ratio of zinc nitrate hexahydrate to aluminum nitrate nonahydrate is 3:1;
[0039] S2: Add 1 mL of 3-aminopropyltriethoxysilane to 40 mL of ethanol aqueous solution, adjust the pH to 10, and hydrolyze for 2 hours to obtain a silane hydrolyzate; add aluminum nitrate nonahydrate, zinc nitrate hexahydrate, and silane hydrolyzate to the ethanol aqueous solution, stir evenly, and obtain a salt silane solution; preheat the salt silane solution to 75-80°C, stir and react at a constant temperature for 1-1.5 hours, crystallize for 24 hours, centrifuge, wash, and vacuum dry to obtain a modified hydrotalcite; wherein the molar ratio of zinc nitrate hexahydrate: aluminum nitrate nonahydrate: 3-aminopropyltriethoxysilane in the silicon hydrolyzate is 1:1:1;
[0040] S3: 10g of vinyl trimethylsiloxane, 100g of acetone, 15g of concentrated hydrochloric acid, and 25g of deionized water were stirred for reaction for 48h, washed, and filtered to obtain vinyl silsesquioxane; 0.2g of vinyl silsesquioxane, 3g of methacrylic acid, 6g of itaconic acid, and sodium dodecyl sulfate were added to 20g of deionized water, ultrasonically dispersed, 1.2g of ammonium persulfate was added, heated to 60°C for reaction for 30min, and the remaining 1.2g of ammonium persulfate, 0.3g of sodium bisulfate, 15g of deionized water, the remaining 3g of methacrylic acid, and the remaining 6g of itaconic acid were added, and the reaction was kept warm for 3-3.5h to obtain carboxylated silsesquioxane;
[0041] S4: Add 10g of carboxylated silsesquioxane to deionized water, add 1g of hydrotalcite and 1g of modified hydrotalcite, and disperse by ultrasonication to obtain a suspension; add the suspension to the remaining 10g of carboxylated silsesquioxane, heat to 60°C, stir and react for 2h, and obtain a highly flame retardant flame retardant composite additive.
[0042] S5: Preheat the mixer to 190°C, add 50g polypropylene, 15g high flame retardant flame retardant composite additive, 1g itaconic acid, 0.2g nano alumina particles, stir and mix for 6min, add 15g flame retardant, 6g epoxy soybean oil, 20g ethylene acrylic acid copolymer, and the remaining 50g polypropylene, stir and mix for 10min, heat to 200°C, extrude and granulate to obtain a polypropylene composite material.
[0043] Example 2: A method for preparing a polypropylene composite material with a highly flame retardant flame retardant composite auxiliary agent: S5: Preheat the mixer to 190°C, add 50g polypropylene, 15g highly flame retardant flame retardant composite auxiliary agent, 1g itaconic acid, 0.6g nano alumina particles, stir and mix for 6 minutes, add 15g flame retardant, 6g epoxy soybean oil, 20g ethylene acrylic acid copolymer, and the remaining 50g polypropylene, stir and mix for 10 minutes, heat to 200°C, extrude and granulate to obtain a polypropylene composite material.
[0044] The remaining steps are the same as those in Example 1.
[0045] Example 3: A method for preparing a polypropylene composite material with a highly flame retardant flame retardant composite auxiliary agent: S5: Preheat the mixer to 190°C, add 50g polypropylene, 25g highly flame retardant flame retardant composite auxiliary agent, 1g itaconic acid, 0.6g nano alumina particles, stir and mix for 7min, add 25g flame retardant, 6g epoxy soybean oil, 20g ethylene acrylic acid copolymer, and the remaining 50g polypropylene, stir and mix for 12min, heat to 200°C, extrude and granulate to obtain a polypropylene composite material.
[0046] The remaining steps are the same as those in Example 1.
[0047] Comparative Example 1: A method for preparing a polypropylene composite material with a highly flame retardant flame retardant composite additive: S1: Add aluminum nitrate nonahydrate and zinc nitrate hexahydrate to deionized water, stir evenly to obtain a salt solution; preheat the salt solution to 80°C, add it to a sodium carbonate solution, stir and react at a constant temperature for 2 hours, crystallize for 8 hours, centrifuge, wash, and freeze-dry to obtain hydrotalcite; wherein the molar ratio of zinc nitrate hexahydrate to aluminum nitrate nonahydrate is 3:1;
[0048] The remaining steps are the same as those in Example 1.
[0049] Comparative Example 2: A method for preparing a polypropylene composite material with a highly flame retardant flame retardant composite auxiliary agent: S1: Add aluminum nitrate nonahydrate and zinc nitrate hexahydrate to deionized water, stir evenly to obtain a salt solution; preheat the salt solution to 80°C, add it to a sodium carbonate solution, stir and react at a constant temperature for 2 hours, crystallize for 8 hours, centrifuge, wash, and freeze-dry to obtain hydrotalcite; wherein the molar ratio of zinc nitrate hexahydrate to aluminum nitrate nonahydrate is 3:1;
[0050] S2: 10g of vinyl trimethylsiloxane, 100g of acetone, 15g of concentrated hydrochloric acid, and 25g of deionized water were stirred for reaction for 48h, washed, and filtered to obtain vinyl silsesquioxane; 0.2g of vinyl silsesquioxane, 3g of methacrylic acid, 6g of itaconic acid, and sodium dodecyl sulfate were added to 20g of deionized water, ultrasonically dispersed, 1.2g of ammonium persulfate was added, heated to 60°C for reaction for 30min, and the remaining 1.2g of ammonium persulfate, 0.3g of sodium bisulfate, 15g of deionized water, the remaining 3g of methacrylic acid, and the remaining 6g of itaconic acid were added, and the reaction was kept warm for 3-3.5h to obtain carboxylated silsesquioxane;
[0051] S3: 10 g of carboxylated silsesquioxane was added to deionized water, and 2 g of hydrotalcite was added, and ultrasonic dispersion was performed to obtain a suspension; the suspension was added to the remaining 10 g of carboxylated silsesquioxane, and the mixture was heated to 60° C. and stirred for reaction for 2 h to obtain a highly flame retardant flame retardant composite auxiliary agent.
[0052] S4: Preheat the mixer to 190°C, add 50g polypropylene, 15g high flame retardant flame retardant composite additive, 1g itaconic acid, 0.2g nano alumina particles, stir and mix for 6min, add 15g flame retardant, 6g epoxy soybean oil, 20g ethylene acrylic acid copolymer, and the remaining 50g polypropylene, stir and mix for 10min, heat to 200°C, extrude and granulate to obtain a polypropylene composite material.
[0053] Comparative Example 3: A method for preparing a polypropylene composite material with a highly flame retardant flame retardant composite auxiliary agent: S5: Preheat the mixer to 190°C, add 50g polypropylene, 15g highly flame retardant flame retardant composite auxiliary agent, 0.2g zinc itaconate, stir and mix for 6min, add 15g flame retardant, 6g epoxy soybean oil, 20g ethylene acrylic acid copolymer, and the remaining 50g polypropylene, stir and mix for 10min, heat to 200°C, extrude and granulate, and obtain a polypropylene composite material.
[0054] The remaining steps are the same as those in Example 1.
[0055] Comparative Example 4: A method for preparing a polypropylene composite material with a highly flame retardant flame retardant composite auxiliary agent: S5: Preheat the mixer to 190°C, add 100g polypropylene, 15g highly flame retardant flame retardant composite auxiliary agent, 1g itaconic acid, 0.2g nano alumina particles, 15g flame retardant, 6g epoxy soybean oil, and 20g ethylene acrylic acid copolymer, stir and mix for 15 minutes, heat to 200°C, extrude and granulate to obtain a polypropylene composite material.
[0056] Experiment: Limiting oxygen index LOI test: Tested according to GB / T 2406-2009, the sample size is 80mm×10mm×4mm;
[0057] Tensile performance test: The test was conducted in accordance with GB / T 1040-2006, with a tensile speed of 50 mm / min, a specimen thickness of 2 mm, a narrow portion width of 4 mm, and each group was tested 5 times, and the average value of the results was taken.
[0058] Table 1 Polypropylene composite material performance test data table
[0059]
[0060]
[0061] Conclusion: The polypropylene composite material with high flame retardancy and flame retardant composite additive prepared by the present invention has excellent flame retardant properties and mechanical properties.
[0062] Comparative Example 1: The hydrotalcite was prepared in a conventional magnesium-aluminum hydrotalcite manner, resulting in irregular lamellae morphology, uneven thickness, and rough surface, which reduced the flame retardancy of the polypropylene composite material.
[0063] Comparative Example 2 uses only a single hydrotalcite, and does not use a composite hydrotalcite containing modified hydrotalcite, which results in reduced dispersion performance, and reduces the flame retardant properties and mechanical properties of the polypropylene composite material.
[0064] In Comparative Example 3, direct addition of zinc itaconate resulted in agglomeration, which reduced the mechanical properties of the polypropylene composite material.
[0065] In Comparative Example 4, the raw material components are directly melt-blended and extruded without any particular order, resulting in reduced mechanical properties of the polypropylene composite material.
[0066] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a highly flame retardant flame retardant composite auxiliary agent, characterized in that: The following steps are involved: Add 1 / 2 of the carboxylated silsesquioxane to deionized water, add hydrotalcite and modified hydrotalcite, and disperse by ultrasonication to obtain a suspension; add the suspension to the remaining 1 / 2 of the carboxylated silsesquioxane, heat to 60-65° C., stir and react for 2-2.5 hours, and obtain a highly flame retardant flame retardant composite additive; The preparation method of the hydrotalcite comprises the following steps: Aluminum nitrate nonahydrate and zinc nitrate hexahydrate are added to deionized water and stirred evenly to obtain a salt solution; the salt solution is preheated to 75-80° C., added to a sodium carbonate solution, stirred at a constant temperature for 2-2.5 hours, crystallized for 7.5-8 hours, centrifuged, washed, and freeze-dried to obtain hydrotalcite; The molar ratio of zinc nitrate hexahydrate to aluminum nitrate nonahydrate is 3:1; The preparation method of the modified hydrotalcite comprises the following steps: 3-aminopropyltriethoxysilane was added to an ethanol aqueous solution, the pH was adjusted to 10, and the solution was hydrolyzed for 2 hours to obtain a silane hydrolyzate; aluminum nitrate nonahydrate, zinc nitrate hexahydrate, and the silane hydrolyzate were added to the ethanol aqueous solution, and the mixture was stirred evenly to obtain a salt silane solution; Preheat the salt silane solution to 75-80°C, stir and react at constant temperature for 1-1.5 hours, crystallize for 24 hours, centrifuge, wash, and vacuum dry to obtain modified hydrotalcite; In the silane hydrolyzate, the volume ratio of 3-aminopropyltriethoxysilane to ethanol aqueous solution is 1:40; In the modified hydrotalcite, the molar ratio of zinc nitrate hexahydrate: aluminum nitrate nonahydrate: 3-aminopropyltriethoxysilane in the silane hydrolyzate is 1:(1-2):(1-2); In the highly flame-retardant flame-retardant composite auxiliary agent, the mass ratio of carboxylated silsesquioxane: hydrotalcite: modified hydrotalcite is (20-40): (1-2): (1-2).
2. The method for preparing a highly flame retardant flame retardant composite auxiliary agent according to claim 1, characterized in that: The preparation method of the carboxylated silsesquioxane comprises the following steps: Vinyl trimethylsiloxane, acetone, concentrated hydrochloric acid and deionized water are stirred and reacted for 48 hours, washed and filtered to obtain vinyl silsesquioxane; vinyl silsesquioxane, 1 / 2 methacrylic acid, 1 / 2 itaconic acid and sodium dodecyl sulfate are added to deionized water, ultrasonically dispersed, 1 / 2 ammonium persulfate is added, heated to 60-65°C for reaction for 30-45 minutes, the remaining 1 / 2 ammonium persulfate, sodium bisulfate, deionized water, the remaining 1 / 2 methacrylic acid and the remaining 1 / 2 itaconic acid are added, and the reaction is kept warm for 3-3.5 hours to obtain carboxylated silsesquioxane; The proportions of the components in the vinylated silsesquioxane are, by weight, 10-20 parts of vinyl trimethylsiloxane, 100-200 parts of acetone, 15-20 parts of concentrated hydrochloric acid, and 25-40 parts of deionized water; The proportions of the components in the carboxylated silsesquioxane are, by mass, 0.2-0.4 parts of vinyl silsesquioxane, 6-8 parts of methacrylic acid, 6-16 parts of itaconic acid, 0.3-0.5 parts of sodium dodecyl sulfate, 2.4-3 parts of ammonium persulfate, and 0.3-0.4 parts of sodium hydrogen sulfate; wherein the mass ratio of methacrylic acid to itaconic acid is 1:(1-2).
3. A highly flame retardant flame retardant composite auxiliary agent prepared according to the method for preparing a highly flame retardant flame retardant composite auxiliary agent according to any one of claims 1 to 2.
4. The polypropylene composite material prepared by the high flame retardant flame retardant composite auxiliary agent according to claim 3, characterized in that: The polypropylene composite material comprises the following components, calculated by weight: 80-100 parts of polypropylene, 15-30 parts of highly flame-retardant flame-retardant composite auxiliary agent, 12-25 parts of flame retardant, 1-2 parts of itaconic acid, 0.2-0.6 parts of nano-alumina particles, 6-8 parts of epoxy soybean oil, and 20-25 parts of ethylene acrylic acid copolymer; wherein the mass ratio of highly flame-retardant flame-retardant composite auxiliary agent to flame retardant is (5-6): (4-5); The preparation method of the polypropylene composite material comprises the following steps: Preheat the mixer to 160-190°C, add 1 / 2 polypropylene, high flame retardant flame retardant composite additive, itaconic acid, nano alumina particles, stir and mix for 6-8 minutes, add flame retardant, epoxy soybean oil, ethylene acrylic acid copolymer, remaining 1 / 2 polypropylene, stir and mix for 10-15 minutes, heat to 190-210°C, extrude and granulate to obtain a polypropylene composite material.
5. The polypropylene composite material prepared by the high flame retardant flame retardant composite auxiliary agent according to claim 4, characterized in that: The method for preparing the flame retardant comprises the following steps: Heat DOPO to 130-135°C, add triglycidyl isocyanurate after it is completely melted, stir evenly, add N,N-dimethylacetamide, heat to 160-165°C, react for 3-3.5h, distill under reduced pressure, wash, and vacuum dry to obtain a flame retardant.
6. The polypropylene composite material prepared by the high flame retardant flame retardant composite auxiliary agent according to claim 5, characterized in that: In the flame retardant, the molar ratio of DOPO to triglycidyl isocyanurate is 1:(1-3).
Citation Information
Patent Citations
Hydrotalcite flame-resistant polypropylene material for woven bags
CN110591225A
Environment-friendly composite flame retardant as well as preparation method and application thereof
CN117247599A
Microparticulate hydrotalcite, method for producing same, resin composition of same, and suspension of same
WO2018169019A1