Ultrafine-grained cemented carbide for numerical control tools and preparation method thereof
By optimizing the ratio and process of matrix materials and additives of cemented carbides, the problem of low cutting efficiency of CNC tools at high cutting speeds is solved, and the cutting efficiency and strength of cemented carbides are significantly improved, and suitable for high-temperature conditions.
Patent Information
- Application Number
- CN202411166550.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The existing cemented carbide used in CNC tools has low cutting efficiency and low stability and poor strength and hardness under high cutting speed and high feed rate conditions, making it difficult to apply to CNC cutting tools, limiting the efficiency of the product.
WC powder, Co powder, Cr3C2 powder, TaC powder, VC powder as matrix material, and co-mixed by adding grain-adjusting refining agent and modified metamorphic liquid, combined with nanostront strontium titanate proton irradiation treatment, ultrasonic blending and The impregnation liquid is blended to optimize the grain structure and interface of the alloy, and optimize the performance through stirring, pressing and sintering processes.
The cutting efficiency stability and strength and hardness of CNC tools are significantly improved. The product shows excellent cutting performance at high cutting speeds, and the density and bending strength are significantly improved, which are suitable for high temperature conditions.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cemented carbide, and in particular to an ultrafine grain cemented carbide for numerical control tools and a preparation method thereof. Background Art
[0002] CNC tools are tools used for cutting processing in mechanical manufacturing, also known as cutting tools. In a broad sense, cutting tools include both cutting tools and grinding tools. At the same time, in addition to cutting blades, CNC tools also include accessories such as tool rods and tool holders. Cemented carbide, as the material basis of advanced cutting processing technology, is also an important research direction in the field of cutting processing.
[0003] With the improvement of cutting processing parameters, the efficiency of cemented carbide used in CNC cutting tools has deteriorated. Under the conditions of high cutting speed and high feed rate, the cutting efficiency stability of the product is low, and it is difficult to apply it to CNC cutting tools. In addition, the strength and hardness of the product are poor, which further limits the efficiency of the product. Summary of the invention
[0004] In view of the defects of the prior art, the purpose of the present invention is to provide an ultra-fine-grained cemented carbide for CNC tools and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0005] The present invention solves the technical problem by adopting the following technical solution:
[0006] The present invention provides an ultrafine-grained cemented carbide for numerical control tools, comprising the following raw materials in parts by weight:
[0007] WC powder (tungsten carbide powder) 45-55 parts, Co powder 10-15 parts, Cr 3 C 2 8~12 parts of powder, 5~7 parts of TaC powder, 2~3 parts of VC powder (vanadium carbide powder); the cemented carbide also includes 4~7 parts of grain refiner and 20~25 parts of modified liquid;
[0008] The preparation method of the grain refiner is as follows:
[0009] S01: The nano-strontium titanate is first subjected to proton irradiation treatment, the irradiation power is 350-400W, the irradiation is carried out for 20-30 minutes, and the irradiation is completed to obtain irradiated nano-strontium titanate;
[0010] The irradiated nano-strontium titanate was thermally modified at 150-170°C for 10-15 min, then cooled to 55°C at a rate of 2-5°C / min and kept warm;
[0011] S02: VN powder (vanadium nitride powder), sodium dodecyl sulfate solution and carboxymethyl cellulose are mixed in a weight ratio of 3: (5-7): 1 to obtain a VN regulating solution;
[0012] S03: adding 3-5 parts of insulated nano-strontium titanate and 1-3 parts of silane coupling agent KH560 to 5-8 parts of chitosan solution, and then adding 1-2 parts of nano-silica sol to blend and ultrasonically treat, and the ultrasonic treatment is terminated to obtain a nano-strontium titanate agent;
[0013] S04: Mix the nano strontium titanate agent and VN regulating liquid in a weight ratio of 5:3 and perform ball milling at a ball milling speed of 1000-1500 r / min for 2 hours. After the ball milling is completed, wash with water and dry to obtain a grain refiner.
[0014] Preferably, WC powder, Co powder, Cr 3 C 2 The particle sizes of TaC powder, VC powder and MgO powder are all 0.1~0.3µm.
[0015] Preferably, the mass fraction of the sodium dodecyl sulfate solution is 4-7%; the mass fraction of the chitosan solution is 2-5%; the ultrasonic power of the blended ultrasonic treatment in SO3 is 400-500W, and the ultrasonic time is 20-30min.
[0016] Preferably, the preparation method of the modified liquid is:
[0017] S101: thermally conditioning the graphene. The specific treatment method is as follows:
[0018] The graphene was first heat treated at 155-165°C for 5-10 min, then the temperature was reduced to 55°C at a rate of 2-5°C / min and kept warm;
[0019] The heat-insulated graphene is immersed in an impregnation solution that is 3 to 5 times the total amount of the heat-insulated graphene. After the impregnation is completed, the impregnation is performed by suction filtration and drying to obtain an impregnated graphene agent;
[0020] The impregnated graphene agent is then heated to 125-130°C at a rate of 1-3°C / min, kept at this temperature for 5-10 minutes, and finally air-cooled to room temperature;
[0021] S102: 4 to 7 parts of heat-treated graphene, 2 to 5 parts of yttrium nitrate solution, 3 to 6 parts of sodium alginate solution and 1 to 2 parts of silane coupling agent KH550 are mixed to obtain a modified liquid.
[0022] Preferably, the mass fraction of the yttrium nitrate solution is 2-5%; the mass fraction of the sodium alginate solution is 4-7%; the immersion power of the immersion treatment is 450-500 W, and the immersion time is 20-30 min.
[0023] Preferably, the preparation method of the impregnation solution is:
[0024] 1-3 parts of stearic acid and 3-5 parts of nano-silicon dioxide are added to 5-8 parts of 5-7% sodium lignin sulfonate solution, and then 2-4 parts of lanthanum nitrate solution and 2-5 parts of scandium oxide are added, and the mixture is ball-milled at a speed of 1000-1500 r / min for 2 hours to obtain an impregnation solution.
[0025] Preferably, the mass fraction of the lanthanum nitrate solution is 2-5%.
[0026] The present invention also provides a method for preparing ultrafine-grained cemented carbide for numerical control tools, comprising the following steps:
[0027] Weigh the raw materials according to weight; mix WC powder, Co powder, Cr 3 C 2 The powder, TaC powder, VC powder and grain refiner are first stirred and mixed thoroughly, and then stirred and modified with the modified liquid. After the stirring is completed, the mixture is dried and then pressed into shape. The pressing pressure is 10-15 MPa. The pressing is performed for 20 minutes. After the pressing is completed, the mixture is sintered. After the sintering is completed, the ultrafine-grained cemented carbide of the present invention is obtained.
[0028] Preferably, the stirring speed of the stirring modification treatment is 450-550 r / min, the stirring temperature is 50-55° C., and the stirring time is 1-2 h; the sintering temperature of the sintering treatment is 1440-1450° C., and the sintering time is 2 h.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1. The ultra-fine grain cemented carbide of the CNC tool of the present invention is made of WC powder, Co powder, Cr 3 C 2 Powder, TaC powder and VC powder are used as the matrix materials. The raw materials between the matrix materials are blended and adjusted with each other, and the grain refiner and modified liquid are added to coordinate and enhance the effect. At the same time, the alloy preparation adopts the method of first mixing, then stirring modification, pressing and finally sintering. Through the coherent process, the performance of the product is optimized. The obtained cemented carbide product has excellent cutting efficiency and stability under the conditions of high cutting speed and high feed rate, and the strength and hardness of the product are remarkable.
[0031] 2. The grain refinement agent adopts nano-strontium titanate to be treated with proton irradiation to optimize the activity efficiency of nano-strontium titanate, and then undergoes thermal improvement at 150-170°C for 10-15 minutes, and then cools to 55°C at a rate of 2-5°C / min to further optimize its activity. At the same time, silane coupling agent KH560, chitosan solution and nano-silica sol are blended and ultrasonically treated, and silane coupling agent KH560 is added to 5-8 parts of chitosan solution, and then 1-2 parts of nano-silica sol are added and ultrasonically treated to obtain VN regulating solution. The nano-strontium titanate agent and VN regulating solution are mutually ball-milled to further enhance the interface between nano-strontium titanate and the system, and the VN system is combined to inhibit grain growth and refine grains. On the other hand, the interaction between the raw materials of the system is coordinated and improved, the system bonding force is enhanced, and the performance effect of the product is coordinated and improved;
[0032] 3. The modified liquid uses graphene to be heat-treated at 155-165°C for 5-10 minutes, and then the temperature is reduced to 55°C at a rate of 2-5°C / min to optimize the activity of graphene. Then, the graphene is impregnated with an impregnation liquid. The impregnation liquid uses nano-silicon dioxide and scandium oxide as the matrix material, and sodium lignin sulfonate solution, lanthanum nitrate solution and stearic acid are coordinated and matched. Through the coordination and coordination between the raw materials, the performance of the system product is improved; the graphene sheet structure is distributed in the system, and the raw materials in the impregnation liquid are improved by the coordination and impregnation. Effect, further enhance the performance of the product, and then heat up to 125~130℃ at a rate of 1~3℃ / min, keep warm for 5~10min, and finally air cool to room temperature, further optimize the activity efficiency of the impregnated graphene agent system, so as to better improve the system product, and then use yttrium nitrate solution, sodium alginate solution and silane coupling agent KH550 to fully blend with the heat-treated graphene, and coordinate and improve the alloy raw material system through the modified metamorphic liquid, optimize the interface effect between the raw materials and enhance the bonding force between the raw materials, and further enhance the performance of the product. DETAILED DESCRIPTION
[0033] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The ultrafine-grained cemented carbide for a numerical control tool of the present embodiment comprises the following raw materials in parts by weight:
[0035] WC powder 45-55 parts, Co powder 10-15 parts, Cr 3 C2 Powder 8-12 parts, TaC powder 5-7 parts, VC powder 2-3 parts; the cemented carbide also includes 4-7 parts of grain refiner and modified liquid 20-25 parts.
[0036] In this embodiment, WC powder, Co powder, Cr 3 C 2 The particle sizes of TaC powder, VC powder and MgO powder are all 0.1~0.3µm.
[0037] The preparation method of the grain refiner of this embodiment is as follows:
[0038] S01: The nano-strontium titanate is first subjected to proton irradiation treatment, the irradiation power is 350-400W, the irradiation is carried out for 20-30 minutes, and the irradiation is completed to obtain irradiated nano-strontium titanate;
[0039] The irradiated nano-strontium titanate was thermally modified at 150-170°C for 10-15 min, then cooled to 55°C at a rate of 2-5°C / min and kept warm;
[0040] S02: VN powder, sodium dodecyl sulfate solution and carboxymethyl cellulose are mixed in a weight ratio of 3: (5-7): 1 to obtain a VN regulating solution;
[0041] S03: adding 3-5 parts of insulated nano-strontium titanate and 1-3 parts of silane coupling agent KH560 to 5-8 parts of chitosan solution, and then adding 1-2 parts of nano-silica sol to blend and ultrasonically treat, and the ultrasonic treatment is terminated to obtain a nano-strontium titanate agent;
[0042] S04: Mix the nano strontium titanate agent and VN regulating liquid in a weight ratio of 5:3 and perform ball milling at a ball milling speed of 1000-1500 r / min for 2 hours. After the ball milling is completed, wash with water and dry to obtain a grain refiner.
[0043] The mass fraction of the sodium dodecyl sulfate solution in this embodiment is 4-7%; the mass fraction of the chitosan solution is 2-5%; the ultrasonic power of the co-mixed ultrasonic treatment in SO3 is 400-500W, and the ultrasonic time is 20-30min.
[0044] The preparation method of the modified deteriorated liquid of the present embodiment is:
[0045] S101: thermally conditioning the graphene. The specific treatment method is as follows:
[0046] The graphene was first heat treated at 155-165°C for 5-10 min, then the temperature was reduced to 55°C at a rate of 2-5°C / min and kept warm;
[0047] The heat-insulated graphene is immersed in an impregnation solution that is 3 to 5 times the total amount of the heat-insulated graphene. After the impregnation is completed, the impregnation is performed by suction filtration and drying to obtain an impregnated graphene agent;
[0048] The impregnated graphene agent is then heated to 125-130°C at a rate of 1-3°C / min, kept at this temperature for 5-10 minutes, and finally air-cooled to room temperature;
[0049] S102: 4 to 7 parts of heat-treated graphene, 2 to 5 parts of yttrium nitrate solution, 3 to 6 parts of sodium alginate solution and 1 to 2 parts of silane coupling agent KH550 are mixed to obtain a modified liquid.
[0050] Preferably, the mass fraction of the yttrium nitrate solution is 2-5%; the mass fraction of the sodium alginate solution is 4-7%; the immersion power of the immersion treatment is 450-500 W, and the immersion time is 20-30 min.
[0051] The preparation method of the impregnation liquid of this embodiment is:
[0052] 1-3 parts of stearic acid and 3-5 parts of nano-silicon dioxide are added to 5-8 parts of 5-7% sodium lignin sulfonate solution, and then 2-4 parts of lanthanum nitrate solution and 2-5 parts of scandium oxide are added, and the mixture is ball-milled at a speed of 1000-1500 r / min for 2 hours to obtain an impregnation solution.
[0053] The mass fraction of the lanthanum nitrate solution of the present embodiment is 2-5%.
[0054] A method for preparing an ultrafine-grained cemented carbide for a numerical control tool in this embodiment comprises the following steps:
[0055] Weigh the raw materials according to weight; mix WC powder, Co powder, Cr 3 C 2 The powder, TaC powder, VC powder and grain refiner are first stirred and mixed thoroughly, and then stirred and modified with the modified liquid. After the stirring is completed, the mixture is dried and then pressed into shape. The pressing pressure is 10-15 MPa. The pressing is performed for 20 minutes. After the pressing is completed, the mixture is sintered. After the sintering is completed, the ultrafine-grained cemented carbide of the present invention is obtained.
[0056] The stirring speed of the stirring modification treatment in this embodiment is 450~550r / min, the stirring temperature is 50~55°C, and the stirring time is 1~2h; the sintering temperature of the sintering treatment is 1440~1450°C, and the sintering time is 2h.
[0057] Example 1.
[0058] The ultrafine-grained cemented carbide for a numerical control tool of the present embodiment comprises the following raw materials in parts by weight:
[0059] WC powder 45 parts, Co powder 10 parts, Cr 3 C 2 8 parts of powder, 5 parts of TaC powder, and 2 parts of VC powder; the cemented carbide also includes 4 parts of grain refiner and 20 parts of modified liquid.
[0060] In this embodiment, WC powder, Co powder, Cr 3 C 2 The particle size of TaC powder, VC powder and MgO powder is 0.1µm.
[0061] The preparation method of the grain refiner of this embodiment is as follows:
[0062] S01: treating the nano-strontium titanate with protons at a power of 350W for 20 minutes, and obtaining irradiated nano-strontium titanate after the irradiation is completed;
[0063] The irradiated nano-strontium titanate was thermally modified at 150°C for 10 min, then cooled to 55°C at a rate of 2°C / min and kept warm;
[0064] S02: VN powder, sodium dodecyl sulfate solution and carboxymethyl cellulose are mixed in a weight ratio of 3:5:1 to obtain a VN regulating solution;
[0065] S03: adding 3 parts of insulated nano-strontium titanate and 1 part of silane coupling agent KH560 to 5 parts of chitosan solution, and then adding 1 part of nano-silica sol to blend and ultrasonically treat, and the ultrasonic treatment is terminated to obtain a nano-strontium titanate agent;
[0066] S04: Mix the nano-strontium titanate agent and VN regulating liquid in a weight ratio of 5:3 and perform ball milling at a ball milling speed of 1000 r / min for 2 hours. After the ball milling is completed, wash with water and dry to obtain a grain refiner.
[0067] The mass fraction of the sodium dodecyl sulfate solution in this embodiment is 4%; the mass fraction of the chitosan solution is 2%; the ultrasonic power of the blended ultrasonic treatment in SO3 is 400W, and the ultrasonic time is 20min.
[0068] The preparation method of the modified deteriorated liquid of the present embodiment is:
[0069] S101: thermally conditioning the graphene. The specific treatment method is as follows:
[0070] The graphene was first heat treated at 155°C for 5 min, then cooled to 55°C at a rate of 2°C / min and kept warm;
[0071] The insulated graphene is immersed in an impregnation solution which is 3 times the total amount of the insulated graphene, and after the insulated graphene is immersed, the impregnation solution is filtered and dried to obtain an immersed graphene agent;
[0072] The impregnated graphene agent was then heated to 125°C at a rate of 1°C / min, kept at this temperature for 5 min, and finally air-cooled to room temperature;
[0073] S102: 4 parts of heat-treated graphene, 2 parts of yttrium nitrate solution, 3 parts of sodium alginate solution and 1 part of silane coupling agent KH550 are mixed to obtain a modified liquid.
[0074] The mass fraction of the yttrium nitrate solution is 2%; the mass fraction of the sodium alginate solution is 4%; the immersion power of the immersion treatment is 450W, and the immersion time is 20 minutes.
[0075] The preparation method of the impregnation liquid of this embodiment is:
[0076] 1 part of stearic acid and 3 parts of nano-silicon dioxide were added to 5 parts of 5% by mass sodium lignin sulfonate solution, followed by adding 2 parts of lanthanum nitrate solution and 2 parts of scandium oxide, and the mixture was ball-milled at a speed of 1000 r / min for 2 hours to obtain an impregnation solution.
[0077] The mass fraction of the lanthanum nitrate solution of the present embodiment is 2%.
[0078] A method for preparing an ultrafine-grained cemented carbide for a numerical control tool in this embodiment comprises the following steps:
[0079] Weigh the raw materials according to weight; mix WC powder, Co powder, Cr 3 C 2 The powder, TaC powder, VC powder and grain refiner are first stirred and mixed thoroughly, and then stirred and modified with the modified liquid. After the stirring is completed, the mixture is dried and then pressed into shape. The pressing pressure is 10 MPa and the pressing is performed for 20 minutes. After the pressing is completed, the mixture is sintered and sintered to obtain the ultrafine-grained cemented carbide of the present invention.
[0080] The stirring speed of the stirring modification treatment in this embodiment is 450 r / min, the stirring temperature is 50° C., and the stirring time is 1 h; the sintering temperature of the sintering treatment is 1440° C., and the sintering time is 2 h.
[0081] Example 2.
[0082] The ultrafine-grained cemented carbide for a numerical control tool of the present embodiment comprises the following raw materials in parts by weight:
[0083] WC powder 55 parts, Co powder 15 parts, Cr 3 C 2 12 parts of powder, 7 parts of TaC powder, and 3 parts of VC powder; the cemented carbide also includes 7 parts of grain refiner and 25 parts of modified liquid.
[0084] In this embodiment, WC powder, Co powder, Cr 3 C 2 The particle size of TaC powder, VC powder and MgO powder is 0.3µm.
[0085] The preparation method of the grain refiner of this embodiment is as follows:
[0086] S01: treating the nano-strontium titanate with protons at a power of 400 W for 30 minutes, and obtaining irradiated nano-strontium titanate after the irradiation is completed;
[0087] The irradiated nano-strontium titanate was thermally modified at 170°C for 15 min, then cooled to 55°C at a rate of 5°C / min and kept warm;
[0088] S02: VN powder, sodium dodecyl sulfate solution and carboxymethyl cellulose are mixed in a weight ratio of 3:7:1 to obtain a VN regulating solution;
[0089] S03: adding 5 parts of insulated nano-strontium titanate and 3 parts of silane coupling agent KH560 to 8 parts of chitosan solution, and then adding 2 parts of nano-silica sol to blend and ultrasonically treat, and the ultrasonic treatment is terminated to obtain a nano-strontium titanate agent;
[0090] S04: Mix the nano-strontium titanate agent and VN regulating liquid in a weight ratio of 5:3 and perform ball milling at a ball milling speed of 1500r / min for 2h. After the ball milling is completed, wash with water and dry to obtain a grain refiner.
[0091] The mass fraction of the sodium dodecyl sulfate solution in this embodiment is 7%; the mass fraction of the chitosan solution is 5%; the ultrasonic power of the blended ultrasonic treatment in S03 is 500W, and the ultrasonic time is 30min.
[0092] The preparation method of the modified deteriorated liquid of the present embodiment is:
[0093] S101: thermally conditioning the graphene. The specific treatment method is as follows:
[0094] The graphene was first heat treated at 165°C for 10 min, then cooled to 55°C at a rate of 5°C / min and kept warm;
[0095] The insulated graphene is immersed in an impregnation solution that is 5 times the total amount of the insulated graphene, and after the impregnation is completed, the impregnation is filtered and dried to obtain an impregnated graphene agent;
[0096] The impregnated graphene agent was then heated to 130°C at a rate of 3°C / min, kept at this temperature for 10 min, and finally air-cooled to room temperature;
[0097] S102: 7 parts of heat-treated graphene, 5 parts of yttrium nitrate solution, 6 parts of sodium alginate solution and 2 parts of silane coupling agent KH550 are mixed to obtain a modified liquid.
[0098] The mass fraction of the yttrium nitrate solution is 5%; the mass fraction of the sodium alginate solution is 7%; the immersion power of the immersion treatment is 500W, and the immersion time is 30 minutes.
[0099] The preparation method of the impregnation liquid of this embodiment is:
[0100] 3 parts of stearic acid and 5 parts of nano-silicon dioxide were added to 8 parts of 7% sodium lignin sulfonate solution, followed by adding 4 parts of lanthanum nitrate solution and 5 parts of scandium oxide, and the mixture was ball-milled at a speed of 1500 r / min for 2 hours to obtain an impregnation solution.
[0101] The mass fraction of the lanthanum nitrate solution in this embodiment is 5%.
[0102] A method for preparing an ultrafine-grained cemented carbide for a numerical control tool in this embodiment comprises the following steps:
[0103] Weigh the raw materials according to weight; mix WC powder, Co powder, Cr 3 C 2 The powder, TaC powder, VC powder and grain refiner are first stirred and mixed thoroughly, and then stirred and modified with the modified liquid. After the stirring is completed, the mixture is dried and then pressed into shape. The pressing pressure is 15 MPa and the pressing is performed for 20 minutes. After the pressing is completed, the mixture is sintered and the ultrafine-grained cemented carbide of the present invention is obtained.
[0104] The stirring speed of the stirring modification treatment in this embodiment is 550 r / min, the stirring temperature is 55° C., and the stirring time is 2 h; the sintering temperature of the sintering treatment is 1450° C., and the sintering time is 2 h.
[0105] Example 3.
[0106] The ultrafine-grained cemented carbide for a numerical control tool of the present embodiment comprises the following raw materials in parts by weight:
[0107] WC powder 50 parts, Co powder 12.5 parts, Cr 3 C 2 10 parts of powder, 6 parts of TaC powder, and 2.5 parts of VC powder; the cemented carbide also includes 5.5 parts of grain refiner and 22.5 parts of modified liquid.
[0108] In this embodiment, WC powder, Co powder, Cr 3 C 2 The particle size of TaC powder, VC powder and MgO powder is 0.2µm.
[0109] The preparation method of the grain refiner of this embodiment is as follows:
[0110] S01: treating the nano-strontium titanate with protons at a power of 375W for 25 minutes, and obtaining irradiated nano-strontium titanate after the irradiation is completed;
[0111] The irradiated nano-strontium titanate was thermally modified at 160°C for 12.5 min, then cooled to 55°C at a rate of 3.5°C / min and kept warm;
[0112] S02: VN powder, sodium dodecyl sulfate solution and carboxymethyl cellulose are mixed in a weight ratio of 3:6:1 to obtain a VN regulating solution;
[0113] S03: adding 4 parts of insulated nano-strontium titanate and 2 parts of silane coupling agent KH560 to 6.5 parts of chitosan solution, and then adding 1.5 parts of nano-silica sol to blend and ultrasonically treat, and the ultrasonic treatment is terminated to obtain a nano-strontium titanate agent;
[0114] S04: Mix the nano-strontium titanate agent and VN regulating liquid in a weight ratio of 5:3, and perform ball milling at a ball milling speed of 1250r / min for 2h. After the ball milling is completed, wash with water and dry to obtain a grain refiner.
[0115] The mass fraction of the sodium dodecyl sulfate solution in this embodiment is 5.5%; the mass fraction of the chitosan solution is 3.5%; the ultrasonic power of the co-mixed ultrasonic treatment in SO3 is 450W, and the ultrasonic time is 25min.
[0116] The preparation method of the modified deteriorated liquid of the present embodiment is:
[0117] S101: thermally conditioning the graphene. The specific treatment method is as follows:
[0118] The graphene was first heat treated at 160°C for 7.5 min, then cooled to 55°C at a rate of 3.5°C / min and kept warm;
[0119] The insulated graphene is immersed in an impregnation solution of 4 times the total amount of the insulated graphene, and after the insulated is finished, the impregnation is filtered and dried to obtain an impregnated graphene agent;
[0120] The impregnated graphene agent was then heated to 127.5°C at a rate of 2°C / min, kept at this temperature for 7.5 min, and finally air-cooled to room temperature;
[0121] S102: 5.5 parts of heat-treated graphene, 3.5 parts of yttrium nitrate solution, 4.5 parts of sodium alginate solution and 1.5 parts of silane coupling agent KH550 are mixed to obtain a modified liquid.
[0122] The mass fraction of the yttrium nitrate solution is 3.5%; the mass fraction of the sodium alginate solution is 5.5%; the immersion power of the immersion treatment is 475W, and the immersion time is 25 minutes.
[0123] The preparation method of the impregnation liquid of this embodiment is:
[0124] 2 parts of stearic acid and 4 parts of nano-silicon dioxide were added to 6.5 parts of 6% sodium lignin sulfonate solution, followed by 3 parts of lanthanum nitrate solution and 3.5 parts of scandium oxide. The mixture was ball-milled at a speed of 1250 r / min for 2 hours to obtain an impregnation solution.
[0125] The mass fraction of the lanthanum nitrate solution in this embodiment is 3.5%.
[0126] A method for preparing an ultrafine-grained cemented carbide for a numerical control tool in this embodiment comprises the following steps:
[0127] Weigh the raw materials according to weight; mix WC powder, Co powder, Cr 3 C 2 The powder, TaC powder, VC powder and grain refiner are first stirred and mixed thoroughly, and then stirred and modified with the modified liquid. After the stirring is completed, they are dried and then pressed into shape. The pressing pressure is 12.5MPa. The pressing is performed for 20 minutes. After the pressing is completed, the powder is sintered. After the sintering is completed, the ultrafine-grained cemented carbide of the present invention is obtained.
[0128] The stirring speed of the stirring modification treatment in this embodiment is 500 r / min, the stirring temperature is 52.5° C., and the stirring time is 1.5 h; the sintering temperature of the sintering treatment is 1445° C., and the sintering time is 2 h.
[0129] Comparative Example 1.
[0130] The difference from Example 3 is that no grain refiner is added.
[0131] Comparative Example 2.
[0132] The difference from Example 3 is that the S01 step is not used in the preparation of the grain refiner.
[0133] Comparative Example 3.
[0134] The difference from Example 3 is that no VN regulating liquid is added in the preparation of the grain refiner.
[0135] Comparative Example 4.
[0136] The difference from Example 3 is that no nano strontium titanate agent is added in the preparation of the grain refiner.
[0137] Comparative Example 5.
[0138] The difference from Example 3 is that no heat-insulated nano-strontium titanate is added in the preparation of the nano-strontium titanate agent.
[0139] Comparative Example 6.
[0140] The difference from Example 3 is that no modified deterioration liquid is added.
[0141] Comparative Example 7.
[0142] The difference from Example 3 is that no thermally treated graphene is added in the preparation of the modified liquid.
[0143] Comparative Example 8.
[0144] The difference from Example 3 is that no yttrium nitrate solution and silane coupling agent KH550 are added in the preparation of the modified deterioration liquid.
[0145] Comparative Example 9.
[0146] The difference from Example 3 is that no immersion liquid treatment is used in the preparation of the thermally treated graphene.
[0147] Comparative Example 10.
[0148] The difference from Example 3 is that in the preparation of the heat-treated graphene, the graphene was not first heat-treated at 160°C for 7.5 minutes, then cooled to 55°C at a rate of 3.5°C / min and kept warm; and the impregnated graphene agent was not heated to 127.5°C at a rate of 2°C / min, kept warm for 7.5 minutes, and finally air-cooled to room temperature.
[0149] The products of Examples 1 to 3 and Comparative Examples 1 to 10 were subjected to performance tests, and the test results are as follows:
[0150]
[0151] It can be seen from Comparative Examples 1 to 10 and Examples 1 to 3 that;
[0152] The product of Example 3 has excellent density and excellent bending strength performance, and the product still has excellent hardness under high temperature conditions. The product can achieve coordinated improvements in density, strength and hardness.
[0153] Based on the above test, the present invention also tests the cutting performance. The processed material is 42CrMo, the cutting depth is controlled at 2.0mm, the feed rate is 0.3mm, and the cutting speed is changed to explore the cutting time of the product. The specific test is as follows:
[0154]
[0155] From the above performance tests, it can be seen that the present invention has excellent cutting efficiency and cutting efficiency stability on the basis of coordinated improvement of density, strength and hardness. The product has excellent cutting time at cutting speeds of 350m / min and 450m / min, and the cutting efficiency of the product is remarkable.
[0156] From Comparative Examples 1-10 and Example 3, it can be seen that when the product does not add a grain refiner or a modified liquid, the performance of the product deteriorates significantly. When the two are used in combination, the performance effect of the product is most significant.
[0157] The performance of the products tended to deteriorate when the S01 step was not used in the preparation of the grain-tuning and refining agent, the VN regulating liquid was not added in the preparation of the grain-tuning and refining agent, the nano-strontium titanate agent was not added in the preparation of the nano-strontium titanate agent, and the nano-strontium titanate agent was not added in the preparation of the nano-strontium titanate agent. The performance of the product was the most significant when the VN regulating liquid obtained by the specific method of the present invention and the nano-strontium titanate agent were used to prepare the grain-tuning and refining agent.
[0158] In the preparation of the modified deterioration liquid, no heat-treated graphene, no yttrium nitrate solution and silane coupling agent KH550 were added, and the performance of the product showed a trend of deterioration to varying degrees. At the same time, no immersion liquid treatment was used in the preparation of the heat-treated graphene, and the performance of the product showed a large change trend. In addition, the conditions for preparing the heat-treated graphene were different, and the product also showed a trend of deterioration. Only the modified deterioration liquid obtained by the method of the present invention has the most significant product performance effect, and other methods are not as obvious as the effect of the present invention.
[0159] The present invention further explores the product performance through the preparation of the impregnation liquid;
[0160] The preparation method of the impregnation solution is:
[0161] 2 parts of stearic acid and 4 parts of nano-silicon dioxide were added to 6.5 parts of 6% sodium lignin sulfonate solution, followed by 3 parts of lanthanum nitrate solution and 3.5 parts of scandium oxide. The mixture was ball-milled at a speed of 1250 r / min for 2 hours to obtain an impregnation solution.
[0162] Experimental example 1.
[0163] The only difference from Example 3 is that no nano-silicon dioxide is added in the preparation of the impregnation solution.
[0164] Experimental example 2.
[0165] The only difference from Example 3 is that no lanthanum nitrate solution is added during the preparation of the impregnation solution.
[0166] Experimental Example 3.
[0167] The only difference from Example 3 is that scandium oxide is not added in the preparation of the impregnation solution.
[0168] Experimental Example 4.
[0169] The only difference from Example 3 is that stearic acid and sodium lignin sulfonate solution are not added in the preparation of the impregnation solution, and deionized water is used instead.
[0170] The product performance test results of Experimental Examples 1-4 are as follows:
[0171]
[0172] It can be seen from Experimental Examples 1-4 that when nano-silicon dioxide is not added in the preparation of the impregnation solution, the performance of the product changes. In the preparation of the impregnation solution, the performance deterioration is most obvious, followed by the fact that scandium oxide is not added. At the same time, when lanthanum nitrate solution, stearic acid and sodium lignin sulfonate solution are not added in the preparation of the impregnation solution and deionized water is used instead, the performance of the product tends to deteriorate. The performance of the product tends to deteriorate to varying degrees when the impregnation solutions are obtained by different methods. Only the impregnation solution obtained by the specific method of the present invention has the most significant product performance effect.
[0173] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0174] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. An ultrafine-grained cemented carbide for CNC tools, characterized in that: The following raw materials by weight: 45-55 parts of WC powder, 10-15 parts of Co powder, 8-12 parts of Cr3C2 powder, 5-7 parts of TaC powder, 2-3 parts of VC powder, 4-7 parts of grain refiner and 20-25 parts of modified liquid; The preparation method of the grain refiner is as follows: S01: The nano-strontium titanate is first subjected to proton irradiation treatment, the irradiation power is 350-400W, the irradiation is carried out for 20-30 minutes, and the irradiation is completed to obtain irradiated nano-strontium titanate; The irradiated nano-strontium titanate was thermally modified at 150-170°C for 10-15 min, then cooled to 55°C at a rate of 2-5°C / min and kept warm; S02: VN powder, sodium dodecyl sulfate solution and carboxymethyl cellulose are mixed in a weight ratio of 3: (5-7): 1 to obtain a VN regulating solution; S03: adding 3-5 parts of insulated nano-strontium titanate and 1-3 parts of silane coupling agent KH560 to 5-8 parts of chitosan solution, and then adding 1-2 parts of nano-silica sol to blend and ultrasonically treat, and the ultrasonic treatment is terminated to obtain a nano-strontium titanate agent; S04: Mix the nano-strontium titanate agent and the VN regulating liquid in a weight ratio of 5:3 and perform ball milling at a ball milling speed of 1000-1500 r / min for 2 h. After the ball milling is completed, wash with water and dry to obtain a grain refiner; The preparation method of the modified liquid is: S101: thermally conditioning the graphene. The specific treatment method is as follows: The graphene was first heat treated at 155-165°C for 5-10 min, then the temperature was reduced to 55°C at a rate of 2-5°C / min and kept warm; The heat-insulated graphene is immersed in an impregnation solution that is 3 to 5 times the total amount of the heat-insulated graphene. After the impregnation is completed, the impregnation is performed by suction filtration and drying to obtain an impregnated graphene agent; The impregnated graphene agent is then heated to 125-130°C at a rate of 1-3°C / min, kept at this temperature for 5-10 minutes, and finally air-cooled to room temperature; S102: 4-7 parts of heat-treated graphene, 2-5 parts of yttrium nitrate solution, 3-6 parts of sodium alginate solution and 1-2 parts of silane coupling agent KH550 are mixed to obtain a modified liquid; The preparation method of the impregnation solution is: 1-3 parts of stearic acid and 3-5 parts of nano-silicon dioxide are added to 5-8 parts of 5-7% sodium lignin sulfonate solution, and then 2-4 parts of lanthanum nitrate solution and 2-5 parts of scandium oxide are added, and the mixture is ball-milled at a speed of 1000-1500 r / min for 2 hours to obtain an impregnation solution.
2. The ultrafine-grained cemented carbide for CNC tools according to claim 1, characterized in that: The particle sizes of WC powder, Co powder, Cr3C2 powder, TaC powder and VC powder are all 0.1~0.3µm.
3. The ultrafine-grained cemented carbide for CNC tools according to claim 1, characterized in that: The mass fraction of the sodium dodecyl sulfate solution is 4-7%; the mass fraction of the chitosan solution is 2-5%; the ultrasonic power of the mixed ultrasonic treatment in S03 is 400-500W, and the ultrasonic time is 20-30min.
4. The ultrafine-grained cemented carbide for CNC tools according to claim 1, characterized in that: The mass fraction of the yttrium nitrate solution is 2-5%; the mass fraction of the sodium alginate solution is 4-7%; the immersion power of the immersion treatment is 450-500W, and the immersion time is 20-30min.
5. The ultrafine-grained cemented carbide for CNC tools according to claim 1, characterized in that: The mass fraction of the lanthanum nitrate solution is 2-5%.
6. A method for preparing ultrafine-grained cemented carbide for numerical control tools according to any one of claims 1 to 5, characterized in that: The following steps are involved: Weigh the raw materials according to weight; stir and mix WC powder, Co powder, Cr3C2 powder, TaC powder, VC powder and grain refiner thoroughly, and then stir and modify them with the modified liquid. After stirring, dry, and then press into shape. The pressing pressure is 10-15MPa. Press for 20 minutes. After pressing, sinter and sinter to obtain ultrafine-grained cemented carbide.
7. The method for preparing ultrafine-grained cemented carbide for numerical control tools according to claim 6, characterized in that: The stirring speed of the stirring modification treatment is 450-550 r / min, the stirring temperature is 50-55° C., and the stirring time is 1-2 h; the sintering temperature of the sintering treatment is 1440-1450° C., and the sintering time is 2 h.
Citation Information
Cited By
WC-based hard alloy of high-entropy alloy binding phase and preparation method of WC-based hard alloy
CN120443021A