A negative electrode binder, a negative electrode sheet and a lithium ion battery thereof

By adopting a negative electrode adhesive with a hollow tubular structure, the problems of low peel strength and poor conductivity in the prior art are solved, and the effect of effectively suppressing expansion and improving battery performance of the silicon-based negative electrode is achieved.

CN118652647BActive Publication Date: 2024-11-29SHENZHEN HAODYNE TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411127581.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-29
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The existing modified polyacrylic negative electrode adhesives have problems such as low peel strength and poor conductivity, and it is difficult to effectively suppress the volume expansion of the silicon-based negative electrode.

Method used

A negative electrode binder with a hollow tubular structure is used, which is composed of copolymer segments, including soluble structural units and crosslinked structural units, and is connected to each other through a crosslinked bridge structure to form a stable tubular structure.

Benefits of technology

The negative electrode binder can restrain the deformation of the silicon negative electrode when it expands, suppress expansion, improve the battery's full-charge rebound and long cycle performance, while improving the ionic conductivity, reducing the electrode sheet resistance, and improving the battery's rate performance and low-temperature performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118652647B_ABST
    Figure CN118652647B_ABST
Patent Text Reader

Abstract

In order to overcome the problems of low peel strength and poor conductivity of the negative electrode binder of modified polyacrylic acid in the prior art, the present invention provides a negative electrode binder, a negative electrode sheet and a lithium ion battery thereof, wherein the negative electrode binder is a hollow tubular structure, and the tubular structure includes a copolymer segment, and the copolymer segment includes a solubility structure unit and a cross-linking structure unit, and the cross-linking structure units are interconnected by a cross-linking bridge structure. The negative electrode binder provided in the present application is a hollow tubular structure, which restrains the deformation of the silicon negative electrode when it expands and inhibits its expansion. The hollow structure is conducive to improving ionic conductivity, reducing electrode sheet resistance, enhancing bonding strength, improving battery full charge rebound, and improving battery low temperature performance, long cycle performance and rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of secondary batteries, and in particular relates to a negative electrode binder, a negative electrode sheet and a lithium ion battery thereof. Background Art

[0002] Lithium-ion batteries have the advantages of high operating voltage, long cycle life, low self-discharge rate, and high specific capacity. They are widely used in the fields of new energy vehicles, portable electronic products, and the aerospace industry. In batteries, the positive and negative electrode materials have the greatest impact on the capacity of the battery. The existing silicon-based negative electrode materials have a high specific capacity of up to 4200mAh / g, and are considered to be the most likely material to replace graphite. However, silicon-based negative electrode materials will experience severe volume expansion and contraction (up to 300%) during the battery charging and discharging process. During the battery charging and discharging process, the high expansion rate makes the material very easy to crack and fall off, resulting in battery capacity loss and battery failure.

[0003] In order to alleviate the volume expansion of silicon-based negative electrodes during the charging and discharging process, it is necessary to select negative electrode binders that can inhibit the expansion of negative electrodes. Existing negative electrode binders are mostly water-based binders, including modified polyacrylic acid binders and modified polyacrylate binders. Among them, although modified polyacrylic acid binders can inhibit the expansion of negative electrodes, their liquid absorption is poor, resulting in poor electrolyte wettability of the pole piece; polyacrylic acid binders such as PAA are mature commercial products with low cost and good adhesion to silicon-based materials. PAA helps to form an effective SEI layer during the cycle process to alleviate the transport of lithium ions in the electrode, thereby improving the first effect and cycle performance of the battery. However, when PAA is used as a single binder, it is difficult to effectively inhibit the volume expansion of silicon-based negative electrodes, and there are problems such as pole piece powdering; PAA is modified by grafting, copolymerization, blending, cross-linking, etc. Although the modified PAA has the effect of inhibiting the volume expansion of silicon-based negative electrodes, it still has problems such as low peeling strength and poor conductivity. Summary of the invention

[0004] The technical problem to be solved by the present invention is that the negative electrode binder using modified polyacrylic acid has low peel strength and poor conductivity. The present invention provides a negative electrode binder, a negative electrode composition, a negative electrode sheet and a lithium ion battery thereof.

[0005] In order to solve the above technical problems, the present invention provides a negative electrode binder, which is a hollow tubular structure; the tubular structure includes a copolymer segment, the copolymer segment contains a solubility-compatible structural unit and a cross-linking structural unit, and the cross-linking structural units are interconnected by a cross-linking bridging structure.

[0006] Preferably, the aspect ratio of the negative electrode binder is 10-40.

[0007] Preferably, the length of the negative electrode binder is 500-2000 nm, and the diameter of the negative electrode binder is 50-100 nm.

[0008] Preferably, the cross-linking structural unit is a structural unit formed by the polymerization of a cross-linking group monomer, and the cross-linking bridging structure is a connection structure formed between different cross-linking structural units after the cross-linking reaction between a multifunctional cross-linking agent and a cross-linking group monomer, and the cross-linking group monomer includes one or more of glycidyl (meth)acrylate, diacetone acrylamide, ethyl acetoacetate methacrylate, hydroxypropyl acrylate, hydroxybutyl acrylate and dimethylaminoethyl acrylate; the multifunctional cross-linking agent includes one or more of an amine compound, adipic acid dihydrazide, a hydroxy resin, an epoxy curing agent and an amino resin.

[0009] Preferably, the mass ratio of the cross-linked structural unit to the cross-linked bridging structure is (30-50): (2-4).

[0010] Preferably, the soluble structural unit is a structural unit formed by polymerization of soluble polymer monomers, and the soluble polymer monomers include one or more of acrylic acid, acrylamide, methacrylic acid, acrylonitrile, N,N-dimethylacrylamide, and isooctyl acrylate.

[0011] Preferably, the mass ratio of the lyophilic structural unit to the cross-linked structural unit is 20:(30-50).

[0012] Preferably, the glass transition temperature of the negative electrode binder is 0-60° C.; and the electrolyte swelling degree of the negative electrode binder is 30%-70%.

[0013] In a second aspect, the present application provides a negative electrode sheet, comprising a negative electrode active material layer, wherein the negative electrode active material layer comprises a negative electrode active material and the negative electrode binder described above, wherein the negative electrode active material comprises a silicon-based negative electrode.

[0014] In a third aspect, the present application provides a lithium-ion battery, comprising a positive electrode sheet, an electrolyte and the negative electrode sheet described above.

[0015] The negative electrode binder provided in the present application is a hollow tubular structure, which restrains the deformation of the silicon negative electrode when it expands, inhibits its expansion, improves the battery's full-charge rebound, and improves the long-cycle performance; the hollow structure is beneficial to improving the ionic conductivity, reducing the electrode sheet resistance, and improving the battery rate performance and low-temperature performance; the tubular structure includes a copolymer segment, and the copolymer segment contains a solubility-philic structure unit and a cross-linking structure unit, and the cross-linking structure units are interconnected by a cross-linking bridge structure. By cross-linking different cross-linking structure units with each other by using the cross-linking bridge structure, it is beneficial to maintain the stability of the hollow tubular structure, improve its structural strength and service life, and thus improve the binding strength for the negative electrode active material; the swelling degree of the negative electrode binder to the electrolyte is 30~70%, which has the effect of improving the electrolyte wettability and flexibility of the electrode sheet, and improving the long-cycle performance and low-temperature performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a schematic diagram of the preparation process of the negative electrode binder provided in this application. DETAILED DESCRIPTION

[0017] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0018] In the description of the present invention, the term "structural unit" refers to the smallest unit formed on the copolymer segment after a single monomer participates in the polymerization, wherein a "solubility-philic structural unit" refers to a structural unit formed by a solubility-philic polymer monomer with a solubility-philic functional group, a "cross-linking structural unit" refers to a structural unit formed by a cross-linking group monomer with a cross-linkable functional group, and a "soluphobic structural unit" refers to a structural unit formed by a solubility-phobic polymer monomer.

[0019] In the description of the present invention, the term "solubility functional group" refers to a group that is soluble in a polar solvent, and the polar solvent includes water and / or an alcohol solvent. Preferably, the polar solvent is a combination of water and an alcohol solvent, wherein the alcohol solvent includes an ethanol solvent.

[0020] In the description of the present invention, the term "solvophobic functional group" refers to a group that is insoluble in a polar solvent.

[0021] An embodiment of the present application provides a negative electrode binder, which is a hollow tubular structure; the tubular structure includes a copolymer segment, the copolymer segment includes a solubility-compatible structural unit and a cross-linking structural unit, and the cross-linking structural units are interconnected by a cross-linking bridging structure.

[0022] The negative electrode binder provided in the present application is a long tubular structure. This long tubular binder restrains the deformation of the silicon negative electrode when it expands and inhibits its expansion. The negative electrode binder is a long tubular structure with a hollow tubular structure, similar to the carbon nanotube structure, which is beneficial to improving ionic conductivity and reducing electrode sheet resistance.

[0023] The negative electrode binder provided in the present application is a hollow tubular structure, which restrains the deformation of the silicon negative electrode when it expands, inhibits its expansion, improves the full-charge rebound of the battery, and improves the long-cycle performance; the hollow structure is beneficial to improving the ionic conductivity, reducing the electrode sheet resistance, and improving the battery rate performance and low-temperature performance; the tubular structure includes a copolymer segment, the copolymer segment contains a solubility-philic structure unit and a cross-linking structure unit, the cross-linking structure units are interconnected by a cross-linking bridge structure, and different cross-linking structure units are cross-linked by using the cross-linking bridge structure, which is beneficial to maintaining the stability of the hollow tubular structure and improving its structural strength and service life; the swelling degree of the negative electrode binder to the electrolyte is 30~70%, which has the effect of improving the electrolyte wettability and flexibility of the electrode sheet, and improving the long-cycle performance and low-temperature performance of the battery; the negative electrode binder with a hollow tubular structure is beneficial to the transmission of lithium ions, can improve the kinetics and reduce the internal resistance, can participate in regulating the desolvation and re-embedding process of lithium ions, and optimize the electrochemical performance of the battery.

[0024] In some embodiments, the aspect ratio of the negative electrode binder is 10-40.

[0025] The binder with a hollow tubular structure has an aspect ratio of 10 to 40. A larger aspect ratio is conducive to the binder being wrapped around the surface of the silicon-based negative electrode, thereby restraining its deformation and inhibiting its expansion when the silicon negative electrode expands.

[0026] The aspect ratio of the negative electrode binder may be any one of the following ranges: 10 to 15, 15 to 18, 18 to 22, 22 to 26, 26 to 30, 30 to 34, or 34 to 40. When the aspect ratio of the negative electrode binder is less than 10, the binding capacity of the negative electrode binder is insufficient and the full charge rebound rate is large; when the aspect ratio of the negative electrode binder is greater than 40, the flexibility of the negative electrode sheet deteriorates.

[0027] In some embodiments, the length of the negative electrode binder is 500-2000 nm, and the diameter of the negative electrode binder is 50-100 nm.

[0028] Specifically, the aspect ratio is calculated by dividing the length by the diameter. The aspect ratio of the negative electrode binder can be calculated by the length and diameter of the negative electrode binder. The length of the negative electrode binder is in the range of 500~2000nm, the diameter of the negative electrode binder is in the range of 50~100nm, and the aspect ratio is in the range of 10~40. It is wound on the surface of the silicon-based negative electrode, which can better inhibit the expansion of the silicon-based negative electrode and improve the battery's full-charge rebound and long-cycle performance; at the same time, it contains a hollow tubular structure, similar to carbon nanotubes, which can improve the ionic conductivity of the negative electrode binder, reduce the electrode sheet resistance, and improve the battery rate performance and low-temperature performance.

[0029] In some embodiments, the cross-linking structural unit is a structural unit formed by the polymerization of a cross-linking group monomer, and the cross-linking bridging structure is a connection structure formed between different cross-linking structural units after the cross-linking reaction between a multifunctional cross-linking agent and a cross-linking group monomer, and the cross-linking group monomer includes one or more of (meth) glycidyl acrylate, diacetone acrylamide, ethyl acetoacetate methacrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, and dimethylaminoethyl acrylate; the multifunctional cross-linking agent includes one or more of an amine compound, adipic acid dihydrazide, a hydroxy resin, an epoxy curing agent, and an amino resin.

[0030] Specifically, the cross-linked structural unit is a structural unit formed by the polymerization of cross-linked group monomers, and the cross-linked bridging structure is formed between different cross-linked structural units and is obtained by the reaction of a multi-functional cross-linking agent; when the multi-functional cross-linking agent is selected from the above compounds, it can be beneficial to maintain the stability of the hollow tubular structure and improve the strength and service life of the tubular structure.

[0031] The solubility-affinity structural unit and the cross-linking structural unit in the negative electrode binder act together in the bonding process between the electrode material and the current collector. When the cross-linking structural unit is selected from the above compounds, it helps the adhesion between the negative electrode binder and the current collector (such as copper foil), and enhances the mechanical strength of the electrode by forming chemical bonds or physical adsorption.

[0032] In some embodiments, the glycidyl (meth)acrylate includes one or more of glycidyl methacrylate and glycidyl acrylate.

[0033] In some embodiments, the amine compound includes one or both of ethylenediamine and hexamethylenediamine.

[0034] In some embodiments, the mass ratio of the cross-linked structural unit to the cross-linked bridging structure is (30-50): (2-4).

[0035] The mass ratio of the cross-linked structural unit to the cross-linked bridging structure is (30-50): (2-4), which can also be understood as the mass ratio of the cross-linked group monomer to the multifunctional cross-linking agent added when preparing the negative electrode binder is (30-50): (2-4), forming a structure in which the cross-linked structural units are interconnected by the cross-linked bridging structure, which helps to maintain the stability of the hollow tubular structure and improve the strength stability of the tubular structure.

[0036] In some embodiments, the solubility-loving structural unit is a structural unit formed by polymerization of solubility-loving polymer monomers.

[0037] In some embodiments, the lyophilic polymer monomers include one or more of acrylic acid monomers, acrylic acid ester monomers, acrylamide monomers, and acrylonitrile monomers.

[0038] In a preferred embodiment, the soluble polymer monomer includes one or more of acrylic acid, acrylamide, methacrylic acid, acrylonitrile, N,N-dimethylacrylamide, and isooctyl acrylate.

[0039] Specifically, when the solubility structural unit is selected from the above compounds, it helps to disperse the negative electrode binder in water or other polar solvents, promotes the uniform mixing of the binder and the active material particles, and at the same time, it has a high affinity for the electrolyte, which is conducive to improving the liquid absorption capacity of the negative electrode binder, improving the liquid absorption rate of the negative electrode binder, and improving the swelling degree of the electrolyte, thereby improving the wettability of the electrode to the electrolyte, improving the long cycle and low temperature performance of the battery. The formed negative electrode binder has a low Tg (glass transition temperature), which can better fit the main material and substrate after the electrode is rolled, and improve the peel strength.

[0040] In some embodiments, the tubular structure further comprises a solvophobic structural unit, wherein the solvophobic structural unit is a structural unit formed by polymerization of a solvophobic polymer monomer, wherein the solvophobic polymer monomer comprises one or more of styrene, methylstyrene, and tert-butyl acrylate.

[0041] Specifically, Figure 1 As shown, the negative electrode binder with a tubular structure also includes a solvophobic structural unit, which is located on the inner wall of the tubular structure and is a residue from the preparation process. The solvophobic structural unit has solvophobicity, and the added solvophobic polymer monomer is conducive to the formation of a negative electrode binder with a tubular structure.

[0042] It should be noted that when the chain transfer agent is removed, the solvophobic structural unit may not be completely removed, or the solvophobic structural unit may be completely removed when the chain transfer agent is removed. Figure 1 The schematic diagram only represents a situation in which the solvophobic structural unit is not completely removed when the chain transfer agent is removed.

[0043] In some embodiments, the weight ratio of the soluble structural unit to the cross-linking structural unit is 20: (30-50).

[0044] Specifically, the weight ratio of the solubility-philic structural unit to the cross-linking structural unit is 20:(30~50), which helps to form a negative electrode binder with an electrolyte swelling degree of 30%~70% and a glass transition temperature of 0~60°C, thereby improving the bonding strength and flexibility of the electrode sheet and improving the low temperature performance and cycle performance of the battery.

[0045] In some embodiments, the glass transition temperature of the negative electrode binder is 0-60°C.

[0046] When the glass transition temperature of the negative electrode binder is within the above range, the negative electrode binder is softer in a low temperature environment without affecting the bonding performance, which can improve the bonding strength and flexibility of the electrode sheet and improve the low temperature performance and long cycle performance of the battery.

[0047] If the glass transition temperature of the negative electrode binder is greater than 60°C, the electrolyte swelling degree of the negative electrode binder will decrease, the flexibility and electrolyte wettability of the prepared electrode will be poor, and the battery's low temperature performance, long cycle performance and rate performance will decrease.

[0048] Specifically, the glass transition temperature of the negative electrode binder can be 0-10°C, 10°C-20°C, 20°C-30°C, 30°C-40°C, 40°C-50°C, 50°C-60°C, etc., as long as the glass transition temperature of the negative electrode binder is within the range of 0-60°C.

[0049] In some embodiments, the electrolyte swelling degree of the negative electrode binder is 30% to 70%.

[0050] Specifically, the electrolyte swelling degree of the negative electrode binder is in the range of 30-70%, which can improve the wettability of the electrode electrolyte. The swelling degree has a wide control range and can be changed according to demand.

[0051] The electrolyte swelling degree of the negative electrode binder may be 30-35%, 35%-40%, 40-50%, 50-60% or 60-70%, etc., as long as the electrolyte swelling degree of the negative electrode binder is within the range of 30%-70%.

[0052] Compared with polyacrylic acid binders, the negative electrode binder provided by the present application has a hollow tubular structure. When the silicon negative electrode expands, the tubular structure restrains its deformation, inhibits its expansion, improves the battery's full-charge rebound, and improves the battery's long-cycle performance. The hollow structure is conducive to lithium ion transmission, improves ion conductivity, reduces the pole piece resistance, reduces the battery impedance, and improves the battery's rate performance and low-temperature performance. The negative electrode binder includes a solubility-philic structural unit and a cross-linking structural unit, wherein the solubility-philic structural unit has a fast absorption rate for the electrolyte, and a swelling degree of 30-70% for the electrolyte, which improves the electrolyte wettability of the pole piece, and improves the battery's long-cycle performance and low-temperature performance; the negative electrode binder has a low glass transition temperature, which improves the bonding strength of the pole piece, improves the peeling strength of the pole piece, and improves the low-temperature performance of the battery.

[0053] like Figure 1 As shown, the present application provides a method for preparing a negative electrode binder, wherein a solubility-philic polymer monomer, a cross-linking group monomer and a chain transfer agent are copolymerized under green light conditions, and then a solubility-phobic polymer monomer is added and copolymerized under the condition of a thermal initiator to obtain a tubular structure material; then a multifunctional cross-linking agent is added, and the multifunctional cross-linking agent and the cross-linking group monomer are cross-linked with each other; finally, a photoinitiator is added and the chain transfer agent is removed to obtain a negative electrode binder with a hollow tubular structure.

[0054] Specifically, the chain transfer agent serves as a linking point between the solubility-philic structural unit and the soluphobic structural unit. First, a tubular structured nanomaterial is prepared by polymerization-induced self-assembly. In the nanomaterial, the solubility-philic structural unit obtained by polymerization of the solubility-philic polymer monomer is located in the inner core, and the solubility-philic structural unit and the cross-linking structural unit formed by the solubility-philic polymer monomer and the cross-linking group monomer are located in the outer layer. Then, a multifunctional cross-linking agent is added, and the multifunctional cross-linking agent and the cross-linking group monomer are cross-linked with each other. Then, the chain transfer agent and the solubility-philic structural unit at the linking point are cut off by a strong oxidizing high initiator or a high free radical high initiator. Finally, the cut solubility-philic structural unit and chain transfer agent are removed by filtration to obtain a hollow tubular structured negative electrode binder.

[0055] In the process of preparing the negative electrode binder, the removed solvophobic structural unit is obtained by polymerization of solvophobic polymer monomers, and the solvophobic polymer monomers include one or more of styrene, methyl styrene, and tert-butyl acrylate.

[0056] The multifunctional cross-linking agent is formed between different cross-linking structural units after a cross-linking reaction with a cross-linking group monomer, thereby improving the mechanical strength of the tubular structure and improving the overall strength and stability of the negative electrode binder.

[0057] In some embodiments, the chain transfer agent is [3-(n-butyl trithiocarbonate) propionic acid-diethylene glycol-(4-cyano-4-(ethylalkylthiocarbonyl) pentanoic acid)].

[0058] In some embodiments, the total mass of the solubility-philic polymer monomer, the solubility-phobic polymer monomer and the cross-linking group monomer is m1, the mass of the chain transfer agent is m2, and the ratio of m1 to m2 is 100:(0.5-2).

[0059] Specifically, the chain transfer agent acts as a link between the solubility-philic structural unit and the solvophobic structural unit, and its addition amount affects the formation of the hollow tubular structure of the negative electrode binder. The ratio of m1 to m2 is in the range of 100:(0.5~2), which helps to generate a hollow tubular polymer with an aspect ratio of 10~40. If the ratio of m1 to m2 is too large, the amount of chain transfer agent added is too small, the number of link points between the solubility-philic structural unit and the solvophobic structural unit is insufficient, and the self-assembled structure formed is unstable, which in turn affects the formation of the tubular morphology; if the ratio of m1 to m2 is too small, it increases the difficulty of removing the subsequent solvophobic structural unit and chain transfer agent.

[0060] In some embodiments, in the preparation of the negative electrode binder, the total weight of the added solubility polymer monomer, the cross-linking group monomer, and the solubility polymer monomer is m3, the weight of the added solubility polymer monomer is m4, and m4:m3 is (30-50):100.

[0061] If the weight portion of the added solvophobic polymer monomer is too low, the aspect ratio of the negative electrode binder with a hollow tubular structure formed will be too large, and the flexibility will decrease; if the weight portion of the added solvophobic polymer monomer is too high, the aspect ratio of the negative electrode binder with a hollow tubular structure formed will be too low, and the effect of inhibiting the expansion of the silicon-based negative electrode will decrease.

[0062] In a second aspect, the present application provides a negative electrode sheet, comprising a negative electrode active material layer, wherein the negative electrode active material layer comprises a negative electrode active material and the negative electrode binder described above, wherein the negative electrode active material comprises a silicon-based negative electrode.

[0063] The negative electrode sheet provided in the present application adopts the above-mentioned negative electrode binder, which is a polyacrylate polymer, and can improve the electrolyte wettability and flexibility of the electrode sheet; the negative electrode binder is a hollow tubular structure, and its tubular structure restrains its deformation when the silicon negative electrode expands and inhibits its expansion. The hollow structure is beneficial to improving ionic conductivity and reducing electrode sheet resistance.

[0064] In some embodiments, the negative electrode active material layer further includes a conductive agent and a thickener.

[0065] Specifically, the conductive agent includes at least one of conductive carbon black, conductive graphite, carbon nanotubes, graphene, acetylene black, Ketjen black, and other novel conductive agents.

[0066] Thickeners include CMC.

[0067] The negative electrode active material layer further includes one of a water-based binder, an oil-based binder, polyvinyl alcohol, polytetrafluoroethylene, polyolefins, and polyurethane. The water-based binder includes styrene-butadiene rubber and PAA, and the oil-based binder includes PVDF.

[0068] In some embodiments, the silicon-based negative electrode includes one of simple silicon, a silicon-carbon composite material, a silicon-oxygen composite material, and a composite material formed by silicon and a metal alloy.

[0069] In a third aspect, the present application provides a lithium-ion battery, comprising a positive electrode sheet, an electrolyte and the negative electrode sheet described above.

[0070] The lithium ion battery provided by the present application adopts the above-mentioned negative electrode sheet, and the negative electrode binder contained therein is a hollow tubular structure with an aspect ratio of 10 to 40. Its large aspect ratio allows the negative electrode binder with a tubular structure to be wrapped around the surface of the silicon-based negative electrode, restraining its deformation when the silicon negative electrode expands and inhibiting its expansion, wherein the hollow structure is conducive to improving ionic conductivity and reducing electrode sheet resistance; the tubular structure includes a copolymer segment, the copolymer segment includes a solubility structure unit and a cross-linking structure unit, and the cross-linking structure units are interconnected by a cross-linking bridge structure. By cross-linking different cross-linking structure units with each other by using the cross-linking bridge structure, it is conducive to maintaining the stability of the hollow tubular structure and improving its structural strength and service life; the negative electrode binder has a fast absorption rate of the electrolyte, and the swelling degree of the electrolyte is 30 to 70%, which improves the electrolyte wettability of the electrode sheet; the negative electrode binder has a low glass transition temperature, which is conducive to the wetting of the binder with the main material and the substrate, and improves the peel strength of the electrode sheet; the battery prepared using the negative electrode binder has high long cycle performance, low temperature performance and rate performance.

[0071] The present invention is further described below by way of examples.

[0072] The negative electrode binder, negative electrode sheet and lithium ion battery disclosed in the present invention are specifically described.

[0073] Example 1

[0074] The hollow tubular structure of the negative electrode binder provided in the present application is prepared by the following method:

[0075] The soluble polymer monomer, crosslinking group monomer and chain transfer agent are added to the solvent and then together under green light (λ = 530nm, 2.0mW / cm 2) to initiate copolymerization, and then add the solvophobic polymer monomer to prepare a long fiber polymer by polymerization induced self-assembly under the thermal initiation of azobisisobutyronitrile. Then add a multifunctional crosslinking agent and stir for a certain period of time, add a photoinitiator TPO (diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide) to initiate cleavage, add a chain transfer agent RAFT agent for excision, and then remove the excised solvophobic structural unit and chain transfer agent core by filtration to obtain a hollow tubular material. The total weight of the solvophilic polymer monomer, the crosslinking group monomer, and the solvophobic polymer monomer is 100 parts, and the photoinitiator TPO is 5 parts.

[0076] 1) Preparation of negative electrode binder

[0077] S1: The negative electrode binder raw material includes the following components: Solubility polymer monomer: 10 parts of acrylic acid, 10 parts of isooctyl acrylate;

[0078] Cross-linking group monomer: 20 parts of diacetone acrylamide, 20 parts of acetoacetoxyethyl methacrylate;

[0079] Solvophobic polymer monomer: 39 parts of styrene, 1 part of methacrylic acid;

[0080] Chain transfer agent [3-(n-butyl trithiocarbonate) propionic acid-diethylene glycol-(4-cyano-4-(ethylalkylthiocarbonyl) pentanoic acid)] 1 part, multifunctional crosslinking agent adipic acid dihydrazide 3 parts, initiator azobisisobutyronitrile 0.1 parts.

[0081] The solvent is ethanol / water = 6:4, and the solid content is controlled to be 30%;

[0082] The negative electrode binder prepared in Example 1 is a long tubular structure with a length of 1200 nm, a diameter of 60 nm, an aspect ratio of 20, a glass transition temperature of 27°C (the theoretical value of the solubility-philic polymer is 15°C, and the actual value is 27°C, which is affected by the post-crosslinking and copolymerization of some solubility-phobic polymer monomers, and only the actual value is recorded later), and the electrolyte swelling degree is 45%.

[0083] 2) Preparation of negative electrode sheet:

[0084] 2.2wt% of the negative electrode binder prepared in step 1) above, 96.4wt% of the negative electrode active material silicon negative electrode, 1wt% of the negative electrode conductive agent conductive carbon black, and 1.2wt% of the thickener sodium carboxymethyl cellulose (CMC) were mixed, and deionized water was added for stirring to prepare the negative electrode slurry. The negative electrode slurry was then coated on both surfaces of the negative electrode current collector copper foil, and after drying, cold pressing, slitting and other processes, the negative electrode sheet was obtained.

[0085] 3) Preparation of positive electrode:

[0086] 97.4wt% of positive electrode active material lithium iron phosphate, 0.9wt% of positive electrode conductive agent conductive carbon black, and 1.7wt% of positive electrode binder polyvinylidene fluoride were added to N-methylpyrrolidone and stirred to prepare positive electrode slurry. The positive electrode slurry was then coated on both surfaces of the positive electrode current collector aluminum foil, and after drying, cold pressing, slitting and other processes, a positive electrode sheet was obtained.

[0087] 4) Lithium-ion battery preparation:

[0088] The positive electrode sheet, the isolation film (PE film) and the negative electrode sheet are stacked in order, so that the isolation film is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, to form an electrode assembly, the electrode assembly is placed in an outer package, and a commercially available electrolyte is injected and packaged, and then a lithium-ion battery is obtained through processes such as liquid injection, formation, and exhaust.

[0089] Example 2

[0090] Most of the steps of Example 2 are the same as those of Example 1, except that 49 parts of styrene, 15 parts of ethyl acetoacetate methacrylate and 15 parts of diacetone acrylamide are added to the raw materials of the negative electrode binder in step S1, and the rest are the same as those of Example 1.

[0091] The negative electrode binder prepared in Example 2 has a length of 550 nm, a diameter of 50 nm, an aspect ratio of 11, a glass transition temperature of 24° C., and an electrolyte swelling degree of 64%.

[0092] Example 3

[0093] Most of the steps of Example 3 are the same as those of Example 1, except that 29 parts of styrene, 25 parts of ethyl acetoacetate methacrylate and 25 parts of diacetone acrylamide are added to the raw materials of the negative electrode binder in step S1, and the rest are the same as those of Example 1.

[0094] The negative electrode binder prepared in Example 3 has a length of 1900 nm, a diameter of 50 nm, an aspect ratio of 38, a glass transition temperature of 31° C., and an electrolyte swelling degree of 32%.

[0095] Example 4

[0096] Most of the steps in Example 4 are the same as those in Example 1, except that 3 parts of chain transfer agent are added to the raw materials of the negative electrode binder in step S1, the total mass of the solubility-philic polymer monomer, the solubility-phobic polymer monomer and the cross-linking group monomer is m1, the mass of the chain transfer agent is m2, and the ratio of m1 to m2 is 100:3; the rest is the same as in Example 1.

[0097] The negative electrode binder prepared in Example 4 has a length of 800 nm, a diameter of 50 nm, an aspect ratio of 16, a glass transition temperature of 26° C., and an electrolyte swelling degree of 51%.

[0098] Example 5

[0099] Most of the steps in Example 5 are the same as those in Example 1, except that 0.5 parts of chain transfer agent are added to the raw materials of the negative electrode binder in step S1, the total mass of the solubility-philic polymer monomer, the solubility-phobic polymer monomer and the cross-linking group monomer is m1, the mass of the chain transfer agent is m2, and the ratio of m1 to m2 is 100:0.5; the rest is the same as in Example 1.

[0100] The negative electrode binder prepared in Example 5 has a length of 1500 nm, a diameter of 65 nm, an aspect ratio of 23, a glass transition temperature of 28° C., and an electrolyte swelling degree of 43%.

[0101] Example 6

[0102] Most of the steps of Example 6 are the same as those of Example 1, except that 25 parts of styrene, 15 parts of acrylic acid, and 35 parts of diacetone acrylamide are added to the raw materials of the negative electrode binder in step S1, and the rest is the same as Example 1.

[0103] The negative electrode binder prepared in Example 6 has a length of 1000 nm, a diameter of 80 nm, an aspect ratio of 12.5, a glass transition temperature of 67° C., and an electrolyte swelling degree of 31%.

[0104] Example 7

[0105] Most of the steps of Example 7 are the same as those of Example 1, except that 59 parts of styrene, 10 parts of ethyl acetoacetate methacrylate and 10 parts of diacetone acrylamide are added to the raw materials of the negative electrode binder in step S1, and the rest are the same as those of Example 1.

[0106] The negative electrode binder prepared in Example 7 has a length of 480 nm, a diameter of 80 nm, an aspect ratio of 6, a glass transition temperature of 21° C., and an electrolyte swelling degree of 73%.

[0107] Example 8

[0108] Most of the steps of Example 8 are the same as those of Example 1, except that 19 parts of styrene, 30 parts of ethyl acetoacetate methacrylate and 30 parts of diacetone acrylamide are added to the raw materials of the negative electrode binder in step S1, and the rest are the same as those of Example 1.

[0109] The negative electrode binder prepared in Example 8 has a length of 2200 nm, a diameter of 40 nm, an aspect ratio of 55, a glass transition temperature of 35° C., and an electrolyte swelling degree of 26%.

[0110] Comparative Example 1

[0111] Most of the steps of Comparative Example 1 are the same as those of Example 1, except that the negative electrode binder is polyacrylic acid. The rest is the same as Example 1.

[0112] Comparative Example 2

[0113] Most of the steps of Comparative Example 2 and Example 1 are the same, except that the solid tubular structure prepared by the negative electrode binder is without the addition of photoinitiator and chain transfer agent RAFT agent, and there is no chain transfer agent excision step.

[0114] Performance Test:

[0115] The test methods for the length and diameter of the adhesives in the above embodiments are as follows:

[0116] The adhesives of the above-mentioned embodiments were prepared into test samples, and the length and diameter of the adhesives were measured using a scanning electron microscope (SEM).

[0117] Pole performance test:

[0118] The negative electrode sheets prepared in the above examples and comparative examples were subjected to the following tests.

[0119] 1) Negative electrode peel strength test:

[0120] The stainless steel plate and the current collector were fixed on the fixture of the peel force tester, and a 180-degree peel test was performed at a speed of 10 mm / min and a load of 10 N.

[0121] Negative electrode flexibility test:

[0122] Wind the negative electrode sheet on the surface of a winding needle with a fixed diameter, and observe the cracking state of the electrode sheet surface under a microscope;

[0123] Electrolyte wettability:

[0124] At 2cm Add 1 drop of electrolyte to the 2 cm thick negative electrode sheet and record the time it takes to diffuse to the edge of the negative electrode sheet;

[0125] The above test results are shown in Table 1.

[0126] (1) The test results obtained in the embodiments and comparative examples are listed in Table 1.

[0127] Table 1

[0128]

[0129] As shown in Table 1, by comparing Examples 1-8 with Comparative Example 1, it can be seen that the negative electrode binder prepared in the present application is a hollow tubular structure and is a polyacrylate polymer, which has a strong bonding strength, can improve the peel strength of the pole piece, and the pole piece has good flexibility and wettability, and the electrolyte swelling degree of the negative electrode binder is improved, and the electrolyte swelling degree of the negative electrode binder reaches 30-70%. By comparing Examples 1-3 with Comparative Example 2, the hollow tubular structure of the negative electrode binder also helps to improve the electrolyte swelling degree of the negative electrode binder.

[0130] Comparing Example 1 with Examples 7-8, the weight ratio of the solubility-philic structural unit to the cross-linking structural unit in Example 7 is higher than the range of 20: (30-50), the weight ratio of the added solubility-phobic polymer monomer is too much, the mass ratio of the cross-linking structural unit to the cross-linking bridging structure is lower than the range of (30-50): (1-2), the aspect ratio of the obtained negative electrode binder is lower than 10, the peel strength of the pole piece is poor, and the flexibility of the pole piece is poor. The weight ratio of the solubility-philic structural unit to the cross-linking structural unit in Example 8 is lower than the range of 20: (30-50), and the addition The weight proportion of the solvophobic polymer monomer is too small, the aspect ratio of the obtained negative electrode binder is higher than 40, and the flexibility and wettability of the pole piece are poor, indicating that the weight proportion of the solvophilic structural unit and the cross-linking structural unit is in the range of 20: (30~50), the mass ratio of the cross-linking structural unit and the cross-linking bridging structure is in the range of (30~50): (1~2), m4: m3 is in the range of (30~50): 100, and the aspect ratio of the obtained negative electrode binder is in the range of 10~40, which helps to improve the peel strength of the negative electrode sheet, and the flexibility and wettability of the pole sheet are good. Comparing Example 1 with Example 6, the glass transition temperature of the negative electrode binder is in the range of 0~60℃, the peel strength of the negative electrode sheet is high, and the flexibility and wettability of the pole sheet are good. Comparing Example 1 with Example 4, the total mass of the solubility-philic polymer monomer, the solubility-phobic polymer monomer and the cross-linking group monomer is m1, the mass of the chain transfer agent is m2, and the ratio of m1 to m2 is in the range of 100:(0.5~2). The negative electrode sheet prepared with the negative electrode binder has better wettability and higher peel strength.

[0131] Electrical performance test:

[0132] The negative electrode sheets and lithium-ion batteries prepared in the above examples and comparative examples were subjected to the following tests.

[0133] 1) Full power rebound test:

[0134] Test the thickness of the negative electrode sheet of the uncharged battery cell D1. At room temperature, 1C constant current and constant voltage to 4.2V, and then test the thickness of the negative electrode sheet D2 after full charge. Full charge thickness rebound = (D2-D1) / D1×100%.

[0135] 2) Low temperature discharge test

[0136] The specific method is:

[0137] Charging: 1C constant current and constant voltage at room temperature to 4.2V, 0.05C cut-off, record capacity C 01 ;

[0138] Discharge: Discharge at 1C constant current to 3.0V at -10℃, record capacity C 02 ; C 02 / C 01 ×100%.

[0139] The test results are shown in Table 2 below.

[0140] 3) Rate performance test

[0141] The specific method is:

[0142] Charging: 1C constant current and constant voltage to 4.2V, 0.05C cut-off; Discharging: discharge at 1C constant current to 3.0V; record the discharge capacity C1.

[0143] Charging: charge to 4.2V with 1C constant current; Discharging: discharge to 3.0V with 1C constant current, and record the discharge capacity C2.

[0144] 3C discharge capacity retention rate = C1 / C2×100%.

[0145] 4) The test method of DCIR test is:

[0146] ①Test temperature: 25℃; ②SOC: 50%; ③DCIR test method: 3C discharge for 30s.

[0147] At 25°C, the battery is left to stand for 30 minutes under the above SOC conditions, and the voltage U1 is recorded. It is discharged at I0 3C for 30 seconds, and the voltage U2 is recorded. DCIR=(U1-U2) / I0.

[0148] 5) 85℃ storage retention rate test

[0149] The method is: after fully charged, place it in an 85℃ oven for 8 hours, take it out and test it at 1C discharge to 3.0V, record the discharge capacity C3. At 25℃, charge the battery at 1C constant current to 4.2V and cut off at 0.05C, discharge it at 1C constant current to 3.0V, and test the battery discharge capacity C4.

[0150] 85℃ storage retention rate = C3 / C4×100%.

[0151] 6) 25℃ cycle test

[0152] The specific method is: let the soft-pack battery stand until the temperature reaches 25℃±2℃, test the first discharge capacity of the soft-pack battery, recorded as C5, 1C constant current and constant voltage to 4.2V, 0.05C cut-off; discharge: 1C constant current discharge to 3.0V, cycle 500 times, and record the discharge capacity C6. 25℃ cycle capacity retention rate = C6 / C5×100%.

[0153] The above test results are shown in Table 2 below.

[0154] Table 2

[0155]

[0156] As can be seen from Table 2, by comparing Examples 1-8 with Comparative Example 1, it can be obtained that the battery full charge rebound rate in Examples 1-8 is lower, the low temperature discharge capacity retention rate is high, the normal temperature cycle capacity retention rate is high, and the rate discharge capacity retention rate is high, indicating that the hollow tubular structure provided by the present application restrains the deformation of the silicon negative electrode when it expands, inhibits its expansion, improves the battery full charge rebound, and improves the long cycle performance and rate performance. By comparing Examples 1-3 with Comparative Example 2, the negative electrode binder in Comparative Example 2 is a non-hollow structure, the battery's 3C rate discharge capacity retention rate is low, and the battery internal resistance is high, indicating that the negative electrode binder provided by the present application, wherein the hollow structure is conducive to improving ionic conductivity, reducing battery impedance, and improving the battery high rate discharge performance.

[0157] Comparison between Example 1 and Example 7-8 shows that if the aspect ratio of the negative electrode binder is too low, the ability to suppress the expansion of the silicon negative electrode is reduced. If the aspect ratio is too high, the internal resistance of the battery increases, the low-temperature discharge capacity retention rate decreases, the rate performance decreases, and the cycle capacity retention rate decreases. This shows that the aspect ratio of the negative electrode binder is in the range of 10 to 40, which helps to improve the low-temperature discharge performance and rate performance of the battery, reduce the internal resistance of the battery and the rebound rate of the pole piece, suppress the expansion of the silicon-based negative electrode, and improve the cycle performance of the battery. Comparison between Example 1 and Example 6 shows that the glass transition temperature of the negative electrode binder is greater than 60°C, the rate performance, long cycle performance and low temperature performance of the battery are poor, and the internal resistance is high, which shows that the glass transition temperature of the negative electrode binder is 0 to 60°C, which helps to improve the low-temperature performance, long cycle performance and rate performance of the battery and reduce the battery impedance.

[0158] Comparing Example 1 with Example 4, with the total mass of the solubility-philic polymer monomer, the solubility-phobic polymer monomer and the cross-linking group monomer as m1, the mass of the chain transfer agent as m2, and the ratio of m1 to m2 being in the range of 100:(0.5~2), the negative electrode sheet prepared with the negative electrode binder has better wettability, and the battery has better low temperature performance, long cycle performance and rate performance, which also helps to reduce the internal resistance of the battery.

[0159] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A negative electrode binder, characterized in that: The negative electrode binder is a hollow tubular structure; the tubular structure includes a copolymer segment, the copolymer segment includes a solubility unit and a cross-linking unit, and the cross-linking units are interconnected by a cross-linking bridge structure; the aspect ratio of the negative electrode binder is 10-40; the length of the negative electrode binder is 500-2000 nm, and the diameter of the negative electrode binder is 50-100 nm; the mass ratio of the cross-linking unit to the cross-linking bridge structure is (30-50): (2-4); the weight ratio of the solubility unit to the cross-linking unit is 20: (30-50); The cross-linked structural unit is a structural unit formed by the cross-linked group monomer participating in the polymerization, the cross-linked bridging structure is a connection structure formed between different cross-linked structural units after the cross-linking reaction between the multifunctional cross-linking agent and the cross-linked group monomer, the cross-linked group monomer is diacetone acrylamide and acetoacetoxyethyl methacrylate; the multifunctional cross-linking agent is adipic acid dihydrazide; The solubility-affinity structural unit is a structural unit formed by polymerization of solubility-affinity polymer monomers, and the solubility-affinity polymer monomers are acrylic acid and isooctyl acrylate.

2. The negative electrode binder according to claim 1, characterized in that The glass transition temperature of the negative electrode binder is 0-60° C.; the electrolyte swelling degree of the negative electrode binder is 30%-70%.

3. A negative electrode sheet, characterized in that: The invention comprises a negative electrode active material layer, wherein the negative electrode active material layer comprises a negative electrode active material and the negative electrode binder according to any one of claims 1 to 2, and the negative electrode active material comprises a silicon-based negative electrode.

4. A lithium ion battery, characterized in that: It comprises a positive electrode sheet, an electrolyte and the negative electrode sheet as claimed in claim 3.

Citation Information

Patent Citations

  • Method for fast eliminating disulfide ester end groups of RAFT polymers

    CN101775102A

  • Lithium ion battery cathode binder

    CN109378478A