A high-strength polyethylene water supply pipe and preparation method thereof
By real-time monitoring and adjustment of bubble parameters during the extrusion process, dynamically adjusting the preparation process of polyethylene water supply pipe, the problem of poor mixing uniformity is solved, the physical performance and production efficiency of the pipe are improved, and high strength and high straightness are achieved. Preparation of polyethylene water feed pipes.
Patent Information
- Application Number
- CN202411083510.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-08
AI Technical Summary
In the existing preparation methods of polyethylene water feed pipes, the mixing method is too simple, resulting in poor controllability of the mixing degree, affecting the straightness and quality stability of the pipe.
By monitoring the bubble diameter and number of melt to be extruded in real time, dynamically adjusting the extrusion speed and melting temperature, combined with the use of exhaust fans, ensure that the number and size of bubbles of the pipe are strictly controlled, and the mixing uniformity and physical performance are improved.
It improves the physical properties and appearance quality of the pipe, optimizes the production process, reduces material waste, ensures high standards of geometric accuracy and usage performance, and produces high strength, high uniformity and high straightness polyethylene water supply pipes.
Smart Images

Figure CN118617706B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer pipe preparation, and in particular to a high-strength polyethylene water supply pipe and a preparation method thereof. Background Art
[0002] With the rapid development of the global construction industry and infrastructure construction, the demand for efficient, environmentally friendly and durable water supply pipe systems is growing. Polyethylene (PE) water supply pipes have been widely used in modern water supply projects due to their excellent corrosion resistance, heat resistance, pressure resistance, good wear resistance and toughness. The lightweight, easy processing and recyclable characteristics of polyethylene materials, coupled with their advantages in ensuring water quality safety and reducing long-term operating costs, make PE water supply pipes an ideal substitute for traditional metal pipes and cement pipes. However, although PE water supply pipes have shown excellent performance in many aspects, their preparation methods and material formulations are still under continuous research and development to further improve their performance.
[0003] Patent document with publication number CN108485026A discloses a polyethylene water supply pipe material and a preparation method thereof, wherein the polyethylene water supply pipe material is prepared by adding different components into a high-speed mixer for mixing. The preparation step of the composite filler in the production process is inefficient, which affects the overall production efficiency. In addition, the mixing method is too simple, resulting in poor controllability of the mixing uniformity, which affects the stability of the straightness quality of the pipe. Summary of the invention
[0004] To this end, the present invention provides a method for preparing a high-strength polyethylene water supply pipe, so as to overcome the problem in the prior art that the mixing method is too simple, resulting in poor controllability of the mixing uniformity and causing low stability of the straightness quality of the pipe.
[0005] To achieve the above object, the present invention provides a method for preparing a high-strength polyethylene water supply pipe, comprising:
[0006] Melting the raw material for preparing the water supply pipe at a preset melting temperature to obtain a melt to be extruded;
[0007] Extruding the melt to be extruded at a preset extrusion speed, and monitoring the real-time bubble diameter and the real-time bubble number of the melt to be extruded at a monitoring point during the extrusion process;
[0008] Adjust the extrusion speed according to the real-time bubble quantity and the preset standard quantity;
[0009] Calculate the diameter standard deviation of the real-time bubble diameter according to the monitoring result after adjusting the extrusion speed, make a judgment according to the real-time bubble diameter, the diameter standard deviation, a preset diameter standard deviation threshold and a preset standard diameter, and adjust the melting temperature according to the judgment result, or monitor the real-time wall thickness of the bubble;
[0010] Calculate the wall thickness standard deviation of the real-time wall thickness according to the real-time wall thickness and the real-time bubble number;
[0011] Make a judgment based on the real-time wall thickness, the preset standard wall thickness, the wall thickness standard deviation and the preset wall thickness standard deviation threshold, and adjust the melting temperature or turn on the exhaust fan according to the judgment result;
[0012] The real-time straightness of the given tube after extrusion and cooling is monitored, and the adjusted melt temperature is corrected according to the real-time straightness and the preset standard straightness.
[0013] Further, adjusting the extrusion speed according to the real-time number of bubbles and a preset standard number includes:
[0014] The extrusion speed is adjusted according to the difference between the real-time bubble quantity greater than the preset standard quantity and the standard quantity and the preset speed adjustment coefficient.
[0015] Further, the calculation of the diameter standard deviation of the real-time bubble diameter according to the monitoring result after adjusting the extrusion speed includes:
[0016] The average value of the real-time bubble diameter is calculated according to the real-time bubble diameter after adjusting the extrusion speed and the real-time bubble number, and the standard deviation of the real-time bubble diameter is calculated according to the calculation result to obtain the diameter standard deviation.
[0017] Further, adjusting the melting temperature according to the determination result includes:
[0018] When the diameter standard deviation is greater than the preset diameter standard deviation threshold and the average value of the real-time bubble diameter is greater than the standard diameter, the melting temperature is adjusted based on the difference between the average value of the real-time bubble diameter and the standard diameter and the preset diameter temperature adjustment coefficient.
[0019] Further, monitoring the real-time wall thickness of the bubble according to the determination result includes:
[0020] When the diameter standard deviation is less than or equal to a preset diameter standard deviation threshold, the real-time wall thickness of the bubble is monitored.
[0021] Further, the wall thickness standard deviation of the real-time wall thickness is calculated according to the real-time wall thickness and the real-time bubble quantity, comprising:
[0022] The average wall thickness is calculated according to the real-time wall thickness and the real-time bubble number, and the wall thickness standard deviation of the real-time wall thickness is calculated according to the average wall thickness.
[0023] Further, adjusting the melting temperature according to the determination result includes:
[0024] When the wall thickness standard deviation is greater than a preset wall thickness standard deviation threshold, the melting temperature is adjusted according to the wall thickness standard deviation, the wall thickness standard deviation threshold, and a preset wall thickness temperature adjustment coefficient.
[0025] Further, turning on the exhaust fan according to the determination result includes:
[0026] When the wall thickness standard deviation is less than or equal to the preset wall thickness standard deviation threshold, and the average wall thickness is less than the preset standard wall thickness, the exhaust fan in the extrusion zone is turned on.
[0027] Furthermore, the melt temperature adjusted according to the real-time straightness and the preset standard straightness correction includes:
[0028] The melt temperature after correction adjustment is reduced according to the real-time straightness that is less than the standard straightness, the standard straightness and a preset correction factor.
[0029] A high-strength polyethylene water supply pipe, the raw materials for preparing the water supply pipe include:
[0030] 80-87 parts of polyethylene, 1-2 parts of N-ethyl-o-p-toluenesulfonamide, 1-2 parts of potassium tetraborate, 2-4 parts of propylene glycol adipic acid polyester, 4-6 parts of polyvinylidene fluoride, 1-2 parts of ammonium dihydrogen phosphate, 0.7-1 parts of 6-di-tert-butyl-p-cresol, 0.7-1 parts of antioxidant, 1-2 parts of zirconium oxide, 2-3 parts of ethyl acetate, 0.5-1 parts of vanadium diboride, 0.5-1 parts of dimethyl sulfoxide, 4-5 parts of lapis lazuli powder and 6-9 parts of composite filler.
[0031] Compared with the prior art, the beneficial effect of the present invention lies in that, through real-time monitoring and adjustment, the number and size of bubbles in the pipe are strictly controlled, thereby improving the physical properties and appearance quality of the pipe. The intelligent temperature and speed adjustment mechanism optimizes the production process, reduces material waste, improves production efficiency, and accurately controls the flow and exhaust of the molten material, further improving the intrinsic quality and performance of the pipe. By monitoring the straightness and fine-tuning the melting temperature, the geometric accuracy of the pipe is ensured, and high quality requirements are met, which helps to produce high-strength, high-uniformity and high-straightness polyethylene water supply pipes, which are suitable for various water supply projects with strict requirements, and effectively solves the problem of low stability of the straightness quality of the pipe due to poor controllability of the mixing uniformity due to the overly simple mixing method.
[0032] Furthermore, by dynamically adjusting the extrusion speed according to the difference between the real-time number of bubbles and the preset standard number, the formation of bubbles in the production process of polyethylene water pipes is effectively controlled. This real-time feedback and adjustment mechanism not only improves production efficiency and reduces the waste of raw materials, but also significantly improves the overall quality and performance of the finished pipes, and can ensure that the produced polyethylene water pipes have fewer defects.
[0033] Furthermore, bubble control is optimized by dynamically adjusting the extrusion speed and melt temperature. Increasing the melt temperature helps improve the fluidity and uniformity of the melt and reduce the formation of large bubbles, thereby improving the physical properties and appearance quality of the pipe. At the same time, real-time monitoring of bubble wall thickness helps to promptly discover and solve problems that may affect the strength and durability of the pipe.
[0034] Furthermore, through real-time monitoring and adjustment, the uniformity of the tube wall is ensured, avoiding potential structural weaknesses caused by uneven wall thickness. Increasing the melt temperature helps to discharge bubbles and evenly mix the materials, while timely opening of the exhaust fan further improves the exhaust efficiency and reduces the generation of bubbles.
[0035] Furthermore, by monitoring the straightness in real time and dynamically adjusting the melt temperature according to the deviation, this method can ensure that the polyethylene water pipe has better geometric accuracy and consistency during the extrusion process. Reducing the melt temperature helps to reduce the fluidity of the material and avoid sagging or bending of the pipe due to overheating, thereby improving the straightness of the pipe. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a flow chart of the method for preparing the high-strength polyethylene water supply pipe of this embodiment;
[0037] Figure 2 It is a schematic diagram of the water pipe composite extrusion system assembly line of this embodiment;
[0038] Figure 3 The decision logic diagram for adjusting the extrusion speed in this embodiment;
[0039] Figure 4 This is a decision logic diagram for adjusting the melting temperature according to the diameter standard deviation in this embodiment. DETAILED DESCRIPTION
[0040] In order to make the objects and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with embodiments; it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0041] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.
[0042] It should be noted that, in the description of the present invention, terms such as "up", "down", "left", "right", "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is merely for the convenience of description and does not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present invention.
[0043] In addition, it should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0044] See also Figure 1 As shown, it is a flow chart of the method for preparing the high-strength polyethylene water supply pipe of this embodiment;
[0045] Please continue reading Figure 2 As shown, it is a schematic diagram of the water pipe composite extrusion system assembly line of this embodiment;
[0046] This embodiment provides a method for preparing a high-strength polyethylene water supply pipe, comprising:
[0047] Putting the raw materials for preparing the water supply pipe into the mixing zone of the water supply pipe composite extrusion system assembly line to melt them at a preset melting temperature to obtain a molten material to be extruded;
[0048] The molten material to be extruded is placed in the extrusion zone of the water supply pipe composite extrusion system assembly line and extruded at a preset extrusion speed, and an image sensor is used to monitor the real-time bubble diameter and the real-time bubble number of the molten material to be extruded at the monitoring point during the extrusion process;
[0049] Adjust the extrusion speed according to the real-time bubble quantity and the preset standard quantity;
[0050] Calculate the diameter standard deviation of the real-time bubble diameter according to the monitoring result after adjusting the extrusion speed, make a judgment according to the real-time bubble diameter, the diameter standard deviation, a preset diameter standard deviation threshold and a preset standard diameter, adjust the melting temperature according to the judgment result, or use an ultrasonic sensor to monitor the real-time wall thickness of the bubble;
[0051] Calculate the wall thickness standard deviation of the real-time wall thickness according to the real-time wall thickness and the real-time bubble number;
[0052] Make a judgment based on the real-time wall thickness, the preset standard wall thickness, the wall thickness standard deviation and the preset wall thickness standard deviation threshold, and adjust the melting temperature or turn on the exhaust fan according to the judgment result;
[0053] A straightness sensor is used to monitor the real-time straightness of the output tube after extrusion and cooling in the cooling zone, and the adjusted melt temperature is corrected based on the real-time straightness and the preset standard straightness.
[0054] First, the raw materials for preparing the water supply pipe are melted at a set melting temperature to form a melt to be extruded. During the extrusion process, the system monitors and records the diameter and number of bubbles in the melt in real time, compares these data with the preset standards, and dynamically adjusts the extrusion speed to reduce the number of bubbles. Furthermore, the consistency of the bubble size is judged by analyzing the standard deviation of the bubble diameter, and the melting temperature is adjusted accordingly to obtain a more uniform and consistent melt. At the same time, by monitoring the bubble wall thickness and calculating the standard deviation of the wall thickness, the melting temperature is further refined or the exhaust system is started to optimize the exhaust effect. Finally, by monitoring the straightness of the pipe and comparing it with the preset straightness standard, the melting temperature is fine-tuned to ensure that the pipe quality meets the standard requirements.
[0055] Through real-time monitoring and adjustment, strict control of the number and size of bubbles in the pipe during the production process is ensured, thereby improving the physical properties and appearance quality of the pipe. The intelligent temperature and speed adjustment mechanism optimizes the production process, reduces material waste, and improves production efficiency. It accurately controls the flow and exhaust of the molten material, further improving the intrinsic quality and performance of the pipe. By monitoring the straightness and fine-tuning the melting temperature, the geometric accuracy of the pipe is ensured, meeting high quality requirements, and helping to produce high-strength, high-uniformity and high-straightness polyethylene water supply pipes, which are suitable for various water supply projects with strict requirements.
[0056] Please continue reading Figure 3 As shown, it is a decision logic diagram for adjusting the extrusion speed in this embodiment;
[0057] Specifically, adjusting the extrusion speed according to the real-time bubble quantity and the preset standard quantity includes:
[0058] The extrusion speed is adjusted according to the difference between the real-time bubble quantity greater than the preset standard quantity and the standard quantity and the preset speed adjustment coefficient.
[0059] When the number of bubbles monitored in real time exceeds the preset standard number, the system will calculate the difference between the two and apply a preset speed adjustment coefficient to determine the adjustment range of the extrusion speed. Based on this calculation, the extrusion speed will be reduced accordingly to reduce the bubble formation rate. This process is achieved through an automated control system, ensuring the accuracy and timeliness of the adjustment process, thereby ensuring the consistency and reliability of product quality.
[0060] By dynamically adjusting the extrusion speed based on the difference between the real-time number of bubbles and the preset standard number, the formation of bubbles in the production process of polyethylene water pipes is effectively controlled. This real-time feedback and adjustment mechanism not only improves production efficiency and reduces the waste of raw materials, but also significantly improves the overall quality and performance of the finished pipes, ensuring that the produced polyethylene water pipes have fewer defects.
[0061] Specifically, the method of calculating the diameter standard deviation of the real-time bubble diameter according to the monitoring result after adjusting the extrusion speed includes:
[0062] The average value of the real-time bubble diameter is calculated according to the real-time bubble diameter after adjusting the extrusion speed and the real-time bubble number, and the standard deviation of the real-time bubble diameter is calculated according to the calculation result to obtain the diameter standard deviation.
[0063] Please continue reading Figure 4 As shown, it is a decision logic diagram for adjusting the melting temperature according to the diameter standard deviation in this embodiment;
[0064] Specifically, adjusting the melting temperature according to the determination result includes:
[0065] When the diameter standard deviation is greater than the preset diameter standard deviation threshold and the average value of the real-time bubble diameter is greater than the standard diameter, the melting temperature is adjusted based on the difference between the average value of the real-time bubble diameter and the standard diameter and the preset diameter temperature adjustment coefficient.
[0066] Specifically, the real-time wall thickness of the bubble is monitored according to the determination results, including:
[0067] When the diameter standard deviation is less than or equal to a preset diameter standard deviation threshold, the real-time wall thickness of the bubble is monitored.
[0068] First, the formation of bubbles is controlled by adjusting the extrusion speed. The adjustment of the extrusion speed is based on the difference between the number of bubbles monitored in real time and the preset standard number. After adjustment, the system monitors and calculates the average value of the bubble diameter and its standard deviation. If the diameter standard deviation exceeds the preset threshold and the bubble diameter average exceeds the standard diameter, the system will increase the melt temperature based on these deviations and the preset adjustment factor. This process ensures the uniformity of the melt, thereby reducing the inconsistency of bubbles. When the diameter standard deviation is within the acceptable range, the system will switch to monitoring the real-time wall thickness of the bubble to further ensure product quality.
[0069] Bubble control is optimized by dynamically adjusting the extrusion speed and melt temperature. Increasing the melt temperature helps improve the fluidity and uniformity of the melt and reduce the formation of large bubbles, thereby improving the physical properties and appearance quality of the pipe. At the same time, real-time monitoring of bubble wall thickness helps to promptly discover and solve problems that may affect the strength and durability of the pipe.
[0070] Specifically, the wall thickness standard deviation calculated according to the real-time wall thickness and the real-time bubble number includes:
[0071] The average wall thickness is calculated according to the real-time wall thickness and the real-time bubble number, and the wall thickness standard deviation of the real-time wall thickness is calculated according to the average wall thickness.
[0072] Specifically, adjusting the melting temperature according to the determination result includes:
[0073] When the wall thickness standard deviation is greater than a preset wall thickness standard deviation threshold, the melting temperature is adjusted according to the wall thickness standard deviation, the wall thickness standard deviation threshold, and a preset wall thickness temperature adjustment coefficient.
[0074] Specifically, turning on the exhaust fan according to the determination result includes:
[0075] When the wall thickness standard deviation is less than or equal to the preset wall thickness standard deviation threshold, and the average wall thickness is less than the preset standard wall thickness, the exhaust fan in the extrusion zone is turned on.
[0076] In the process of preparing high-strength polyethylene water supply pipes, the wall thickness and number of bubbles are monitored in real time, and the average wall thickness and the standard deviation of the wall thickness are calculated based on these data. If the standard deviation of the wall thickness exceeds the preset threshold, it indicates that the wall thickness is uneven. At this time, the system will increase the melting temperature accordingly based on the difference between the wall thickness standard deviation and the threshold and the wall thickness temperature adjustment coefficient to improve the melting and flow characteristics of the material. When the wall thickness standard deviation remains within the preset threshold, but the average wall thickness is lower than the standard requirement, the system will automatically turn on the exhaust fan to increase exhaust efficiency, reduce bubbles, and ensure wall thickness uniformity.
[0077] Through real-time monitoring and adjustment, the uniformity of the tube wall is ensured, avoiding potential structural weaknesses caused by uneven wall thickness. Increasing the melt temperature helps to discharge bubbles and evenly mix the materials, while timely opening of the exhaust fan further improves the exhaust efficiency and reduces the generation of bubbles.
[0078] Specifically, the melt temperature adjusted according to the real-time straightness and the preset standard straightness correction includes:
[0079] The melt temperature after correction adjustment is reduced according to the real-time straightness that is less than the standard straightness, the standard straightness and a preset correction factor.
[0080] In the process of producing high-strength polyethylene water supply pipes, the straightness of the pipe is monitored in real time and compared with the preset standard straightness. If the monitored straightness is lower than the standard straightness, the system will calculate the adjustment range of the melting temperature based on this deviation and a preset correction factor. Based on this calculation result, the system will automatically reduce the melting temperature in the hope of increasing the fluidity of the material and the stability after molding by lowering the temperature, thereby improving the straightness of the pipe.
[0081] By monitoring straightness in real time and dynamically adjusting the melt temperature based on deviations, this method can ensure better geometric accuracy and consistency of polyethylene water pipes during extrusion. Reducing the melt temperature helps reduce the fluidity of the material and avoid sagging or bending of the pipe due to overheating, thereby improving the straightness of the pipe.
[0082] Standard quantity:
[0083] Depending on the quality of the tube and the application requirements, it is usually set as the maximum allowable number of bubbles per unit length or unit volume.
[0084] Standard diameter:
[0085] Used to limit the maximum allowable size of a single bubble to ensure the uniformity and strength of the pipe.
[0086] Diameter standard deviation threshold:
[0087] Used to evaluate the consistency of bubble diameter, a smaller standard deviation means more uniform bubble size.
[0088] Wall thickness standard deviation threshold:
[0089] Used to evaluate the consistency of pipe wall thickness and ensure balanced mechanical properties of the pipe at different locations.
[0090] Standard wall thickness:
[0091] It is set according to the design pressure of the pipe and the application environment, which affects the pressure bearing capacity and service life of the pipe.
[0092] Standard straightness:
[0093] Used to limit the degree of bending or twisting of the pipe in the length direction, affecting installation and use.
[0094] Speed adjustment factor:
[0095] Depends on the degree of impact on production speed when the number of bubbles exceeds the standard number. Usually set based on historical data and production experience.
[0096] Diameter temperature adjustment factor:
[0097] Used to adjust the melt temperature based on the deviation of the bubble diameter standard deviation and wall thickness standard deviation from the preset threshold. This factor takes into account the effect of temperature changes on the material's melt state and fluidity.
[0098] Wall thickness temperature adjustment factor:
[0099] Used when the wall thickness standard deviation exceeds a preset threshold to determine the amount of adjustment to the melt temperature to improve the uniformity of the wall thickness.
[0100] Correction factor:
[0101] Used to correct the adjusted melt temperature according to straightness deviations to improve the geometric accuracy of the tube.
[0102] In this embodiment, the setting of these thresholds is based on the following considerations:
[0103] Industry Standard: Set according to industry standards or specifications for polyethylene pipe.
[0104] Application requirements: set according to the pipe use environment and engineering requirements.
[0105] Material properties: set according to the physical and chemical properties of polyethylene materials.
[0106] Historical data: set based on historical data and experience values collected during the production process.
[0107] The adjustment factor is set based on the following factors:
[0108] Experience and historical data: Based on previous production experience or historical data, determine the proportion of process parameters that need to be adjusted under specific parameter deviations.
[0109] Material properties: Understand the sensitivity of the material to changes in process parameters such as temperature and pressure to determine the appropriate adjustment factor.
[0110] Equipment characteristics: Consider the reaction characteristics of the production equipment to parameter adjustments, such as the response time and adjustment range of the extruder.
[0111] Quality control standards: Determine adjustment factors based on product quality requirements and allowable deviation range to ensure that products can quickly return to quality control standards.
[0112] Production efficiency and cost: Balance production efficiency and cost, and choose an adjustment factor that can quickly correct deviations without excessively consuming resources.
[0113] For example, in this embodiment:
[0114] The standard quantity is set at no more than 5 pcs / m.
[0115] The standard diameter is set at no more than 2 mm.
[0116] The diameter standard deviation threshold was set at 0.5 mm.
[0117] The wall thickness standard deviation threshold was set to 0.2 mm.
[0118] The standard wall thickness is set as the minimum wall thickness calculated based on the pipe diameter and design requirements.
[0119] Standard straightness is set at 0.1% of the tube length.
[0120] The adjustment coefficient set in this embodiment is:
[0121] Speed adjustment factor: 1.5 (meaning that for every bubble that exceeds the limit, the extrusion speed will be reduced by 1.5 times the amount of excess bubbles);
[0122] Diameter temperature adjustment coefficient: According to the difference between the standard deviation of bubble diameter and the preset threshold, a ratio is determined, such as 0.2 (indicating that for every 0.1 mm excess, the melting temperature increases by 0.2 times the difference);
[0123] Wall thickness temperature adjustment coefficient: It may be set to 0.1, which means that for every 0.1 mm wall thickness standard deviation, the melting temperature will increase by 0.1 times the difference;
[0124] Correction factor: 0.5 (indicates that if the real-time straightness is 1% lower than the standard straightness, the melting temperature will decrease by 0.5°C).
[0125] The advantages of the preset value setting in this embodiment include:
[0126] Improve product quality: Improve the overall performance of the pipe by strictly controlling the consistency of bubbles and wall thickness.
[0127] Ensure safe use: meet the pressure and temperature requirements of engineering design and ensure long-term stable operation.
[0128] Optimize production process: reduce scrap rate and improve production efficiency through real-time monitoring and adjustment.
[0129] Strong adaptability: Flexibly adjust threshold settings according to different application environments and engineering requirements.
[0130] The advantages of the adjustment coefficient set in this embodiment include:
[0131] Flexibility: Dimensionless coefficients provide flexibility to adjust process parameters in proportion to actual deviations.
[0132] Simplicity: The adjustment calculation is simplified, and adjustments can be made quickly based on monitoring results without complicated conversions.
[0133] Adaptability: It can adapt to different production conditions and material batches to maintain production stability and consistency of product quality.
[0134] A high-strength polyethylene water supply pipe, the raw materials for preparing the water supply pipe include:
[0135] 80-87 parts of polyethylene, 1-2 parts of N-ethyl-o-p-toluenesulfonamide, 1-2 parts of potassium tetraborate, 2-4 parts of propylene glycol adipic acid polyester, 4-6 parts of polyvinylidene fluoride, 1-2 parts of ammonium dihydrogen phosphate, 0.7-1 parts of 6-di-tert-butyl-p-cresol, 0.7-1 parts of antioxidant, 1-2 parts of zirconium oxide, 2-3 parts of ethyl acetate, 0.5-1 parts of vanadium diboride, 0.5-1 parts of dimethyl sulfoxide, 4-5 parts of lapis lazuli powder and 6-9 parts of composite filler.
[0136] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.
[0137] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a high-strength polyethylene water supply pipe, characterized in that: include: Melting the raw material for preparing the water supply pipe at a preset melting temperature to obtain a melt to be extruded; Extruding the melt to be extruded at a preset extrusion speed, and monitoring the real-time bubble diameter and the real-time bubble number of the melt to be extruded at a monitoring point during the extrusion process; Adjust the extrusion speed according to the real-time bubble quantity and the preset standard quantity; Calculating the diameter standard deviation of the real-time bubble diameter according to the monitoring result after adjusting the extrusion speed, making a judgment according to the real-time bubble diameter, the diameter standard deviation, a preset diameter standard deviation threshold and a preset standard diameter, adjusting the melting temperature according to the first judgment result, and monitoring the real-time wall thickness of the bubble according to the second judgment result; Calculate the wall thickness standard deviation of the real-time wall thickness according to the real-time wall thickness and the real-time bubble number; Making a judgment based on the real-time wall thickness, the preset standard wall thickness, the wall thickness standard deviation, and the preset wall thickness standard deviation threshold, adjusting the melting temperature based on the third judgment result, and turning on the exhaust fan based on the fourth judgment result; Monitor the real-time straightness of the extruded and cooled tube, and correct the adjusted melt temperature according to the real-time straightness and the preset standard straightness; The adjusting of the extrusion speed according to the real-time bubble quantity and the preset standard quantity comprises: The extrusion speed is adjusted by reducing the difference between the real-time bubble quantity greater than the preset standard quantity and the standard quantity and the preset speed adjustment coefficient; Adjusting the melting temperature according to the first determination result includes: When the diameter standard deviation is greater than a preset diameter standard deviation threshold and the average value of the real-time bubble diameter is greater than the standard diameter, the melting temperature is increased and adjusted according to the difference between the average value of the real-time bubble diameter and the standard diameter and the preset diameter temperature adjustment coefficient; Monitoring the real-time wall thickness of the bubble according to the second determination result includes: When the diameter standard deviation is less than or equal to a preset diameter standard deviation threshold, the real-time wall thickness of the bubble is monitored; Adjusting the melting temperature according to the third determination result includes: When the wall thickness standard deviation is greater than a preset wall thickness standard deviation threshold, the melting temperature is increased and adjusted according to the wall thickness standard deviation, the wall thickness standard deviation threshold, and a preset wall thickness temperature adjustment coefficient; Turning on the exhaust fan according to the fourth determination result includes: When the wall thickness standard deviation is less than or equal to the preset wall thickness standard deviation threshold, and the average wall thickness is less than the preset standard wall thickness, the exhaust fan in the extrusion zone is turned on.
2. The method for preparing a high-strength polyethylene water supply pipe according to claim 1, characterized in that: The method of calculating the diameter standard deviation of the real-time bubble diameter according to the monitoring result after adjusting the extrusion speed includes: The average value of the real-time bubble diameter is calculated according to the real-time bubble diameter after adjusting the extrusion speed and the real-time bubble number, and the standard deviation of the real-time bubble diameter is calculated according to the calculation result to obtain the diameter standard deviation.
3. The method for preparing a high-strength polyethylene water supply pipe according to claim 2, characterized in that: The wall thickness standard deviation calculated according to the real-time wall thickness and the real-time bubble quantity includes: The average wall thickness is calculated according to the real-time wall thickness and the real-time bubble number, and the wall thickness standard deviation of the real-time wall thickness is calculated according to the average wall thickness.
4. The method for preparing a high-strength polyethylene water supply pipe according to claim 3, characterized in that: The melt temperature adjusted according to the real-time straightness and the preset standard straightness correction includes: The melt temperature after correction adjustment is reduced according to the real-time straightness that is less than the standard straightness, the standard straightness and a preset correction factor.
Citation Information
Patent Citations
Polyethylene water supply pipe material and preparation method thereof
CN108485026A
Method of energy distribution and consumption control for plastic injection and extrusion processes
CN101890792A
Polyethylene water supply pipe
CN103524854A