Gold-silver alloy structure for semiconductor devices and preparation method thereof
By forming a porous gold layer on the surface of the bumps of gold and silver alloy and removing silver by reverse electroplating, the problem of oxidation or vulcanization of gold and silver alloy in semiconductor devices is solved, and the effect of gold and silver alloys is realized instead of pure gold is simplified, and the process is simplified. Reduced costs.
Patent Information
- Application Number
- CN202410852249.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Gold and silver alloys are prone to oxidation or vulcanization in semiconductor devices, resulting in poor bonding, the prior art is complex and increases costs, and a simple and effective solution is urgently needed to replace pure gold.
By forming a porous gold layer on the surface of the gold-silver alloy bump, silver is removed by reverse plating, forming a stacked or surrounded structure to avoid silver oxidation or vulcanization. The process is simple and can be achieved by using the same electroplating equipment to change the current direction.
It effectively avoids silver oxidation or vulcanization problems, ensures the reliability of bonding, reduces costs, and does not require new equipment, the process is easy to achieve, and the hardness is consistent with pure gold.
Smart Images

Figure CN118398588B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of semiconductor device preparation, and in particular relates to a gold-silver alloy structure for semiconductor devices and a preparation method thereof. Background Art
[0002] Due to the continuous rise in gold prices, the manufacturing cost of semiconductor devices that use a large amount of gold, such as liquid crystal driver chips, memory chips or compound semiconductor chips, faces great pressure. Using gold-silver alloys instead of pure gold for the bumps of packaged chips can greatly save costs, but when the gold content in the gold-silver bumps is low, the surface of the gold-silver alloy is not resistant to oxidation or sulfurization. In the subsequent flip-chip process, the gold-silver bumps need to be bonded to the copper circuit of the flexible circuit board (FPC) through tin or gold microparticles in anisotropic conductive adhesive (ACF), and poor bonding occurs due to oxidation or sulfurization of silver. Therefore, the use of gold-silver alloys to replace pure gold urgently needs to solve the problem of insufficient oxidation or sulfurization resistance of silver in gold-silver alloys. In particular, the top surface of the bump, which is the location of the bonding interface, needs to avoid silver oxidation or sulfurization.
[0003] In order to solve the cost increase problem faced by semiconductor devices due to the continuous rise in gold prices, the existing technology adopts a variety of technical solutions to achieve cost reduction by replacing pure gold with gold-silver alloy. TWI469288B mentions electroplated gold-silver bumps. In order to prevent the problem of silver oxidation, the top or side of the gold-silver bump is electroplated or chemically plated with one of gold, palladium, copper or nickel to prevent silver oxidation, but copper or nickel is more easily oxidized than silver. TW201044527A mentions that the electroplated gold-silver bump contains no less than 80% silver content, and then a protective layer is formed on the gold and silver surface by replacing gold or reducing gold to prevent silver oxidation. TW201019440A mentions that the material of the silver bump can be selected from pure silver or silver alloy, and the silver alloy system of these silver bumps can contain no less than 80% silver content, and then a layer of pure gold or gold alloy is plated on the surface of the silver alloy to solve the problem of anti-oxidation. In the above operation, since the protective layer uses a component different from the gold-silver alloy electroplating, in actual operation, it is necessary to add another plating tank containing different chemicals to prepare the protective layer, which undoubtedly increases the complexity of the process and the investment cost of the production line.
[0004] In order to solve the above process complexity problem, CN117542818B has found through extensive research that by increasing the gold content in the gold-silver bump to more than 60%, the anti-oxidation or anti-sulfurization performance of the silver in the gold-silver bump can be significantly improved. Specifically, in the same electroplating tank, using the same gold-silver alloy plating solution, a gold-silver alloy body with a gold content of 20% to 50% is prepared by low current density electroplating as a connecting layer, and the plating height is 7 to 20 μm, and then a protective layer with a gold content of more than 60% is prepared by electroplating at a high current density, and the height of the protective layer is 10 to 500 nm. Since the above gold-silver bump structure can be prepared by using the same electroplating solution in the same plating tank only by the current density, the implementation of the process is greatly simplified and the equipment investment is reduced.
[0005] US5773897A invented a flip chip structure, including a monolithic microwave integrated circuit, formed on a module substrate and mounted on a component substrate, the module substrate also includes a plurality of solder bumps for fixing the module substrate to the component substrate, the solder bumps include a silver-plated column with a first diameter and covered with a plated solder (tin-lead solder) with a second diameter, wherein the second diameter is larger than the first diameter (approximately 25-50 μm), wherein the solder is also used to prevent oxidation of silver. However, if the solder diameter is large, adjacent bumps are prone to short circuit during the hot pressing process.
[0006] Through the above analysis of the prior art, it can be seen that in order to solve the technical problem that silver in the gold-silver alloy is easily oxidized or sulfided, the prior art adopts three solutions: First, a layer of gold or alloy is electroplated on the surface of gold and silver as a protective layer. In addition to the gold-silver alloy electroplating tank, a new pure gold electroplating tank or chemical plating needs to be added, which increases the complexity of the process and equipment investment. Second, CN117542818B uses the same electroplating solution to prepare gold-silver bumps with different gold contents by controlling the current density. The top surface of the bump contains a gold-silver alloy with a gold content of more than 60%, but the silver may also oxidize after the gold-silver alloy is placed for a long time. Third, solder is used to protect the top surface of the gold-silver bump, but because the solder is easy to flow at high temperature, it is not suitable for preparing fine lines. At present, the spacing between the bumps of some advanced liquid crystal driver chips has been reduced to less than 10μm, and the solder protection technical solution is not applicable; secondly, considering that silver and tin form alloys or intermetallic compounds, flakes may be formed to cause short circuits between bumps.
[0007] There is an urgent need for a gold-silver alloy structure for semiconductor devices and a preparation method thereof to solve the technical problem that silver in the gold-silver alloy bump is easily oxidized or sulfided, and to use the gold-silver alloy instead of pure gold for semiconductor devices, while the process is simple and easy to implement. Summary of the invention
[0008] The purpose of the present invention is to provide a gold-silver alloy structure for semiconductor devices and a preparation method thereof. After intensive research, the inventor has invented a simple and practical process method according to the material properties of the gold-silver alloy. After preparing the gold-silver alloy bump by electroplating, the same electroplating solution or an etching solution (the main difference between the etching solution and the electroplating solution is that it does not contain gold salt and silver salt) is used for reverse electroplating to etch the silver on the surface of the gold-silver alloy bump, so as to form a porous gold layer on the surface of the gold-silver alloy bump, thereby solving the technical problem that the silver in the gold-silver alloy bump is easily oxidized or sulfided, and realizing the use of gold-silver alloy to replace pure gold for semiconductor devices.
[0009] The primary aspect of the present invention is to provide a gold-silver alloy structure for semiconductor devices, wherein the main body of the gold-silver alloy structure is a gold-silver alloy bump, and a porous gold layer is provided on the surface of the gold-silver alloy bump. By forming a porous gold layer on the surface of the gold-silver alloy bump, the porous gold layer and the gold-silver alloy bump form a laminated structure (the porous gold layer is located on the top surface of the gold-silver alloy bump) or a surrounding structure (the porous gold layer is located on the top surface and the side of the gold-silver alloy bump), and the porous gold layer does not contain silver, thereby avoiding the problem of silver being easily oxidized or sulfided. Since only porous gold is formed on the surface, the bump body is still a gold-silver alloy material, which, on the one hand, realizes the replacement of pure gold by gold-silver alloy, and on the other hand, does not change the overall hardness of the bump (the hardness is equivalent to that of the pure gold bump). During the bonding process, the porous gold on the top surface of the bump will deform and cover the material below, so even if the silver in the main body of the gold-silver alloy bump below the porous gold is oxidized or sulfided, it will not affect the bonding quality of the porous gold with tin or gold micron particles in ACF.
[0010] Furthermore, the gold-silver alloy bump is obtained by electroplating; the porous gold layer is obtained by reverse electroplating, after the silver is etched away from the surface of the gold-silver alloy bump. The reverse electroplating described in the present invention refers to electroplating with a current direction opposite to that of preparing the gold-silver alloy bump. The method of reverse electroplating and etching to remove silver provided by the present invention has a simple process and is easy to implement, which is specifically embodied in that: there is no need to replace the electroplating equipment, only the current direction of the electroplating needs to be changed; the same electroplating solution can be used for reverse electroplating, and the etching solution can also be used for reverse electroplating. The main difference between the etching solution and the electroplating solution is that the etching solution does not contain gold salt and silver salt, and the preparation process of the etching solution is similar to that of the electroplating solution.
[0011] It should be pointed out that although there are many methods for etching and removing silver, in addition to the reverse electroplating provided by the present invention, there is also a chemical etching method. For example, Lothar et al. (Proceedings-Electronic Components and Technology Conference, 2022, 873-882) reported the use of nitric acid to etch silver in a gold-silver alloy to form a porous gold structure. However, the chemical etching method has the following defects and is not suitable for gold-silver alloy bumps of semiconductors, because semiconductor devices contain many materials, such as TiW adhesion layer, aluminum electrode, silicon substrate, silicon dioxide or silicon nitride passivation layer, and nitric acid can easily corrode these materials. The present invention, by reverse electroplating etching, only forms a very thin porous gold layer on the surface of the gold-silver bump, which not only meets the hardness requirements of the gold-silver bump package, but also ensures the reliability of subsequent bonding through the porous gold layer; at the same time, the reverse electroplating method is used, which is the same as the method for preparing the gold-silver alloy bump body, except that the current direction is opposite, and it will not cause damage to other materials on the semiconductor device.
[0012] Furthermore, the height of the gold-silver alloy bump is 7-20 μm, and the thickness of the porous gold layer is 0.02-2.0 μm. It should be pointed out that the thickness of the porous gold layer is the thickness of the porous gold layer on the top surface or side of the final semiconductor device product. In the process of preparing semiconductor device products, when etching the seed layer, especially when the seed layer is also gold, etching the seed layer will also etch the porous gold. In this way, when reverse electroplating is used to obtain porous gold, the thickness of the porous gold should be appropriately thicker to leave room for etching losses when etching the seed layer.
[0013] Another aspect of the present invention is to provide a method for preparing a gold-silver alloy structure for a semiconductor device, wherein the semiconductor device comprises a substrate, an electrode, a seed layer, an adhesion layer and a photoresist, and the preparation method comprises the following steps:
[0014] S1: preparing a gold-silver electroplating solution, placing a semiconductor device in the electroplating solution for electroplating, and obtaining a gold-silver alloy bump;
[0015] S2 using the same electroplating equipment, using the gold-silver electroplating solution of step S1 or using an etching solution, changing the direction of the current to perform reverse electroplating on the semiconductor device, removing the silver component in the alloy on the top surface of the bump, thereby forming a porous gold layer on the top surface of the bump;
[0016] S3 uses a stripping solution to remove the photoresist;
[0017] S4 removes the seed layer;
[0018] S5 removes the adhesion layer;
[0019] S6: annealing the gold-silver alloy bumps.
[0020] This preparation method finally obtains a gold-silver alloy bump with a laminated structure. First, the gold-silver alloy bump is electroplated without removing the photoresist. Then, the silver on the top surface of the bump is removed by reverse electroplating to form porous gold. Since the side wall is protected by the photoresist, the side wall does not change. Then, the photoresist, seed layer and adhesion layer are removed to form a gold-silver alloy main body-porous gold top surface laminated structure bump. By adjusting the annealing time and annealing temperature, the hardness of the gold-silver alloy bump can meet the packaging requirements.
[0021] Furthermore, the electroplating temperature of step S1 is 20-60°C, and the current density is 0.3-1.0 A / dm 2 (ASD), the electroplating time is 10~60min; the electroplating temperature of step S2 is 20~60℃, and the current density is 0.01~10 A / dm 2 , the electroplating time is 0.5~5min.
[0022] Another aspect of the present invention is to provide another method for preparing a gold-silver alloy structure for a semiconductor device, wherein the semiconductor device comprises a substrate, an electrode, a seed layer, an adhesion layer and a photoresist, and the preparation method comprises the following steps:
[0023] S1: preparing a gold-silver electroplating solution, placing a semiconductor device in the electroplating solution for electroplating, and obtaining a gold-silver alloy bump;
[0024] S2 uses a stripping solution to remove the photoresist;
[0025] S3: using the same electroplating equipment, using the gold-silver electroplating solution of step S1 or using the etching solution, changing the direction of the current to perform reverse electroplating on the semiconductor device, removing the silver component in the alloy on the top surface and side of the bump, thereby forming a porous gold layer on the top surface and side of the bump;
[0026] S4 removes the seed layer;
[0027] S5 removes the adhesion layer;
[0028] S6: annealing the gold-silver alloy bumps.
[0029] This preparation method finally obtains a gold-silver alloy bump with an encapsulating structure. First, the gold-silver alloy is electroplated, and after removing the photoresist, reverse electroplating is used to remove the silver on the top surface and side of the bump, thereby forming a porous gold layer on the top surface and side of the bump, and then the seed layer and adhesion layer are removed to form a gold-silver alloy body-porous gold top surface and side surrounding structure bump. By adjusting the annealing time and annealing temperature, the hardness of the gold-silver alloy bump can meet the packaging requirements.
[0030] Furthermore, the electroplating temperature of step S1 is 20-60°C, and the current density is 0.3-1.0 A / dm 2, the electroplating time is 10~60min; the electroplating temperature of step S3 is 20~60℃, and the current density is 0.01~10 A / dm 2 , the electroplating time is 0.5~5min.
[0031] Furthermore, the components of the gold-silver electroplating solution in the above two preparation methods include potassium aurous cyanide (molecular formula KAu(CN)2) 8-15 g / L, potassium silver cyanide (molecular formula KAg(CN)2) 2-6 g / L, hydantoin or its derivatives 1-100 g / L, and a buffer 10-100 g / L. The pH of the gold-silver electroplating solution is 8-11, and the hydantoin derivatives include 5,5-dimethylhydantoin, 5-methylhydantoin, 3,5,5-trimethylhydantoin, 3-methyl-5-ethylhydantoin, 3-methyl-5,5-diethylhydantoin, 3,5 ,5-triethylhydantoin, 3,5-diethylhydantoin, 5-propylhydantoin, 5-isopropylhydantoin, 1-(hydroxymethyl)-5,5-dimethylhydantoin, the buffer is selected from one or more of boric acid, sodium tetraborate, phosphate, pyrophosphate, hydroxyethylidene diphosphonic acid, aminotrimethylene phosphoric acid, tartrate, citrate, ethylenediaminetetraacetate, N-hydroxyethylethylenediaminetriacetate, nitrilotriacetate or iminodiacetate.
[0032] Furthermore, the components of the etching solution in the above two preparation methods include 1-100 g / L of hydantoin or its derivatives and 10-100 g / L of a buffer, the pH of the etching solution is 8-11, and the hydantoin derivatives include 5,5-dimethylhydantoin, 5-methylhydantoin, 3,5,5-trimethylhydantoin, 3-methyl-5-ethylhydantoin, 3-methyl-5,5-diethylhydantoin, 3,5 ,5-triethylhydantoin, 3,5-diethylhydantoin, 5-propylhydantoin, 5-isopropylhydantoin, 1-(hydroxymethyl)-5,5-dimethylhydantoin, the buffer is selected from one or more of boric acid, sodium tetraborate, phosphate, pyrophosphate, hydroxyethylidene diphosphonic acid, aminotrimethylene phosphoric acid, tartrate, citrate, ethylenediaminetetraacetate, N-hydroxyethylethylenediaminetriacetate, nitrilotriacetate or iminodiacetate.
[0033] The content of hydantoin and its derivatives is 1-100 g / L. If it is lower than 1 g / L, the plating solution or etching solution needs to be replaced frequently. If it is higher than 100 g / L, the solution viscosity is too high and may affect the uniformity of plating or etching. The content of the buffer is 10~100 g / L. The buffer not only keeps the pH value stable, but also acts as a conductive salt. The pH of the plating solution or etching solution is 8~11. This is because the pKa of 5,5-dimethylhydantoin is 8.1. Therefore, 5,5-dimethylhydantoin can form ionic complex electrolytic silver ions above pH 8. Too high a pH may cause swelling of the photoresist or plating.
[0034] Another aspect of the present invention is to provide a gold-silver alloy structure obtained according to the above preparation method.
[0035] The present invention has the following beneficial technical effects: the present invention solves the problem that the surface of the gold-silver alloy bump is easily oxidized or sulfurized, thereby ensuring the electrical interconnection reliability of the flip chip; the method provided by the present invention does not require the addition of new electroplating equipment or chemical plating equipment, and the process is simple and easy to implement. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The invention discloses a method and process for preparing a gold-silver alloy bump with a laminated structure.
[0037] Figure 2 The invention discloses a preparation method and process of a gold-silver alloy bump having an enveloping structure.
[0038] Figure 3a and Figure 3b is a SEM photo of the top surface of the gold-silver alloy bump obtained in Example 1, Figure 3c This is a SEM photograph of the cross section of the gold-silver alloy bump obtained in Example 1.
[0039] Figure 4a and Figure 4b is a SEM photo of the top surface of the gold-silver alloy bump obtained in Example 2, Figure 4c This is a SEM photograph of the cross section of the gold-silver alloy bump obtained in Example 2.
[0040] Figure 5 These are electrochemical curves of the etching solution of Example 2 etching a gold electrode or a silver electrode respectively.
[0041] Figure numerals: 101 - substrate, 102 - electrode, 103 - passivation layer, 104 - adhesion layer, 105 - seed layer, 106 - photoresist, 107 - gold-silver alloy bump, 108 - porous gold layer. DETAILED DESCRIPTION
[0042] The technical solution of the present invention is described clearly and completely below in conjunction with the accompanying drawings of the specification. Obviously, the described implementation is only a part of the implementation of the present invention, not all of the implementations. Based on the implementation of the present invention, all other implementations obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0043] This embodiment provides a gold-silver alloy bump with a laminated structure and a preparation method thereof. The preparation method flow is as follows: Figure 1 As shown, the specific steps are as follows.
[0044] S1. Prepare a gold-silver electroplating solution, place a semiconductor device in the electroplating solution for electroplating, the semiconductor device includes a substrate 101, an electrode 102, a passivation layer 103, an adhesion layer 104, a seed layer 105 and a photoresist 106, and obtain a gold-silver alloy bump 107. The electroplating solution contains 12 g / L of potassium gold cyanide, 4 g / L of potassium silver cyanide, 60 g / L of potassium pyrophosphate, 20 g / L of hydantoin, and the pH is 9. The electroplating temperature is 45°C, the current density is 0.8 ASD, and the electroplating time is 20 min. The height of the gold-silver alloy bump 107 is 10 μm, the gold content is 40 wt%, and the roughness Ra is 71 nm.
[0045] S2 Using the same electroplating equipment, using the gold-silver electroplating solution of step S1, changing the current direction for electroplating, a porous gold layer 108 is formed on the top surface of the gold-silver alloy bump 107. The electroplating temperature is 30° C., the current density is 0.2 ASD, and the electroplating time is 1 min.
[0046] S3 uses NMP (N-methylpyrrolidone) as a photoresist removal solution to remove the photoresist 106 .
[0047] S4: The copper seed layer 105 is removed by using H2O2 having a mass concentration of 30%.
[0048] S5: The TiW adhesion layer 104 is removed using H2O2 having a mass concentration of 30%.
[0049] S6: Annealing treatment is performed on the gold-silver alloy bump 107.
[0050] The morphology of the porous gold layer was observed using a scanning electron microscope. Figure 3a and 3b The SEM photos of the top surface of the gold and silver bumps magnified 1,000 times and 10,000 times respectively. Figure 3c This is a slice photo of the gold-silver bump. It can be clearly seen that a nanoporous structure (porous gold layer) has been formed on the surface of the bump. This is the result of the removal of surface silver. The thickness of the porous gold layer is about 1.45μm. Example 2
[0051] This embodiment provides a gold-silver alloy bump of an enclosing structure and a preparation method thereof. The preparation method flow is as follows: Figure 2 As shown, the specific steps are as follows.
[0052] S1. Prepare a gold-silver electroplating solution, place a semiconductor device in the electroplating solution for electroplating, the semiconductor device includes a substrate 101, an electrode 102, a passivation layer 103, an adhesion layer 104, a seed layer 105 and a photoresist 106, and obtain a gold-silver alloy bump 107. The electroplating solution contains 12 g / L of potassium gold cyanide, 4 g / L of potassium silver cyanide, 60 g / L of potassium pyrophosphate, 40 g / L of 5,5-dimethylhydantoin, and the pH is 9. The electroplating temperature is 45°C, the current density is 0.4 ASD, and the electroplating time is 45 min. The height of the gold-silver alloy bump 107 is 10 μm, the gold content is 25 wt%, and the roughness Ra is 61 nm.
[0053] S2: The photoresist 106 is removed using NMP as a degumming solution.
[0054] S3 uses an etching solution to perform reverse electroplating on the semiconductor device to remove the silver component in the top surface and side alloy of the gold-silver alloy bump 107, thereby forming a porous gold layer 108 on the top surface and side of the gold-silver alloy bump 107. The etching solution contains 60 g / L 5,5-dimethylhydantoin and 30 g / L potassium pyrophosphate, with a pH of 10. The electroplating temperature is 30°C, the current density is 0.2 ASD, and the electroplating time is 1 min.
[0055] S4: The gold seed layer 105 is removed using a thiourea-based etching solution.
[0056] S5: The TiW adhesion layer 104 is removed using H2O2 having a mass concentration of 30%.
[0057] S6: Annealing treatment is performed on the gold-silver alloy bump 107.
[0058] The morphology of the porous gold layer was observed using a scanning electron microscope. Figure 4a and 4b The SEM photos of the top surface of the gold and silver bumps magnified 1,000 times and 10,000 times respectively. Figure 4cThis is a slice photo of the gold-silver bump. It can be clearly seen that a nanoporous structure (porous gold layer) is formed on the surface of the bump. This is the result of the removal of silver. The thickness of the porous gold layer is about 1.62 μm. Compared with Example 1, since the gold content of the gold-silver alloy in Example 1 is 40wt%, while the gold content in Example 2 is only 25wt%, the nanoporous structure formed in Example 2 is more obvious. In addition, it should be noted that the pore structure etched on the sidewall in Example 2 is not very obvious. This may be because the surface is closer to the cathode than the sidewall, resulting in a stronger electric field on the surface than on the sidewall. The etching of the sidewall can be made more obvious by changing the distribution of the electric field or strengthening the flow of the etching solution.
[0059] Figure 5 By comparing the etching effects of the etching solution on the gold electrode and the silver electrode, it can be seen that the gold electrode has almost no dissolution, the silver electrode starts to dissolve from 0.15 V, and the current density increases with the increase of voltage. This means that the silver on the surface of the gold-silver alloy can be selectively etched by controlling the current density or voltage, thereby forming a porous gold structure.
[0060] Although the embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and cannot be understood as limiting the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and purpose of the present invention. The protection scope of the present invention is defined by the claims and their equivalent technical solutions.
Claims
1. A gold-silver alloy structure for a semiconductor device, wherein the main body of the gold-silver alloy structure is a gold-silver alloy bump, and a porous gold layer is provided on the surface of the gold-silver alloy bump; the porous gold layer is located on the top surface of the gold-silver alloy bump, or the porous gold layer is located on the top surface and side of the gold-silver alloy bump; the height of the gold-silver alloy bump is 7-20 μm, and the thickness of the porous gold layer is 0.02-2.0 μm.
2. The gold-silver alloy structure according to claim 1, characterized in that: The gold-silver alloy bump is obtained by electroplating; the porous gold layer is obtained by reverse electroplating, after etching away silver on the surface of the gold-silver alloy bump.
3. A method for preparing a gold-silver alloy structure for a semiconductor device, wherein the semiconductor device comprises a substrate, an electrode, a seed layer, an adhesion layer and a photoresist, characterized in that: The preparation method comprises the following steps: S1: preparing a gold-silver electroplating solution, placing a semiconductor device in the electroplating solution for electroplating, and obtaining a gold-silver alloy bump, wherein the height of the gold-silver alloy bump is 7-20 μm; S2: using the same electroplating equipment, using the gold-silver electroplating solution of step S1 or using the etching solution, changing the current direction to perform reverse electroplating on the semiconductor device, removing the silver component in the alloy on the top surface of the bump, thereby forming a porous gold layer on the top surface of the bump, wherein the thickness of the porous gold layer is 0.02-2.0 μm; S3 uses a stripping solution to remove the photoresist; S4 removes the seed layer; S5 removes the adhesion layer; S6: annealing the gold-silver alloy bumps.
4. The preparation method according to claim 3, characterized in that The electroplating temperature of step S1 is 20~60℃, and the current density is 0.3~1.0 A / dm 2 , the electroplating time is 10~60min; the electroplating temperature of step S2 is 20~60℃, and the current density is 0.01~10 A / dm 2 , the electroplating time is 0.5~5min.
5. A method for preparing a gold-silver alloy structure for a semiconductor device, wherein the semiconductor device comprises a substrate, a seed layer, an adhesion layer and a photoresist, characterized in that: The preparation method comprises the following steps: S1: preparing a gold-silver electroplating solution, placing a semiconductor device in the electroplating solution for electroplating, and obtaining a gold-silver alloy bump, wherein the height of the gold-silver alloy bump is 7-20 μm; S2 uses a stripping solution to remove the photoresist; S3: using the same electroplating equipment, using the gold-silver electroplating solution of step S1 or using the etching solution, changing the current direction to perform reverse electroplating on the semiconductor device, removing the silver component in the alloy on the top surface and side of the bump, thereby forming a porous gold layer on the top surface and side of the bump, wherein the thickness of the porous gold layer is 0.02-2.0 μm; S4 removes the seed layer; S5 removes the adhesion layer; S6: annealing the gold-silver alloy bumps.
6. The preparation method according to claim 5, characterized in that The electroplating temperature of step S1 is 20~60℃, and the current density is 0.3~1.0 A / dm 2 , the electroplating time is 10~60min; the electroplating temperature of step S3 is 20~60℃, and the current density is 0.01~10 A / dm 2 , the electroplating time is 0.5~5min.
7. The preparation method according to claim 3 or 5, characterized in that: The components of the gold-silver electroplating solution include 8-15 g / L potassium aurite cyanide, 2-6 g / L potassium silver cyanide, 1-100 g / L hydantoin or its derivatives, and 10-100 g / L buffer. The pH of the gold-silver electroplating solution is 8-11. The hydantoin derivatives include 5,5-dimethylhydantoin, 5-methylhydantoin, 3,5,5-trimethylhydantoin, 3-methyl-5-ethylhydantoin, 3-methyl-5,5-diethylhydantoin, 3,5 ,5-triethylhydantoin, 3,5-diethylhydantoin, 5-propylhydantoin, 5-isopropylhydantoin, 1-(hydroxymethyl)-5,5-dimethylhydantoin, the buffer is selected from one or more of boric acid, sodium tetraborate, phosphate, pyrophosphate, hydroxyethylidene diphosphonic acid, aminotrimethylene phosphoric acid, tartrate, citrate, ethylenediaminetetraacetate, N-hydroxyethylethylenediaminetriacetate, nitrilotriacetate or iminodiacetate.
8. The preparation method according to claim 3 or 5, characterized in that The components of the etching solution include 1-100 g / L of hydantoin or its derivatives and 10-100 g / L of a buffer. The pH of the etching solution is 8-11. The hydantoin derivatives include 5,5-dimethylhydantoin, 5-methylhydantoin, 3,5,5-trimethylhydantoin, 3-methyl-5-ethylhydantoin, 3-methyl-5,5-diethylhydantoin, 3,5,5-triethylhydantoin, 3,5-diethylhydantoin, 5-propylhydantoin, 5-isopropylhydantoin, and 1-(hydroxymethyl)-5,5-dimethylhydantoin. The buffer is selected from one or more of boric acid, sodium tetraborate, phosphate, pyrophosphate, hydroxyethylidene diphosphonic acid, aminotrimethylene phosphoric acid, tartrate, citrate, ethylenediaminetetraacetate, N-hydroxyethylethylenediaminetriacetate, nitrilotriacetate, or iminodiacetate.
9. The gold-silver alloy structure obtained according to the preparation method according to any one of claims 3 to 8.
Citation Information
Patent Citations
A gold-silver alloy bump and its preparation method and application
CN117542818B
Bumped chip and semiconductor flip-chip device applied from the same
TW201019440A
Chip architecture having film-faced metal bumps and semiconductor flip-chip device applied from the same
TW201044527A
Flip chip monolithic microwave integrated circuit with mushroom-shaped, solder-capped, plated metal bumps
US5773897A
Gold-silver alloy bump as well as preparation method and application thereof
CN117542818A
Cited By
Semiconductor device structure, preparation method thereof and corresponding chip
CN119340299A
A semiconductor device structure, a method of fabricating the same, and a corresponding chip
CN119340299B
Semiconductor device structure, preparation method thereof and chip
CN119852281A
A semiconductor device structure and its manufacturing method and chip
CN119852281B
Etching method for removing anisotropic conductive adhesive in gold-silver alloy bump manufacturing process
CN121285266A