Liquid crystal alignment agent and liquid crystal alignment film and liquid crystal display element using the same
By introducing a liquid crystal alignment film of a specific structural unit A-1 into the liquid crystal alignment agent, the flickering and afterimage problems caused by DC bias under low frequency driving of the liquid crystal display element are solved, and adhesion is enhanced through covalent bonds with the sealant. Improves the high temperature stability and display quality of LCD display components.
Patent Information
- Application Number
- CN202411204069.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2024-06-07
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-30
AI Technical Summary
Under low-frequency driving conditions, liquid crystal display elements are prone to flickering and afterimage problems caused by DC bias, and poor sealing under narrow frame design leads to external impurities entering and affecting the display quality.
A liquid crystal alignment agent is adopted, including a polyimide precursor and its imidized product, and has a specific structural unit A-1, which can be arranged spatially with other monomer molecules after film formation, thereby improving DC bias charge release The rate and covalent bond with the sealant at high temperature enhance adhesion and suppress flicker and afterimage.
The high temperature stability of the liquid crystal orientation film and strong adhesive bonding power are achieved, which effectively suppresses flicker and afterimage problems caused by DC bias, and improves the display quality of the liquid crystal display element.
Smart Images

Figure CN118702917B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a liquid crystal alignment agent and a liquid crystal alignment film and a liquid crystal display element used therein, belonging to the technical field of liquid crystal display. Background Art
[0002] Liquid crystal displays (LCDs) are widely used in various display fields such as televisions, computers, and mobile phones because of their significant advantages such as low driving voltage, low power consumption, light weight, small size, and no harmful rays.
[0003] Polyimide resins are widely used in LCD boxes as liquid crystal alignment films due to their excellent antioxidant and corrosion resistance and simple synthesis methods. Their main function is to align and orient the liquid crystal molecules inside the LCD. Liquid crystal display elements are divided into TN (twisted nematic), STN (super twisted nematic), IPS / FFS (in-plane switching / fringe field switching), VA (vertical alignment) and other types according to their internal structure and driving mode. The working principle of liquid crystal display is to apply an external electric field to the liquid crystal, so that the polar molecules of the liquid crystal are twisted under the action of the external electric field, changing the arrangement state of the liquid crystal molecules inside, changing the direction of the incident polarized light, and then using a polarizer to control whether the light passes through, thereby achieving the purpose of display.
[0004] In recent years, with the development of LCD panels and the improvement of display quality requirements, LCD panels have gradually moved towards high performance, large area, energy saving, narrow frame, etc., and the utilization rate of liquid crystal display components has gradually increased, such as car LCD instrument panels, car entertainment displays, public control instrument panels, etc. Along with this, various LCD display problems have become serious.
[0005] In terms of energy conservation, low-frequency and wide-band driving of LCD panels has become the development direction. Under low-frequency conditions, the AC driving cycle becomes longer, and the LCD driving feed-through voltage, raw materials in the LCD box and direct current (DC) charges in the preparation process are more likely to accumulate, forming a DC bias. Especially under high temperature conditions, the overflow rate of impurity ions and impurities in the box is significantly accelerated, and the DC bias becomes larger, resulting in flicker and afterimage problems caused by the asymmetry of positive and negative voltages under AC driving, which seriously affects the display quality of the LCD panel.
[0006] In terms of large-area and appearance design, narrow-border products have become the development direction of LCD. Narrow borders require full coverage of sealant and PI film (polyimide oriented film), and the width of the sealant is becoming narrower and narrower, which is prone to problems such as box opening due to poor sealing, and poor display caused by external impurities and water vapor entering the LCD. Summary of the invention
[0007] The present invention aims at the problems in the existing liquid crystal display elements and provides a liquid crystal alignment agent, a liquid crystal alignment film and a corresponding liquid crystal display element which have strong adhesive force with sealant, excellent high temperature residual image resistance and can inhibit long-term flickering.
[0008] The technical solution of the present invention to solve the above technical problems is as follows: a liquid crystal alignment agent, comprising at least one of a polyimide precursor and an imidization product of the polyimide precursor, wherein the polyimide precursor has a structural unit as shown in Formula 1 below:
[0009] Formula 1;
[0010] In Formula 1, R1 and R2 are independently selected from a hydroxyl group or an alkoxy group with 1 to 5 carbon atoms;
[0011] In Formula 1, A is a divalent organic group, including at least one of the structures shown in Formula A-1 below, and "*—" represents a bonding position;
[0012] A-1;
[0013] R3 and R4 are independently selected from C 1-5 an alkylene group or a single bond, Z1 and Z2 are independently selected from any one of -O- and -NH-, and C1 is selected from one of C-1:
[0014] C-1;
[0015] R5 is selected from one of O, S and N;
[0016] In Formula 1, B is a tetravalent organic group, and B includes any one of the following B-1 and B-2 groups:
[0017] .
[0018] Further, said R3 and R4 are independently selected from C 2-3 of alkylene.
[0019] Furthermore, the A-1 structural unit has any one of the following structural formulas A-1-1 to A-1-6:
[0020] .
[0021] Furthermore, the structures A-1-1 to A-1-6 are derived from diamine monomers represented by the following formulae DA (A-1-1) to DA (A-1-6):
[0022] .
[0023] Furthermore, the divalent organic group A in Formula 1 may also include other structures other than the A-1 structure, and the other structures are one or more of the following formulae:
[0024] .
[0025] Furthermore, the tetravalent organic group B in Formula 1 may also include other structures other than the structures B-1 and B-2, and the other structures are one or more of the following formulae:
[0026] .
[0027] Furthermore, the A-1 structural unit accounts for 10 to 90% of the total molar number of the A structural unit.
[0028] Furthermore, the liquid crystal alignment agent also includes a solvent, and the solvent is one or more of N-methyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylacetamide, N,N-dimethylformamide, diethylene glycol monoethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol methyl ethyl ether, ethylene glycol dimethyl ether, and diethylene glycol monomethyl ether ethyl ester.
[0029] The invention also discloses a liquid crystal alignment film, which is made of the liquid crystal alignment agent of the invention.
[0030] The invention also discloses a liquid crystal display element, which comprises the liquid crystal alignment film of the invention.
[0031] The beneficial effects of the present invention are:
[0032] The liquid crystal alignment film prepared by the liquid crystal alignment agent of the present invention has the advantages of strong adhesion with sealant, excellent resistance to high temperature residual image performance, and suppression of long-term flicker. The liquid crystal alignment agent of the present invention contains a specific structural unit "A-1", and the unique conjugated group in its molecule, as well as the spatial distribution arrangement of the A-1 structure and other monomer molecules after film formation, so that the liquid crystal alignment film of the present invention has the advantage of fast DC bias charge release rate, so as to suppress flicker and high temperature residual image problems caused by DC bias; on the other hand, the specific molecular structure of A-1 can improve the van der Waals force with the liquid crystal molecules, and suppress the high temperature residual image problem caused by the decrease of anchoring force due to elastic deformation of the PI film surface under high temperature conditions; in addition, the double bond in the "A-1" molecular structural unit is easy to form a covalent bond with the acrylate or bridging agent in the sealant at high temperature, thereby improving the adhesion between the PI film and the sealant. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is compound a-3 1 H-NMR spectrum;
[0034] Figure 2 for Figure 1 The chemical shift of 1 H-NMR spectrum;
[0035] Figure 3 for Figure 1 The chemical shift of 6.4-9.4 1 H-NMR spectrum;
[0036] Figure 4 is the DSC melting point spectrum of compound a-3;
[0037] Figure 5 The diamine compound DA (A-1-1) 1 H-NMR spectrum;
[0038] Figure 6 for Figure 5 The chemical shift of 1.5-5.5 1 H-NMR spectrum;
[0039] Figure 7 for Figure 5 Chemical shifts of 6-9 1 H-NMR spectrum;
[0040] Figure 8 is the DSC melting point spectrum of the diamine compound DA (A-1-1);
[0041] Fig. 9 Schematic diagram of the positions of A, B, C, and D pixels on a liquid crystal display element in the evaluation of the high-temperature afterimage performance of the liquid crystal display element. DETAILED DESCRIPTION
[0042] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0044] <Liquid Crystal Alignment Agent>
[0045] A liquid crystal alignment agent includes at least one of a polyimide precursor and an imidization product of the polyimide precursor, wherein the polyimide precursor has a structural unit as shown in Formula 1 below:
[0046] Formula 1;
[0047] In Formula 1, R1 and R2 are independently selected from a hydroxyl group or an alkoxy group with 1 to 5 carbon atoms;
[0048] In Formula 1, A is a divalent organic group, including at least one of the structures shown in Formula A-1 below, and "*—" represents a bonding position;
[0049] A-1;
[0050] R3 and R4 are independently selected from C 1-5 an alkylene group or a single bond, Z1 and Z2 are independently selected from any one of -O- and -NH-, and C1 is selected from one of C-1:
[0051] C-1;
[0052] R5 is selected from one of O, S and N;
[0053] In Formula 1, B is a tetravalent organic group, and B includes any one of the following B-1 and B-2 groups:
[0054] .
[0055] Further, said R3 and R4 are independently selected from C 2-3 of alkylene.
[0056] Furthermore, the A-1 structural unit has any one of the following structural formulas A-1-1 to A-1-6:
[0057] .
[0058] Furthermore, the structures A-1-1 to A-1-6 are derived from diamine monomers represented by the following formulae DA (A-1-1) to DA (A-1-6), respectively:
[0059] .
[0060] Furthermore, the divalent group A in Formula 1 may also include other structures other than the A-1 structure, and the other structures are one or more of the following formulae:
[0061] .
[0062] Furthermore, the tetravalent organic group B in Formula 1 may also include other structures other than the structures B-1 and B-2, and the other structures are one or more of the following formulae:
[0063] .
[0064] Furthermore, the A-1 structural unit accounts for 10 to 90% of the total molar number of the A structural unit.
[0065] Furthermore, the liquid crystal alignment agent also includes a solvent, and the solvent is one or more of N-methyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylacetamide, N,N-dimethylformamide, diethylene glycol monoethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol methyl ethyl ether, ethylene glycol dimethyl ether, and diethylene glycol monomethyl ether ethyl ester.
[0066] A liquid crystal alignment film is made of the liquid crystal alignment agent of the present invention.
[0067] A liquid crystal display element comprises the liquid crystal alignment film of the present invention.
[0068] The concentration of the finished liquid crystal alignment agent of the present invention is preferably 2-10%, more preferably 3-7%. The concentration of the liquid crystal alignment agent directly affects the thickness of the liquid crystal alignment film, and the concentration of the liquid crystal alignment agent can be freely adjusted according to the required film thickness.
[0069] (1) Synthesis of polyimide precursor - polyamic acid
[0070] A diamine of structure A and a tetraacid dianhydride of structure B in formula 1 are provided, and a polymer solution is obtained by stirring polymerization in the presence of an organic solvent, and then the polymer solution is added to a solvent for dilution to prepare a liquid crystal alignment agent, or the polymer solution is added to a poor solvent for precipitation, filtration and drying to obtain a purified polymer solid, and then a diluting solvent is added to the purified polymer solid to prepare the liquid crystal alignment agent of the present invention.
[0071] The polymerization reaction needs to be carried out in a solvent to accelerate the reaction rate. There is no particular limitation on the organic solvent used for the reaction. It only needs to dissolve the diamine and dianhydride monomers. It is preferably a non-protonic polar solvent, which may include one or a mixture of N-methyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylacetamide, and N,N-dimethylformamide. The concentration of the polymerization reaction is preferably 5 to 30%, and more preferably 10 to 20%.
[0072] There are no particular limitations on the stirring speed and temperature of the polymerization reaction. The stirring speed may be 100 to 1000 rpm, and the reaction temperature may be 0 to 180° C., preferably 20 to 100° C.
[0073] The solvent used for the purification and precipitation of the polymer solid of the present invention is not particularly limited, as long as the solvent used can precipitate the polymer solid, and can be listed as a mixture of one or more of methanol, ethanol, water, propanol, isopropanol, butanol, ethyl acetate, ethyl carboxylic acid and halogen-containing solvents. The solvent used for the polymerization reaction liquid or polymer solid dilution of the present invention can be listed as a mixture of one or more of N-methyl-2-pyrrolidone, N-ethylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, γ-butyrolactone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol methyl ethyl ether, ethylene glycol dimethyl ether, and diethylene glycol methyl ether acetate. The first five solvents listed above (N-methyl-2-pyrrolidone, N-ethylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, γ-butyrolactone) are benign solvents, which mainly play the role of dissolving the polymer. The last six solvents (ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol methyl ethyl ether, ethylene glycol dimethyl ether, diethylene glycol methyl ether acetate) are poor solvents, which mainly play the role of reducing the surface tension of the solution and increasing the leveling effect of the alignment agent. The present invention does not particularly limit the ratio of benign solvents to poor solvents, as long as there is no precipitation in the prepared liquid crystal alignment agent and it has a good coating leveling effect. The mass ratio of the poor solvent in the solvent system is preferably 10-60%, and more preferably 25-40%.
[0074] (2) Synthesis of polyimide precursor - polyamic acid ester
[0075] Polyamic acid ester can be obtained by esterifying a dianhydride compound with an alcohol compound to obtain a tetracarboxyl diester compound intermediate, and then the intermediate is polymerized with a diamine compound under a catalyst to obtain a polyamic acid ester polymer. The polymer is then added to a poor solvent for precipitation, filtered and dried to obtain a polyamic acid ester solid, and then the polyamic acid ester solid is dissolved in an organic solvent, and mechanical impurities are removed by filtering to obtain a liquid crystal alignment agent.
[0076] The synthesis of polyamic acid ester can also be obtained by esterifying the above-mentioned polyamic acid solution. Specifically, the polyamic acid solution can be reacted with an esterifying agent to obtain a polyamic acid ester solution through a dehydration esterification reaction, and then the solution is added to a poor solvent for precipitation, and the esterifying agent is removed by filtering and drying to obtain a polyamic acid ester solid, and then the polyamic acid ester solid is dissolved in an organic solvent, and mechanical impurities are removed by filtering to obtain a liquid crystal alignment agent. The above-mentioned esterifying agent can be listed as one of N,N-dimethylformamide dimethyl acetal, N,N-dimethylformamide diethyl acetal, N,N-dimethylformamide dipropyl acetal, N,N-dimethylformamide dibutyl acetal, and N,N-dimethylformamide dipentyl acetal. The amount of the esterifying agent is 1 to 8 times the molar equivalent of the polyamic acid dianhydride used, and more preferably 2 to 5 times. The temperature for the esterification reaction is preferably 10 to 150°C, and more preferably 20 to 60°C. The reaction time of the polyamic acid ester is preferably 0.5 to 20 hours, more preferably 3 to 8 hours, and the concentration in the esterification reaction is preferably 2 to 15%, more preferably 5 to 10%.
[0077] The poor solvents used for solute precipitation and extraction in the above two polyamic acid ester preparation methods and the solvents used for polyamic acid ester solid dissolution can be the same as the solvents used for the above polyamic acid solution precipitation and polyamic acid solid dissolution, so they are not repeated here.
[0078] (3) Synthesis of polyimide
[0079] Polyimide can be obtained by dehydrating imidization of synthesized polyamic acid. Polyimide can be a partially imidized product formed by dehydrating imidization of a part of the polyamic acid as its precursor to form a polyimide and polyamic acid coexisting, or it can be a completely imidized product obtained by dehydrating imidization of all polyamic acid. The imidization rate of polyimide is preferably 20-95%, more preferably 40-70%. The imidization rate refers to the sum of the number of imide ring structures relative to the amic acid structure and the number of imide ring structures. Here, a part of the imide ring can be an isoimide ring.
[0080] The preparation method of polyimide can adopt the chemical imidization method, and the chemical imidization method refers to the preparation of polyimide by dehydration and ring closure of polyamic acid at a relatively low temperature in the presence of a dehydrating agent and a catalyst.
[0081] In chemical imidization, the types of dehydrating agents can be listed as one or more mixtures of acetic anhydride, propionic anhydride or trifluoroacetic anhydride, and the catalyst can be selected from one or more mixtures of pyridine, 4-methylpyridine, trimethylamine or triethylamine. The reactant ratio of the dehydrating agent and the catalyst is not particularly limited in the present invention, and the ratio can be adjusted according to the degree of imidization. The temperature for the chemical imidization reaction is 20-70°C, preferably 30-50°C; the reaction time is 1-20 hours, more preferably 3-10 hours; the dehydrating agent and catalyst remaining in the solution after the polyimide reaction are preferably removed by precipitation. The precipitation method refers to adding the polyimide reaction solution to a poor solvent to precipitate a polyimide solid, and removing the imidization dehydrating agent and catalyst by filtering and drying. The poor solvent used for precipitation can be the same as the solvent used for the precipitation of the above-mentioned polyamic acid solid, so it will not be repeated here. The obtained polyimide solid is redissolved to obtain a polyimide solution.
[0082] The present invention has no particular limitation on the solvent used for dissolving the polyimide solid, which can be exactly the same as the solvent used for dissolving the polyamic acid solid, so it will not be described here. The prepared solution is filtered to remove mechanical impurities to obtain the liquid crystal alignment agent of the present invention.
[0083] Furthermore, the liquid crystal alignment agent of the present invention may also include a molecular weight regulator, whose main purpose is to adjust the molecular weight of the polymer so that the degree of polymerization of the polymer is controlled within a suitable range to facilitate the dissolution of the polymer and the feasibility of coating on the PI film production line. The molecular weight regulator refers to monoamine compounds, monoanhydride compounds or monoisocyanate compounds; specifically, monoamine compounds refer to butylamine, pentylamine, aniline, p-aminostyrene, p-aminophenylethane, etc.; monoanhydride compounds refer to phthalic anhydride, o-cyclohexanedicarboxylic anhydride, maleic anhydride, itaconic anhydride, nadicacid anhydride, n-dodecylsuccinic anhydride, etc.; monoisocyanate compounds refer to phenyl isocyanate, naphthyl isocyanate, etc. There is no particular limitation on the amount of the molecular weight regulator used in the present invention, as long as the prepared liquid crystal alignment agent has excellent dissolution effect and coating effect.
[0084] Furthermore, the liquid crystal alignment agent of the present invention may also include additives, wherein the additives are silane compounds and epoxy compounds. The silane additives can improve the adhesion between the PI film and the substrate, and the presence of the epoxy compound can improve the uniformity and stability of the liquid crystal alignment film.
[0085] The silane compound includes but is not limited to N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyldimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-bis(ethylene oxide)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, diethoxy(3-glycidyloxypropyl)methylsilane, 2-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane. The amount of the silane compound additive added is 0.1-15% of the total weight of the polymer, and more preferably 0.5-5%.
[0086] The epoxy compound includes but is not limited to polypropylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycerol diglycidyl ether, N,N, N',N'-tetraglycidyl-m-xylene diamine, N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, 3-(N,N-diglycidyl)aminopropyltrimethoxysilane, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether. The amount of epoxy additive added is 0.1-15% of the total weight of the polymer, and more preferably 0.5-5%.
[0087] <Liquid crystal alignment film>
[0088] The liquid crystal alignment film of the present invention is preferably manufactured by the following steps: coating the liquid crystal alignment agent of the present invention on a substrate, obtaining a liquid crystal alignment film through pre-curing and main curing, subjecting the obtained liquid crystal alignment film to an orientation treatment, and then cleaning the orientation film surface with water or an organic solvent or subjecting it to a secondary curing treatment, and finally obtaining the liquid crystal alignment film of the present invention.
[0089] The substrate used for coating the liquid crystal alignment agent of the present invention is not particularly limited as long as it is a substrate with high transparency. In addition to the glass substrate, polypropylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycerol diglycidyl ether, N,N, N',N'-tetraglycidyl-m-xylene diamine, N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane or 3-(N,N-diglycidyl)aminopropyltrimethoxysilane plate, silicon nitride substrate, transparent polyimide substrate and polyester substrate can also be used. Preferably, the glass substrate coated with ITO electrode is preferred. The above-mentioned ITO is indium tin oxide, which is used to provide an electric field to control the movement and deflection of liquid crystal, and then cooperate with a polarizer to achieve the purpose of display.
[0090] The coating method of the liquid crystal alignment agent of the present invention is not particularly limited. The coating method is usually relief printing, screen printing, inkjet, dipping, slit coating, spin coating, etc., and any of these methods can be used as needed.
[0091] The main purpose of pre-curing the liquid crystal alignment agent is to remove the solvent in the liquid crystal alignment agent. The pre-curing temperature is usually 60-140°C and the pre-curing time is 1-10 minutes. The main purpose of the main curing is to imide the polyamic acid component in the pre-cured film into polyimide, or to increase the imidization rate of the alignment film whose component is already polyimide, thereby improving the stability of the film. The main curing temperature of the liquid crystal alignment film of the present invention is preferably 150-300°C, and the main curing time is 5-180 minutes.
[0092] There is no particular limitation on the thickness of the liquid crystal alignment film of the present invention, and the film thickness is usually 30-200 nm, preferably 50-120 nm. Too thick a film thickness may easily affect the orientation effect of the liquid crystal alignment film, whereas too thin a film thickness may easily lead to a decrease in the stability of the later LCD. The appropriate thickness of the liquid crystal alignment film may be selected according to needs.
[0093] For the orientation treatment of the film, friction orientation and photo orientation treatment methods can be listed. Since the friction orientation method is prone to dust and electrostatic breakdown, the present invention prefers the photo orientation treatment method, but the present invention is not limited thereto. The wavelength of the polarized light during the photo orientation treatment is 100 to 400 nm, more preferably 200 to 365 nm. The light dose required for the film photo orientation treatment is preferably 10 to 2000 mj / cm 2 , more preferably 100 to 1000 mj / cm 2 .
[0094] After the alignment treatment is completed, the solvent used in the cleaning process is not particularly limited in the present invention, and one or a mixture of water, methanol, ethanol, and methyl lactate can be used. The liquid crystal alignment film of the present invention can also omit the cleaning step and directly perform a secondary curing treatment.
[0095] The oriented film obtained after the above-mentioned photo-alignment treatment can also be subjected to a post-baking treatment, the purpose of which is to remove the small molecular compounds generated in the photo-alignment treatment or remove the solvent used in the cleaning process, and promote the re-orientation of the molecular chains on the film surface.
[0096] The post-baking temperature of the liquid crystal alignment film of the present invention is preferably 150-300°C, more preferably 180-250°C, and the baking time is preferably 5-120 minutes, more preferably 10-60 minutes. The higher the temperature, the more it can promote the reorientation of the molecules on the film surface, but too high a temperature will cause the molecules on the film surface to break, and the baking temperature and time can be appropriately selected according to the characteristics of the molecules on the film surface.
[0097] <Liquid Crystal Display Element>
[0098] There is no particular limitation on the liquid crystal used for the liquid crystal display element of the present invention. For example, nematic liquid crystal, smectic liquid crystal or cholesteric liquid crystal can be used. The liquid crystal model with positive or negative dielectric anisotropy can be selected according to the mode of the liquid crystal display element. There is no particular limitation on the type of liquid crystal display element prepared by the liquid crystal alignment agent and liquid crystal alignment film of the present invention. It can be TN type (twisted nematic), STN type (super twisted nematic), VA type (vertical alignment), IPS\FFS (in-plane switching\fringe field switching), etc. The present invention uses an IPS / FFS lateral liquid crystal display element to characterize the beneficial effects of the present invention, which includes a liquid crystal alignment film obtained by the aforementioned liquid crystal alignment film manufacturing method, but the beneficial effects of the present invention are not limited to this IPS / FFS liquid crystal display element.
[0099] The preparation method of the above-mentioned IPS or FFS type liquid crystal display element includes the following steps: preparing two substrates, one of which has an IPS or FFS type ITO electrode, and the other substrate has no ITO electrode or has ITO or other conductive materials used to shield electromagnetic interference, coating the liquid crystal orientation agent of the present invention on the two substrates, baking them on a hot plate at 90°C for 5 minutes and in an oven at 230°C for 25 minutes, and then irradiating the two substrates with ultraviolet polarized light of 254nm wavelength in a certain direction, and then placing the two substrates in an oven for heat baking again, the secondary curing temperature is 230°C, and the time is 30 minutes.
[0100] For the two substrates after the above-mentioned post-baking treatment, spacer particles with a diameter of 4μm are scattered on one of the substrates (if the substrate used has its own thick support material, there is no need to spread the spacer particles), and sealant is coated on the other substrate, and the box is attached in a manner that the orientation films are face to face and the upper and lower substrates are oriented in anti-parallel directions. The sealant is then cured to obtain an empty liquid crystal box, and liquid crystal is injected into the empty liquid crystal box by vacuum filling, and the liquid crystal liquid inlet is sealed to obtain an IPS or FFS type liquid crystal display element.
[0101] In the above polarized light alignment treatment process, the incident angle of light is not particularly limited in the present invention. The incident light may be perpendicular to the substrate or may form a certain tilt angle with the substrate.
[0102] <Synthesis Example of Diamine Compound>
[0103] Synthesis example 1:
[0104] The preparation method of the diamine compound DA (A-1-1) represented by the structural unit A-1-1 is shown in the following synthetic route:
[0105] ;
[0106] (1) Synthesis of compound a-3
[0107] In a 500mL three-necked round-bottom flask, a-1 (39.88g, 240mmol), triethylamine (22.26g, 220mmol) and 200g of solvent toluene were added, the temperature was raised to 50°C, and a mixture of a-2 (19.30g, 100mmol) and 100g of solvent toluene was slowly added dropwise to the system. The addition was completed within one hour. The system was kept at 50°C for 5 hours. TLC tracking showed that there was no residue of the raw material furandicarbonyl chloride. The reaction was stopped, and the reaction solution was washed with water until neutral. The upper organic phase was desolvated and the solid obtained was added with 45g of tetrahydrofuran and 90g of methanol. The mixture was stirred for 1 hour, and 34g of yellow solid a-3 was obtained after filtration and drying. The yield was 76%.
[0108] 1 H-NMR (such as Figure 1-Figure 3 The structure was determined to be the target compound a-3, and its melting point (as shown Figure 4 The temperature of the air in the air is 232.90~238.59℃.
[0109] ;
[0110] Figure 1-Figure 3 Among them, δ=2.979~3.350ppm is c, d 8H, δ= 7.122ppm is f 2H, δ=7.523~8.185ppm is a, b 8H, δ=8.575~8.605ppm is e 2H, which shows that compound a-3 is the target structure.
[0111] (2) Synthesis of compound DA (A-1-1)
[0112] The above-mentioned compound a-3 (45 g, 100 mmol), palladium carbon (2.25 g, containing water, solid content of 44.1%) and 450 g of tetrahydrofuran solvent (5% by mass of compound a-3) were added into a 1L autoclave. The autoclave was sealed and replaced with hydrogen 3 to 5 times. The hydrogen was pressurized to 1.0 to 1.5 MPa and reacted at 50 ° C for 12 hours under stirring. After the reaction, the catalyst palladium carbon was filtered with a filter membrane with a pore size of 0.2 μm, the filtrate was desolventized, and the obtained solid was added to 120 g of ethanol and stirred for 0.5 hours. After filtration and drying, 32 g of yellow solid compound DA (A-1-1) was obtained with a yield of 82%.
[0113] 1 H-NMR( Figure 5-Figure 7 ) The test confirmed that the structure was the target compound DA (A-1-1), and its melting point ( Figure 8 ) is 159.35~170.85℃.
[0114] ;
[0115] Figure 5-7 Among them, δ = 2.646~3.412ppm is c, d 8H, δ = 7.117ppm is f 2H, δ = 6.480~6.902ppm is a, b 8H, δ = 8.569~8.598ppm is e 2H, δ = 4.877ppm is g 2H, which shows that compound DA (A-1-1) is the target structure.
[0116] The diamine compounds DA(A-1-2)~DA(A-1-6) represented by "Formula A-1-2~Formula A-1-6" can all be synthesized according to the process route of Synthesis Example 1, and can all be used to synthesize the target diamine compounds DA(A-1-2)~DA(A-1-6) through amidation or esterification of their respective parent compounds, and then catalytic hydrogenation reaction, wherein the structural formulas of DA(A-1-2)~DA(A-1-6) are as follows, and the high-resolution mass spectrometry results and elemental analysis results of the corresponding target compounds are shown in Table 1 below.
[0117] .
[0118] Table 1 Mass spectrometry and elemental analysis data of target diamine compounds DA (A-1-2) to DA (A-1-6)
[0119]
[0120] <Example>
[0121] The present invention will be further explained in detail by way of specific examples, but it is not intended to limit the present invention. The abbreviations of the compounds used in this example and the comparative example and the determination methods of various properties are as follows:
[0122] NMP: N-methyl-2-pyrrolidone;
[0123] BC: ethylene glycol monobutyl ether;
[0124] DA (A-1-1): ;
[0125] DA (A-1-2): ;
[0126] DA (A-1-3): ;
[0127] DA (A-1-4): ;
[0128] DA (A-1-5): ;
[0129] DA (A-1-6): ;
[0130] DA(A-2): p-phenylenediamine;
[0131] DA(A-3): 4,4'-diaminodiphenyl ether;
[0132] DA(A-4): 2,4-diaminododecyloxybenzene;
[0133] DA(A-5): 4,4'-diaminodiphenylmethane;
[0134] DA(A-6): 1,2-bis(4-aminophenoxy)ethane;
[0135] DAH (B-1): 1,2,3,4-cyclobutanetetracarboxylic dianhydride;
[0136] DAH (B-2): 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride;
[0137] DAH (B-3): 2,3,5-tricarboxycyclopentaneacetic dianhydride;
[0138] DAH (B-4): 3,3',4,4'-biphenyltetracarboxylic dianhydride.
[0139] ﹤Determination of imidization rate﹥
[0140] The method for determining the imidization rate in the polyimide solution is as follows: the imidized solid powder is added to a deuterated dimethyl sulfoxide solvent to prepare a solution with a mass concentration of 5%, and the solution is completely dissolved by ultrasonication. The solution is added to a nuclear magnetic sample tube, and the nuclear magnetic hydrogen spectrum is measured using a nuclear magnetic instrument (JNM-ECZ400, manufactured by JEOL DATUM). The protons of the structure that do not change before and after imidization are set as reference protons, and the product value of this proton and the product value of the carboxylic acid protons near 11 to 14 ppm are used to calculate the imidization rate according to the following formula.
[0141] Imidization rate = (1-a / b) 100%
[0142] In the above formula, a is the ratio of the product value of the carboxylic acid protons in the tested H1-NMR to the reference protons, and b is the ratio of the number of carboxyl protons to the number of reference protons when imidization does not occur.
[0143] Embodiment 1:
[0144] A 500mL three-necked round-bottom flask was vented for protection, and then compounds DA(A-1-1) (7.85g, 20 mmol), DA(A-2) (2.70g, 25 mmol), DA(A-4) (1.46g, 5mmol) and NMP (81.55g) were added into the three-necked flask at room temperature. The reaction system was heated to 40°C and kept warm for 0.5 hours to completely dissolve. Then DAH(B-1) (6.86g, 35mmol), DAH(B-2) (3.36g, 215mmol) and NMP (81.55g) were added into the system, and the temperature was maintained at 80°C for 10 hours. The reaction was then cooled to room temperature to obtain a polyamic acid polymer PA-1 with a concentration of 12%.
[0145] Dilution: 100 g of PA-1 polyamic acid solution was added with 71.6 g of NMP and 68.4 g of BC, stirred at room temperature for 2 hours, and then filtered through a 0.2 μm filter membrane to obtain the liquid crystal alignment agent LCA-1 of Example 1. The concentration of the polymer in the liquid crystal alignment agent was 5.0%, and the solvent ratio was NMP:BC=70:30.
[0146] Embodiment 2-12:
[0147] The liquid crystal alignment agents corresponding to Examples 2-12 are (LCA-2) to (LCA-12), respectively, and can be prepared in the same manner as Example 1, except that the types and material ratios of the monomers used are changed, the initial concentration of the polymerization reaction is 12.0%, the concentration of the liquid crystal alignment agent obtained after dilution is 5.0%, and the solvent ratio in the alignment agent is NMP:BC=70:30. The specific types of monomers and material ratios are shown in Table 2 below.
[0148] Table 2 Types and amounts of monomers used in the liquid crystal alignment agent of the examples
[0149]
[0150] Embodiment 13:
[0151] Synthesis of polyamic acid ester: A 500 mL three-necked round-bottom flask was added with the amic acid solution PA-1 (100 g) prepared in Example 1 and 140 g of solvent NMP, the reaction concentration was diluted to 5%, and then 4 times the molar equivalent of dianhydride was added to the system, the temperature was raised to 50°C and stirred for reaction for 5 hours to carry out esterification reaction, and then the obtained reaction solution was dripped into 2000 mL of methanol while stirring, the esterifying agent N, N-dimethyl diethyl acetal was removed, the white precipitate was filtered out, the filter cake was rinsed with methanol, and then dried to obtain 11.5 g of white solid, 10 g of the solid was taken and dissolved in 133 g of NMP and 57 g of BC solvent, and then 200 g of the liquid crystal alignment agent LCA-2 corresponding to Example 2 was added to the system, stirred at room temperature for 3 hours, and filtered to obtain the liquid crystal alignment agent (LCA-13) corresponding to Example 13.
[0152] Embodiment 14:
[0153] Synthesis of SPI (soluble polyimide): Add the amic acid solution PA-1 (100 g) prepared in Example 1 and 140 g of solvent NMP into a 500 mL three-necked round-bottom flask, dilute the reaction concentration to 5%, then add 3 times the molar equivalent of dianhydride acetic anhydride and 2.5 times the molar equivalent of dianhydride pyridine into the system, heat to 30 ° C and stir for 5 hours to carry out chemical imidization. Then, the obtained reaction solution is added dropwise into 2000 mL of methanol while stirring, acetic anhydride and pyridine are removed, the white precipitate is filtered out, the filter cake is rinsed with methanol, and then dried to obtain a white solid powder. The imidization rate of the solid powder is 65% when detected by nuclear magnetic hydrogen spectrum. Take 12 g of the solid and add it to 88 g of solvent NMP and stir to dissolve it completely to obtain a polyimide solution SPI-1 with a concentration of 12%.
[0154] Dilution: Take 100 g of the above SPI-1 solution, add 71.6 g of NMP solvent and 68.4 g of BC solvent, stir evenly, and obtain the liquid crystal alignment agent LCA-14 corresponding to Example 14 by filtering.
[0155] Embodiment 15:
[0156] 30 g of liquid crystal alignment agent LCA-1 and 20 g of liquid crystal alignment agent LCA-13 were stirred evenly in a 100 mL three-necked bottle, and the liquid crystal alignment agent LCA-15 corresponding to this embodiment was obtained by filtration.
[0157] Embodiment 16:
[0158] 20 g of liquid crystal alignment agent LCA-14 and 80 g of liquid crystal alignment agent LCA-4 were stirred evenly in a 100 mL three-necked bottle, and the liquid crystal alignment agent LCA-16 corresponding to this embodiment was obtained by filtration.
[0159] Comparative Examples 1-6:
[0160] The liquid crystal alignment agents (LCA-17) ~ (LCA-22) corresponding to Comparative Examples 1-6 can all be prepared by the same method as Example 1. The concentration of the polymer in the obtained liquid crystal alignment agents is 5%, and the solvent ratio is NMP:BC=70:30. The difference is that the types and dosage ratios of the monomers used are changed. The specific results are shown in Table 3 below.
[0161] Table 3 Monomer types and amounts used in each liquid crystal alignment agent of Comparative Examples 1-6
[0162]
[0163] Specific characterization of liquid crystal display element sealant adhesion, resistance to high temperature residual image and long-term flicker:
[0164] An IPS type liquid crystal display box was prepared according to the following method: two glass substrates with a length and width of 3cm×4cm and a thickness of 0.7mm were prepared, wherein the lower substrate had a comb-shaped ITO electrode with a thickness of 50nm, and the spacing between adjacent comb-shaped electrodes was 3μm, and the pixel electrodes and the common electrodes were arranged in a cross pattern. There were 4 pixel electrodes, which could be driven separately. The upper glass substrate had no electrode, and the liquid crystal alignment agent prepared in Example 1 was coated on the two substrates, and after pre-curing (hot plate, 85°C, 3 minutes) and main curing (circulation oven, 230°C, 60 minutes), a polyimide coating with a film thickness of 700Å was obtained.
[0165] The upper and lower glass substrates with polyimide coating were irradiated with ultraviolet polarized light for photo-alignment treatment. The wavelength of the irradiated ultraviolet polarized light was 254nm and the light dose was 450mj / cm 2 , and then heated in a heat cycle oven at 230°C for 30 minutes, the upper and lower glass substrates that had been oriented were sprayed with spacer particles with a diameter of 4μm on one substrate, and a square sealant was printed on the other substrate at a position 5mm away from the periphery of the glass. The sealant was directly printed on the surface of the orientation agent film, and a liquid crystal injection port with a diameter of 5mm was left. Then, the upper and lower substrates were bonded together in a manner that the orientation films were face to face, the polarization axes of the light orientation treatment were parallel, and the upper and lower substrates overlapped with a width of 3cm. The two bonded substrates were fixed with a clamp, and cured at a temperature of 150°C for 1 hour to prepare a liquid crystal empty box, and IPS negative liquid crystal was injected into the empty box by decompression, and the liquid crystal injection port was sealed. The liquid crystal display element corresponding to Example 1 was prepared.
[0166] The liquid crystal display elements corresponding to Examples 2-16 and Comparative Examples 1-6 are all prepared according to the same method as described above, except that the coated liquid crystal alignment agent needs to be changed to the liquid crystal alignment agents LCA-2~LCA-16 corresponding to Examples 2-16 and the liquid crystal alignment agents LCA-17~LCA-22 corresponding to Comparative Examples 1-6.
[0167] A. Evaluation of the adhesive strength of liquid crystal display element sealant
[0168] The prepared liquid crystal display element was placed in a 1L high-pressure reactor, 500ml of deionized water was added to the high-pressure reactor, and 10ml of red ink was added dropwise. The reactor was sealed, the temperature was raised to 130°C, the pressure was 0.3MPa, and the temperature was kept for 10 hours. Then the temperature was lowered and the liquid crystal display element was taken out. The liquid crystal display element was observed and powered on.
[0169] The evaluation criteria for sealant adhesion are as follows:
[0170] √: The liquid crystal display element is not immersed in red ink, and the drive display is normal.
[0171] ×: The liquid crystal display element is immersed in red ink and cannot be driven to display.
[0172] B. Evaluation of the high temperature image retention performance of liquid crystal display elements
[0173] Place the prepared liquid crystal unit between two orthogonal polarizers, light up the backlight source without applying voltage, and adjust the configuration angle of the liquid crystal unit in a way that minimizes the brightness of the transmitted light. Then, apply an AC voltage with a frequency of 30Hz to the liquid crystal unit to drive the liquid crystal box, while measuring the VT curve of the liquid crystal box (equipment: PWW-VT VT test system, manufactured by Dongxu Electric Technology Co., Ltd.), and calculate the AC driving voltage V23 when the relative transmittance is 23% and the AC driving voltage V100 when the relative transmittance is 100%. Fig. 9 As shown: The liquid crystal display element is placed on a high-temperature backlight source, the backlight brightness is 10,000 lumens, the temperature is set to 70°C, and the A and B pixels are V 100 Drive for 24 hours, then switch pixels A, B, C, and D to V at the same time 23 Voltage drive, calculated from the applied V 23 The time Ts required from the start of voltage to the time when the brightness of pixels A, B and C, D are the same as those observed by the naked eye.
[0174] The evaluation criteria for high temperature afterimage resistance are as follows:
[0175] Excellent: Ts≤30s, excellent resistance to high temperature afterimage.
[0176] General: 3min≥Ts>30s, the resistance to high temperature afterimage is average.
[0177] Poor: Ts>3min, poor resistance to high temperature afterimage.
[0178] C. Evaluation of long-term flicker characteristics of liquid crystal display elements
[0179] The liquid crystal display elements of the embodiments of the present invention and the comparative examples were subjected to a long-term flicker test using a CA-410 test instrument (manufacturer: Konica Minolta, Japan).
[0180] Test method: driving voltage is V 23 , the frequency is 15 Hz, the measurement time is 24 hours, and the Flicker value F is recorded.
[0181] The long-term flicker suppression characteristics evaluation criteria are as follows:
[0182] √: F≤-50DB, excellent long-term flicker suppression characteristics.
[0183] △: -50DB<F≤-30DB°, long-term flicker suppression characteristics are average;
[0184] ×: Pt>-20DB°, poor long-term flicker suppression characteristics;
[0185] The DC charge relaxation characteristics and pretilt angle performance of the corresponding liquid crystal alignment agents LCA-1 to LCA-22 in Examples 1-16 of the present invention and Comparative Examples 1-6 were tested and evaluated according to the above method.
[0186] Evaluation results:
[0187] The evaluation results of the liquid crystal alignment agents, liquid crystal alignment films and corresponding liquid crystal display elements prepared in Examples 1-16 and Comparative Examples 1-6 are shown in Table 4 below.
[0188] Table 4 Evaluation results of liquid crystal display elements in Examples and Comparative Examples
[0189]
[0190] It can be seen that compared with the prior art, the liquid crystal alignment agent of the present invention introduces a unit containing a specific structure of "A-1" during the synthesis process, and the prepared liquid crystal alignment film has the advantage of strong adhesion to the sealant, and the prepared liquid crystal display element has excellent resistance to high-temperature residual image performance and outstanding long-term flicker suppression characteristics. In addition, the implementation method of the present invention is simple and suitable for large-scale promotion.
[0191] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0192] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A liquid crystal alignment agent, comprising at least one of a polyimide precursor and an imidization product of the polyimide precursor, It is characterized in that The polyimide precursor has a structural unit shown in the following formula 1: Formula 1; In formula 1, R 1 , R 2 Each independently selected from a hydroxyl group or an alkoxy group with 1 to 5 carbon atoms; In formula 1, A is a divalent organic group, including at least one of the structures shown in formula A-1 below, "*—" represents the bonding position; the A-1 structural unit accounts for 20 to 60% of the total molar number of the A structural unit; A-1; R 3 , R 4 Each independently selected from C 1-5 An alkylene group, a single bond, Z 1 , Z 2 are independently selected from any one of -O- and -NH-, C 1 One selected from C-1: C-1; R 5 One selected from O, S, and NH; In Formula 1, B is a tetravalent organic group, and B includes any one of the following B-1 and B-2 groups: 。 2. A liquid crystal alignment agent according to claim 1, It is characterized in that The R 3 , R 4 Each independently selected from C 2-3 of alkylene.
3. A liquid crystal alignment agent according to claim 1, It is characterized in that The A-1 structural unit has any one of the following structural formulas A-1-1 to A-1-6: 。 4. A liquid crystal alignment agent according to claim 3, It is characterized in that The structures A-1-1 to A-1-6 are derived from diamine monomers represented by the following formulas DA (A-1-1) to DA (A-1-6): 。 5. The liquid crystal alignment agent according to claim 1, It is characterized in that The divalent organic group A in Formula 1 may also include other structures other than the A-1 structure, and the other structures are one or more of the following formulae: 。 6. A liquid crystal alignment agent according to claim 1, It is characterized in that The tetravalent organic group B in Formula 1 may also include other structures other than the structures B-1 and B-2, and the other structures are one or more of the following formulae: 。 7. A liquid crystal alignment agent according to any one of claims 1 to 6, It is characterized in that The liquid crystal alignment agent also includes a solvent, which is one or more of N-methyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylacetamide, N,N-dimethylformamide, diethylene glycol monoethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol methyl ethyl ether, ethylene glycol dimethyl ether, and diethylene glycol monomethyl ether ethyl ester.
8. A liquid crystal alignment film, It is characterized in that The liquid crystal alignment film is made of the liquid crystal alignment agent according to any one of claims 1 to 7.
9. A liquid crystal display element, It is characterized in that The liquid crystal display element includes the liquid crystal alignment film according to claim 8.