A renewable high-strength and tough heat-treatable reinforced aluminum alloy material and preparation method thereof
Aluminum alloy materials with specific component ratios and T6 heat treatment process have solved the problem of insufficient strength in existing high-strength and high-toughness aluminum alloy materials for automobiles, achieving a significant improvement in both strength and toughness, and are suitable for lightweighting automotive parts.
Patent Information
- Application Number
- CN202411177482.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-26
AI Technical Summary
Existing high-strength and high-toughness aluminum alloy materials for automobiles are insufficient in terms of tensile strength and yield strength, making it difficult to meet the requirements for lightweighting. Furthermore, the proportion of recycled aluminum alloys added is limited, resulting in high costs and making it difficult to achieve weight reduction of parts and energy conservation and emission reduction.
By designing aluminum alloy materials with specific component ratios, including elements such as Cu, Si, Zn, Mn, Mg, Fe, Sr, V, and Ga, and combining them with the T6 heat treatment process, the microstructure of the alloy can be controlled to form nanoscale particles and dispersed phases, thereby improving the strength and toughness of the material.
It achieves high strength and toughness improvement of aluminum alloy materials, with tensile strength ≥350MPa, yield strength ≥250MPa, and elongation after fracture ≥7.0%, which is suitable for automotive steering knuckles, control arms and engine cylinder heads and other components, meeting the requirements of lightweighting.
Smart Images

Figure CN118685669B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum alloys, and in particular to a renewable high-strength and tough heat-treatable reinforced aluminum alloy material and a preparation method thereof. Background Art
[0002] High-strength and toughness materials are widely needed in the automotive field (steering knuckles, car wheels, control arms, engine cylinder heads). From the perspective of technological development trends, the demand for lightweight, high-strength and toughness materials will further increase; for example, higher standard aluminum alloy materials can increase tensile strength and yield strength by more than 30% compared to traditional automotive steering knuckle materials. Therefore, the yield strength and toughness of the materials are required to be high, which can achieve weight reduction of parts and achieve the goal of lightweighting. At present, the commonly used aluminum alloy for automotive shells is A356.2, which belongs to hypoeutectic aluminum alloy. The overall product hardness and strength are low, with tensile strength of (260-280) MPa, yield strength of (180-220) MPa, and elongation after fracture of (7.5-9.5)%. All of them are strictly restricted for impurity elements such as Fe, Zn, Cu, and Mn. The choice of recycled aluminum in alloy preparation is severely limited, and it is difficult to increase the addition ratio of recycled aluminum, which is not conducive to reducing costs and energy conservation and emission reduction.
[0003] In order to overcome the problems and shortcomings of existing high-strength and toughness aluminum alloy materials for automobiles, the present invention further improves the strength and toughness of aluminum alloys by designing the composition, component ratio and smelting technology of aluminum alloys to meet the performance requirements of high-strength and toughness components represented by automobile steering. Summary of the invention
[0004] The object of the present invention is to provide a renewable high-strength and high-toughness heat-treatable strengthened aluminum alloy material and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0005] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a renewable high-strength and tough heat-treatable strengthened aluminum alloy material, composed of the following materials: Cu 0.2%-0.6%, Si 7.5%-9.5%, Zn 0.1%-0.5%, Mn 0.1%-0.3%, Mg 0.25%-0.5%, Fe 0.2%-0.45%, Sr 0.010%-0.045%, V 0.015%-0.065%, Ga0.0065%-0.085%, and the remainder is Al and impurities, wherein the total impurity content is not more than 0.25%.
[0006] As a further improvement of the present invention, the mass fraction ratio of 20≤(Si / (Ga+Mg))≤34.5, and the mass fraction ratio of (Fe+Mn) / V elements is between 6.5 and 23.5.
[0007] As a further improvement of the present invention, the tensile strength of the aluminum alloy component is ≥350MPa, the yield strength is ≥250MPa, and the elongation after fracture is ≥7.0%.
[0008] The present invention also discloses a method for preparing a renewable high-strength and tough heat-treatable reinforced aluminum alloy material, the preparation method comprising the following steps:
[0009] S1. Prepare raw materials according to the formula of aluminum alloy materials, weigh corresponding percentages of each raw material, dry and preheat, heat melt and stir evenly to obtain alloy melt;
[0010] S2. Refining the alloy melt, degassing and removing impurities. After online degassing, the alloy melt enters the filter box and purifies the alloy melt through the preheated ceramic filter plate. The ceramic filter plate can block large-sized impurities and adsorb small-sized impurities. The pore size of the filter plate is 25-45ppi.
[0011] S3. The alloy melt that has been degassed and impurity-removed is sent to a forming device for preparation and then formed. The forming device is low-pressure, gravity or extrusion to obtain an aluminum alloy component.
[0012] As a further improvement of the present invention, the specific steps of the refining treatment in step S2 are to introduce a protective gas into the alloy melt, wherein the protective gas is nitrogen or argon, the amount of the protective gas introduced is 0.15-6 L / min, RJ-01 refining agent is added, the refining time is 15-30 minutes, and the amount of solid refining agent added is 0.2%-0.5% of the melt mass.
[0013] As a further improvement of the present invention, the specific step of degassing in step S2 is to place the alloy melt into a degassing box along the flow channel, and the degassing box is equipped with a dual-rotor rotary degasser for full-line degassing, the rotor speed is set at 400-550r / min, the argon pressure is 0.2-0.4MPa, and the flow rate is 18-28L / min.
[0014] As a further improvement of the present invention, after the step S3 is completed, T6 heat treatment is performed, and the T6 heat treatment process is as follows: the solution temperature is 510±10°C, the insulation time is 3-8 hours, water cooling is 3 minutes to below 60°C, the artificial aging temperature is 160-185°C, the insulation time is 5-8 hours, and the furnace is cooled to room temperature.
[0015] As a further improvement of the present invention, the specific steps of hot melting in step S1 are: adding the recycled aluminum alloy ingot into the smelting furnace for melting, and after it is completely melted, adding pure metals or intermediate alloys of Cu, Mg, Zn, Si and Mn elements, and after it is completely melted, adding AlV, AlSr and AlGa intermediate alloys.
[0016] As a further improvement of the present invention, in step S1, the drying preheating temperature is 100-450° C., the hot melting temperature is 730-800° C., and the stirring time is 5-15 minutes.
[0017] The invention also discloses the application of renewable high-strength and tough heat-treatable reinforced aluminum alloy materials. The renewable high-strength and tough heat-treatable reinforced aluminum alloy materials are applied to steering knuckles, control arms, automobile wheels and engine cylinder head parts.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The aluminum alloy composition of the present invention does not contain precious metals such as Ni and Zr, and elements that may cause poisoning are avoided as much as possible, thereby eliminating the source of "poisoning". The ranges of Si / ((Ga+Mg)) and (Fe+Mn) / V are designed, and the design ranges of elements such as V are controlled at the same time. The harmful AlSiFeMn quaternary second phase is converted into quinary AlSiFeMnV by using the V element, thereby achieving effective control of the precipitation of the primary iron-rich phase, facilitating effective regulation of the morphology, size and distribution of the iron-rich phase, achieving the dual effects of fine grain strengthening and interface coherence strengthening, and enhancing the relative toughness of the alloy while improving the strength. The influence of the alloy on the properties is minimized; combined with the solid solution strengthening brought by Cu, Mg and Zn elements, and the V and Ga elements form nano-sized V-rich and Ga-rich particles in high-pressure and high-speed rapid cooling, which is conducive to the precipitation of Mg2Si strengthening phase during the alloy heat treatment process, thereby improving the high-temperature mechanical properties of the alloy. After forming and undergoing T6 heat treatment, the tensile strength of the aluminum alloy component is ≥350MPa, the yield strength is ≥250MPa, and the elongation after fracture is ≥7.0%. It can be widely used in steering knuckles, control arms, automobile wheels, engine cylinder heads and other automotive parts. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a representative microstructure of the aluminum alloy after gravity casting of the present invention;
[0021] Figure 2 It is a representative post-tensile fracture microstructure of the aluminum alloy after gravity casting of the present invention;
[0022] Figure 3 It is a representative microstructure of the aluminum alloy T6 after heat treatment of the present invention;
[0023] Figure 4 This is the AlSiFeMnV quinary microstructure diagram in the aluminum alloy prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] The invention provides a renewable high-strength and tough heat-treatable aluminum alloy material, which is composed of the following materials: Cu 0.2%-0.6%, Si 7.5%-9.5%, Zn 0.1%-0.5%, Mn 0.1%-0.3%, Mg 0.25%-0.5%, Fe 0.2%-0.45%, Sr 0.010%-0.045%, V 0.015%-0.065%, Ga 0.0065%—0.085%, the balance is Al and impurities, of which the total impurity content is not more than 0.25%, 20≤(Si / (Ga+Mg)) mass fraction ratio≤34.5, (Fe+Mn) / V element mass fraction ratio is 6.5-23.5, renewable high-strength and tough heat-treatable strengthened aluminum alloy material is used in steering knuckles, control arms, automobile wheels and engine cylinder head parts. The tensile strength of the components of this aluminum alloy material is ≥350MPa, the yield strength is ≥250MPa, and the elongation after fracture is ≥7.0%.
[0027] Example 2
[0028] See also Figure 1-2 The present invention provides the following technical solution: a method for preparing a renewable high-strength and tough heat-treatable reinforced aluminum alloy material, the preparation method comprising the following steps:
[0029] S1. Prepare raw materials according to the formula of aluminum alloy materials, weigh corresponding percentages of each raw material, dry and preheat, heat melt and stir evenly to obtain alloy melt, specifically:
[0030] Add the recycled aluminum alloy ingot into the smelting furnace for melting. After it is completely melted, add pure metal or intermediate alloy of Cu, Mg, Zn, Si and Mn elements. After it is completely melted, add Al-V, Al-Sr and AlGa intermediate alloys. The drying preheating temperature is 250°C, the hot melting temperature is 800°C, and the stirring time is 10 minutes.
[0031] S2. Refining the alloy melt, introducing a protective gas into the alloy melt, wherein the protective gas is nitrogen or argon, the amount of the protective gas introduced is 3 L / min, RJ-01 refining agent is added, the refining time is 25 minutes, and the amount of the solid refining agent added is 0.4% of the melt mass;
[0032] The specific steps of degassing are to place the alloy melt along the flow channel into the degassing box, and the degassing box is equipped with a double-rotor rotary degasser for full-time online degassing. The rotor speed is set at 500r / min, the argon pressure is 0.4MPa, and the flow rate is 25L / min.
[0033] Specific steps of impurity removal: After online degassing, the alloy melt enters the filter box and is purified by the preheated ceramic filter plate. The ceramic filter plate can block large-sized impurities and adsorb small-sized impurities. The pore size of the filter plate is 25ppi.
[0034] S3, feeding the alloy melt that has been degassed and impurity-removed into a forming device for preparation and forming, wherein the forming device is low pressure, gravity or extrusion, to obtain an aluminum alloy component;
[0035] T6 heat treatment is carried out. The T6 heat treatment process is as follows: the solution temperature is 510°C, the holding time is 4 hours, water cooling is 3 minutes to 60°C, the artificial aging temperature is 160°C, the holding time is 7 hours, and the furnace is cooled to room temperature.
[0036] After the above smelting, the aluminum alloy composition and mass percentage are: Cu 0.5%, Si 8.0%, Zn 0.15%, Mn0.15%, Mg 0.35%, Fe 0.25%, Sr 0.025%, V 0.055%, Ga 0.025%, the balance is Al and impurities, wherein the total impurity content is not more than 0.25%, (Si / (Ga+Mg)) mass fraction ratio is 21.3, (Fe+Mn) / V element mass fraction ratio is 7.3, gravity casting, preparation of standard specimens for testing main mechanical properties are as follows: tensile strength 365MPa, yield strength 260MPa, elongation after fracture 7.5%, such as Figure 2 shown.
[0037] Example 3
[0038] The present invention provides the following technical solution: a method for preparing a renewable high-strength and tough heat-treatable strengthened aluminum alloy material, which is prepared according to the method in Example 2.
[0039] After the above smelting, the aluminum alloy composition and mass percentage are: Cu 0.25%, Si 8.8%, Zn 0.25%, Mn0.22%, Mg 0.25%, Fe 0.28%, Sr 0.028%, V 0.025%, Ga 0.0068%, the balance is Al and impurities, wherein the total impurity content is not more than 0.25%, (Si / (Ga+Mg)) mass fraction ratio is 34.3, (Fe+Mn) / V element mass fraction ratio is 20, gravity casting, standard specimens are prepared for testing, and the main mechanical properties are as follows: tensile strength 368MPa, yield strength 265MPa, elongation after fracture 7.8%, such as Figure 2 shown.
[0040] Example 4
[0041] The present invention provides the following technical solution: a method for preparing a renewable high-strength and tough heat-treatable strengthened aluminum alloy material, which is prepared according to the method in Example 2.
[0042] After the above smelting, the aluminum alloy composition and mass percentage are: Cu 0.3%, Si 8.5%, Zn 0.2%, Mn0.19%, Mg 0.28%, Fe 0.25%, Sr 0.025%, V 0.030%, Ga 0.084%, the balance is Al and impurities, wherein the total impurity content is not more than 0.25%, (Si / (Ga+Mg)) mass fraction ratio is 23.4, (Fe+Mn) / V element mass fraction ratio is 14.67, gravity casting, preparation of standard specimens for testing main mechanical properties are as follows: tensile strength 378MPa, yield strength 275MPa, elongation after fracture 7.6%, such as Figure 2 shown.
[0043] Comparative Example 1
[0044] The preparation was carried out according to the method in Example 2 without adding AlGa.
[0045] The alloy composition and mass percentage are: Cu 0.3%, Si 7.6%, Zn 0.22%, Mn 0.18%, Mg 0.48%, Fe 0.27%, Sr 0.025%, V 0.025%, the balance is Al and impurities, the total impurity content is not more than 0.25%,
[0046] After the above smelting and gravity casting, standard specimens were prepared and tested for the following main mechanical properties: tensile strength 348MPa, yield strength 245MPa, elongation after fracture 6.6%. Figure 2 shown.
[0047] Comparative Example 2
[0048] The preparation was carried out according to the method in Example 2.
[0049] The alloy composition and mass percentage are: Cu 0.31%, Si 7.7%, Zn 0.23%, Mn 0.25%, Mg0.47%, Fe 0.37%, Sr 0.025%, V 0.016%, Ga0.087%, the remainder is Al and impurities, of which the total impurity content is not more than 0.25%, the mass fraction ratio of (Si / (Ga+Mg)) is 13.8, and the mass fraction ratio of (Fe+Mn) / V elements is 38.75.
[0050] After the above smelting and gravity casting, standard specimens were prepared and tested for the following main mechanical properties: tensile strength 338MPa, yield strength 235MPa, elongation after fracture 5.8%. Figure 2 shown.
[0051] Comparative Example 3
[0052] The preparation was carried out according to the method in Example 2, and T5 heat treatment was performed, the artificial aging temperature was 180° C., the heat preservation time was 6 hours, and the furnace was cooled to room temperature.
[0053] The alloy composition and mass percentage are: Cu 0.36%, Si 8.5%, Zn 0.25%, Mn 0.23%, Mg0.37%, Fe 0.22%, Sr 0.025%, V 0.056%, Ga0.050%, the balance is Al and impurities, of which the total impurity content is not more than 0.25%, the mass fraction ratio of (Si / (Ga+Mg)) is 20.2, and the mass fraction ratio of (Fe+Mn) / V element is 8.0.
[0054] After the above smelting and gravity casting, standard specimens were prepared and tested for the following main mechanical properties: tensile strength 342MPa, yield strength 242MPa, elongation after fracture 5.5%. Figure 2 shown.
[0055] The metallographic structures of the samples prepared in Examples 2, 3 and 4 were observed under an electron microscope and were generally distributed in the same manner (select representative structures, see Appendix Figure 1 ), as can be seen from the figure, the introduction of AlV and AlGa master alloys can also make the distribution of intermetallic compounds more dispersed, the size of the dispersed matter is effectively limited, the segmentation effect on the grain boundary is weakened, and the pinning effect is significantly enhanced; in addition, considering the (Si / (Ga+Mg)) mass fraction ratio and the (Fe+Mn) / V element mass fraction ratio when designing elements, the grain size, the size of the precipitates, and the concentration gradient are significantly improved, and the combined effect of fine grain strengthening on strength and toughness is fully exerted.
[0056] From the cross-section microstructure (select representative structures, see Appendix Figure 2 ) It can also be seen that the dimples at the cross section are evenly distributed, with moderate density and relatively uniform size. Combined with the measured data, it can be determined that the material described in this application can meet the mechanical property requirements of the next generation of parts.
[0057] To further verify the mechanical performance advantages of the material described in this application over the prior art, the laboratory organized the following comparative tests.
[0058] The commonly used A356.2 and high-strength and toughness aluminum alloys of Example 1 of the present invention were used to prepare standard die-casting specimens using the same process: the main chemical composition and mechanical properties were tested, and the results shown in Table 2 were obtained:
[0059]
[0060] Table 1 Comparison of main chemical composition and mechanical properties of different aluminum alloys
[0061] It can be seen from Table 1 above that, under the same conditions, the aluminum alloy material designed in the present application has better mechanical properties after low-pressure casting, and its tensile strength and yield strength are significantly better than those of existing materials.
[0062] In order to verify whether the performance of the aluminum alloy prepared by the above preparation method meets the requirements, different batches of finished high-strength and toughness aluminum alloys were randomly selected, and their composition and mechanical properties (standard samples) were measured. The results shown in Table 2 were obtained:
[0063]
[0064] Table 2 Main components and mechanical properties of different batches of high-strength and toughness aluminum alloys
[0065] It can be seen from Table 3 that the aluminum alloy materials prepared according to the design principle and method of the present application have a tensile strength of ≥350 MPa, a yield strength of ≥250 MPa, and an elongation after fracture of ≥7.0%, which fully meets the requirements of the automotive field for light weight, high strength, and medium toughness of materials, and can be used for the manufacture of automotive steering knuckles, control arms, and swing arms, providing excellent materials for reducing the weight of parts and improving performance.
[0066] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0067] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A renewable high-strength and tough heat-treatable aluminum alloy material, characterized in that: It is composed of the following materials: Cu 0.2% - 0.6%, Si 7.5% - 9.5%, Zn 0.1% - 0.5%, Mn 0.1% - 0.3%, Mg 0.25% - 0.5%, Fe 0.2% - 0.45%, Sr 0.010% - 0.045%, V 0.015% - 0.065%, Ga 0.0065% - 0.085%, the balance is Al and impurities, of which the total impurity content is not more than 0.25%; 20≤(Si / (Ga+Mg)) mass fraction ratio≤34.5, (Fe+Mn) / V element mass fraction ratio is between 6.5-23.
5.
2. The renewable high-strength and tough heat-treatable aluminum alloy material according to claim 1, characterized in that: The aluminum alloy material has a tensile strength of ≥350MPa, a yield strength of ≥250MPa, and an elongation after fracture of ≥7.0%.
3. The method for preparing a renewable high-strength and tough heat-treatable aluminum alloy material according to any one of claims 1 to 2, characterized in that: This preparation method comprises the following steps: S1. Prepare raw materials according to the formula of aluminum alloy materials, weigh corresponding percentages of each raw material, dry and preheat, heat melt and stir evenly to obtain alloy melt; S2. Refining the alloy melt, degassing and removing impurities. After online degassing, the alloy melt enters the filter box and purifies the alloy melt through the preheated ceramic filter plate. The ceramic filter plate can block large-sized impurities and adsorb small-sized impurities. The pore size of the filter plate is 25-45ppi. S3. The alloy melt that has been degassed and impurity-removed is sent to a forming device for preparation and then formed. The forming device is low-pressure, gravity or extrusion to obtain an aluminum alloy component.
4. The method for preparing the renewable high-strength and high-toughness heat-treatable strengthened aluminum alloy material according to claim 3, characterized in that: The specific steps of the refining treatment in step S2 are: introducing a protective gas into the alloy melt, wherein the protective gas is nitrogen or argon, the amount of the protective gas introduced is 0.15-6 L / min, RJ-01 refining agent is added, the refining time is 15-30 minutes, and the amount of solid refining agent added is 0.2%-0.5% of the melt mass.
5. The method for preparing the renewable high-strength and high-toughness heat-treatable strengthened aluminum alloy material according to claim 3, characterized in that: The specific steps of degassing in step S2 are as follows: placing the alloy melt into a degassing box along the flow channel, and installing a double-rotor rotary degasser in the degassing box for full-line degassing. The rotor speed is set at 400-550r / min, the argon pressure is 0.2-0.4MPa, and the flow rate is 18-28L / min.
6. The method for preparing the renewable high-strength and high-toughness heat-treatable strengthened aluminum alloy material according to claim 3, characterized in that: After step S3 is completed, T6 heat treatment is performed. The T6 heat treatment process is as follows: the solution temperature is 510±10°C, the heat preservation time is 3-8 hours, water cooling is performed to below 60°C for 3 minutes, the artificial aging temperature is 160-185°C, the heat preservation time is 5-8 hours, and the furnace is cooled to room temperature.
7. The method for preparing the renewable high-strength and high-toughness heat-treatable strengthened aluminum alloy material according to claim 3, characterized in that: The specific steps of hot melting in step S1 are: adding the recycled aluminum alloy ingot into a smelting furnace for melting, and after it is completely melted, adding pure metals or intermediate alloys of Cu, Mg, Zn, Si and Mn elements, and after it is completely melted, adding AlV, AlSr and AlGa intermediate alloys.
8. The method for preparing the renewable high-strength and high-toughness heat-treatable strengthened aluminum alloy material according to claim 3, characterized in that: In the step S1, the drying preheating temperature is 100-450° C., the hot melting temperature is 730-800° C., and the stirring time is 5-15 minutes.
9. The use of the renewable high-strength and high-toughness heat-treatable reinforced aluminum alloy material according to any one of claims 1 to 8, characterized in that: Renewable high-strength and tough heat-treatable aluminum alloy materials are used in steering knuckles, control arms, automotive wheels and engine cylinder head components.