Sound insulation and heat preservation layer, preparation method thereof and floor heating system

By using a glass fiber skeleton to fill the sound insulation layer with rubber particles and phase change particles of different particle sizes in the electric floor heating system, the problems of high energy consumption and excessive thickness of the electric floor heating system are solved, and both sound insulation and thermal insulation are achieved. , reducing noise and energy consumption, and optimizing material thickness and cost.

CN118702976APending Publication Date: 2024-09-27CHINA SOUTHWEST ARCHITECTURAL DESIGN & RES INST CORP LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410832486.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-09-27

AI Technical Summary

Technical Problem

When taking into account the thermal insulation performance, sound insulation performance and material thickness, the existing electric floor heating system has the problems of high energy consumption, low thermal efficiency and too high total thickness, making it difficult to achieve sound insulation and thermal insulation effects at the same time.

Method used

A sound insulation layer based on a glass fiber skeleton is used. Rubber particles and phase change particles of different particle sizes are filled in the gaps of the glass fiber. The damping and shock-absorbing properties of the rubber particles and the heat storage function of the phase change particles are used to optimize the particle size. and proportioning to achieve both sound insulation and thermal insulation, and the layer is prepared through spinning and pressing processes.

Benefits of technology

It achieves both sound insulation performance and heat storage performance within a lower thickness range, reduces noise and energy consumption, simplifies the structure of the floor heating system, saves the use area, and maximizes the dissipation of vibration energy by optimizing the particle size ratio. , reducing resin consumption and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118702976A
    Figure CN118702976A
Patent Text Reader

Abstract

The invention relates to the technical field of building sound insulation and heat preservation, in particular to a sound insulation and heat preservation layer, a preparation method of the sound insulation and heat preservation layer and a floor heating system.The sound insulation and heat preservation layer comprises glass fibers and resin mixed liquid mixed with the glass fibers, and the resin mixed liquid comprises first rubber particles, second rubber particles, phase change particles and resin; the particle size of the first rubber particles is 40-60 meshes; the particle size of the second rubber particles is 400-600 meshes; the sum of the mass of the first rubber particles and the mass of the second rubber particles accounts for 10wt%-30wt% of the whole material; the mass ratio of the first rubber particles to the second rubber particles is (0-2): 5; the particle size of the phase change particles is 90-110 meshes; the mass of the phase change particles accounts for 35wt%-45wt% of the whole material; the mass of the resin accounts for 5wt%-15wt% of the whole material. According to the scheme, interaction and interface friction between large and small particles (between rubber and rubber and between rubber and phase change particles) in the structure are fully considered, noise between floors is reduced, the phase change particles serve as phase change energy storage materials, heat storage and heat release functions are provided, and meanwhile the purposes of sound insulation and heat preservation are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building sound insulation and heat preservation, and in particular to a sound insulation and heat preservation layer and a preparation method thereof, and a floor heating system. Background Art

[0002] In today's society, as people's requirements for quality of life and comfort continue to increase, smart energy-saving electric floor heating and wall heating have attracted much attention as an efficient and energy-saving heating method. Electric floor heating has a simple structure and can effectively replace cement mortar landfill structure. When constructing electric floor heating structure, it can not only greatly shorten the construction period and reduce on-site construction waste, but also has the advantages of high construction efficiency, clean operation, and low construction cost. Electric floor heating heats up quickly, uses intelligent temperature control such as thermostat, has low energy consumption, and saves energy, electricity and money when used.

[0003] Phase change material (PCM) is a material that can change the state of matter and provide latent heat without changing the temperature. This material absorbs or releases a large amount of latent heat during the phase change process. However, in the existing electric floor heating systems, heating cables or carbon fiber cores are mostly used to release heat. These two floor heating systems usually do not have a phase change energy storage layer, resulting in high energy consumption and low thermal efficiency of the floor heating system. In addition, as people's quality of life improves, the requirements for residential sound environment also increase.

[0004] The current solution is usually to stack functional structures layer by layer, which is unable to take into account the thermal insulation performance, sound insulation performance and material thickness at the same time. The end result is that the total thickness of the floor heating system is too high and too much indoor usable area is occupied. Summary of the invention

[0005] The purpose of the present invention is to overcome the problem that the existing phase change material layer is difficult to take into account the thermal insulation performance, sound insulation performance and material thickness at the same time, resulting in the total thickness of the floor heating system being too high, and to provide a sound insulation layer and a preparation method thereof, and a floor heating system.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: A sound insulation layer, comprising glass fibers and a resin mixture mixed with the glass fibers, wherein the resin mixture comprises first rubber particles, second rubber particles, phase change particles, and resin; The particle size of the first rubber particles is 40-60 mesh; The particle size of the second rubber particles is 400-600 mesh; The sum of the weight of the first rubber particles and the second rubber particles accounts for 10wt% to 30wt% of the entire material; The mass ratio of the first rubber particles to the second rubber particles is 0-2:5; The particle size of the phase change particles is 90-110 meshes; The mass of the phase change particles accounts for 35wt% to 45wt% of the whole material; The mass of the resin accounts for 5wt% to 15wt% of the entire material.

[0007] The sound insulation and heat preservation layer provided by the present invention is based on a glass fiber skeleton, and rubber particles and organic phase change materials are filled in the gaps of the glass fibers, wherein the first rubber particles have a larger particle size and can fill the pores of the glass fiber skeleton over a large area, but in some small gaps, second rubber particles and phase change particles with smaller particle sizes are required for filling. The scheme of the present invention utilizes the characteristics of rubber particles in damping, shock absorption and sound insulation, which can effectively reduce the noise generated by the collision between floor slabs, while the phase change particles can act as phase change energy storage materials, providing heat storage and heat release functions, thereby achieving the purpose of sound insulation and heat preservation at the same time. By specially limiting the particle size and ratio of the first rubber particles, the second rubber particles and the phase change particles, the rubber particles and the phase change particles are dispersed in the middle of the glass fiber skeleton in the best ratio, achieving the maximum dissipation of vibration energy, the minimum resin usage and cost investment, and thus the sound insulation and heat preservation layer takes into account both sound insulation performance and heat storage performance within a relatively low thickness range.

[0008] Optionally, the particle size of the first rubber particles is 50 mesh, the particle size of the second rubber particles is 500 mesh, the sum of the masses of the first rubber particles and the second rubber particles accounts for 30wt% of the overall material, the mass ratio of the first rubber particles to the second rubber particles is 2:5, the particle size of the phase change particles is 100 mesh, the mass of the phase change particles accounts for 40wt% of the overall material, and the mass of the resin accounts for 5wt%~15wt% of the overall material.

[0009] By adopting this configuration, the optimal particle sizes and mass proportions of the first rubber particles, the second rubber particles, and the phase change particles are further limited, and the relationship among the thickness, sound insulation performance, and heat storage performance of the sound insulation layer is further optimized.

[0010] Optionally, the mass of the resin accounts for 5wt% of the entire material, and in the resin mixture, the mass ratio of the sum of the mass of the first rubber particles and the second rubber particles: the phase change particles: the resin is 6:8:1.

[0011] This setting is used to further optimize the mass proportion of the resin and the mass ratio of the rubber particles, phase change particles, and resin, thereby maximizing the dissipation of vibration energy and minimizing the resin usage and cost investment, thereby achieving the optimization of the thickness, sound insulation performance, and heat storage performance of the sound insulation layer.

[0012] Optionally, the phase change particles are paraffin wrapped in a silica shell.

[0013] The preferred phase change particles are paraffin wrapped in a silica shell. Paraffin itself is a good phase change material. The introduction of the silica shell layer realizes the encapsulation of the phase change core material to prevent its leakage. At the same time, it improves the overall thermal conductivity of the composite material, enhances the thermal stability of the phase change material, and makes the material have advantages such as flame retardancy, which greatly enhances the safety of the use of the phase change particles.

[0014] Optionally, the resin is epoxy resin or polyurethane.

[0015] Optionally, the sound insulation and heat preservation layer is in the form of a long coil, the width of the sound insulation and heat preservation layer is 0.8m~1.2m, and the thickness of the sound insulation and heat preservation layer is 10mm~20mm.

[0016] Optionally, the width of the sound insulation layer is 1m, and the thickness of the sound insulation layer is 10mm.

[0017] The sound insulation layer provided by the present invention preferably has a thickness of 10 mm, which further optimizes the relationship between the thickness, sound insulation performance and heat storage performance of the sound insulation layer.

[0018] A method for preparing a sound insulation layer, used for manufacturing the above-mentioned sound insulation layer, comprises the following steps: While the glass fibers are being spinned, the resin mixture is sprayed, and then integrally pressed and formed.

[0019] The method for preparing the sound insulation layer provided by the present invention is based on a glass fiber skeleton, and rubber particles and organic phase change materials are filled in the gaps between the glass fibers, so that the sound insulation layer has both sound insulation performance and heat storage performance within a relatively low thickness range.

[0020] A floor heating system comprises the above-mentioned sound insulation and heat preservation layer, an electric heating film layer is laid on the sound insulation and heat preservation layer, a heat equalization layer is laid on the electric heating film layer, and a finishing layer is laid on the heat equalization layer.

[0021] The floor heating system provided by the present invention can be laid on the floor slab, and used as the sound insulation layer of the electric floor heating. The rubber particles therein can effectively dissipate the noise energy generated by the impact of the floor slab and reduce the noise; the phase change material can store heat energy when the power is on, and slowly release the heat after the power is off to maintain the temperature of the room. The entire system can continue to release the originally stored heat after the power is off to maintain the set temperature. Since the floor heating system has a small thickness and a simple structure, it can save the use area and achieve a rapid temperature response. Considering the peak and valley electricity prices, an intermittent electric heating method can be adopted to effectively reduce the cost of users.

[0022] Optionally, the heat-spreading layer is an aluminum plate heat-spreading layer.

[0023] Compared with the prior art, the present invention has the following beneficial effects: 1. The sound insulation and heat preservation layer provided by the present invention is based on a glass fiber skeleton, and rubber particles and organic phase change materials are filled in the gaps of the glass fibers. The first rubber particles have a large particle size and can fill the pores of the glass fiber skeleton over a large area, but in some small gaps, the second rubber particles and phase change particles with a smaller particle size are required to be filled. The scheme of the present invention utilizes the characteristics of rubber particles in damping, shock absorption and sound insulation, fully considers the interaction and interface friction between large and small particles inside the structure (between rubber particles and rubber particles, between rubber particles and phase change particles), and effectively reduces the noise generated by the collision between the floor slabs, while the phase change particles can act as phase change energy storage materials, providing heat storage and heat release functions, thereby achieving the purpose of sound insulation and heat preservation at the same time. By specially limiting the particle size and ratio of the first rubber particles, the second rubber particles and the phase change particles, the rubber particles and the phase change particles can achieve the best dispersion ratio in the middle of the glass fiber skeleton, achieve the maximum dissipation of vibration energy, the minimum resin dosage and cost investment, and thus make the sound insulation and heat preservation layer take into account both sound insulation performance and heat storage performance within a relatively low thickness range. It can be understood that the sound insulation and heat preservation layer provided by the present invention is not limited to being used in floor heating systems and floors, but can also be used in other building structures such as roofs and walls, and can exert good sound insulation and heat storage performance.

[0024] 2. The method for preparing the sound insulation layer provided by the present invention is based on a glass fiber skeleton, and rubber particles and organic phase change materials are filled in the gaps between the glass fibers, so that the sound insulation layer has both sound insulation performance and heat storage performance within a relatively low thickness range.

[0025] 3. The floor heating system provided by the present invention can be laid on the floor slab, and used as the sound insulation layer of the electric floor heating. The rubber particles therein can effectively dissipate the noise energy generated by the impact of the floor slab and reduce the noise; the phase change material can store heat energy when the power is on, and slowly release the heat after the power is off to maintain the temperature of the room. The entire system can continue to release the originally stored heat after the power is off to maintain the set temperature. Since the floor heating system has a small thickness and a simple structure, it can save the use area and achieve a rapid temperature response. Taking into account the peak and valley electricity prices, an intermittent electric heating method can be adopted to effectively reduce the cost of users. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a schematic diagram of the materials of the sound insulation layer of Example 1; Figure 2 This is a schematic structural diagram of the floor heating system of Example 3; Figure 3A graph showing the temperature variation over time of a floor heating system using the sound insulation layer provided in Example 4; Figure 4 A graph showing the temperature variation over time of a floor heating system using the sound insulation layer provided in Example 8; Figure 5 A graph showing the temperature variation over time of a floor heating system using the sound insulation layer provided in Example 9; Figure 6 A graph showing the temperature variation over time of a floor heating system using the sound insulation layer provided in Comparative Example 3; Figure 7 A graph showing the temperature variation over time of a floor heating system using the sound insulation layer provided in Example 10; Figure 8 This is a graph showing the temperature variation over time of a floor heating system using the sound insulation layer provided in Example 11.

[0027] Figure numerals: 1-first rubber particles, 2-second rubber particles, 3-phase change particles, 4-resin, 5-glass fiber, 100-sound insulation layer, 200-electric heating film layer, 300-heat equalizing layer, 400-finishing layer, 500-floor slab. DETAILED DESCRIPTION

[0028] The present invention is further described in detail below in conjunction with test examples and specific implementation methods. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following embodiments, and all technologies realized based on the content of the present invention belong to the scope of the present invention.

[0029] Unless otherwise specified, in the description of the specific embodiments of the present invention, the terms indicating the orientation or position relationship such as "up", "down", "left", "right", "center", "inside", "outside", etc. are all expressions based on the orientation or position relationship shown in the drawings, or the orientation or position relationship when the invented product / equipment / device is usually used. These terms of orientation or position relationship are only for the convenience of describing the scheme of the present invention or simplifying the description in the specific embodiments, so as to facilitate the technicians to quickly understand the scheme, rather than indicating or implying that a specific device / component / element must have a specific orientation, or be constructed and operated in a specific position relationship, and therefore cannot be understood as a limitation on the present invention.

[0030] In addition, if the terms "horizontal", "vertical", "overhanging", "parallel" and the like appear, it does not mean that the corresponding devices / components / elements are required to be absolutely horizontal or vertical or overhanging or parallel, but may be slightly tilted or have deviations. For example, "horizontal" only means that its direction is more horizontal than "vertical", and does not mean that the structure must be completely horizontal, but may be slightly tilted. Alternatively, it can be simplified to mean that the corresponding devices / components / elements are set in directions such as "horizontal", "vertical", "overhanging", "parallel", etc., and can have an error / deviation of ±10% relative to the corresponding direction setting, more preferably an error / deviation within ±8%, more preferably an error / deviation within ±6%, more preferably an error / deviation within ±5%, and more preferably an error / deviation within ±4%. As long as the corresponding device / component / element is within the error / deviation range, it can still achieve its role in the scheme of the present invention.

[0031] In addition, the expressions “first”, “second”, “third”, etc. that appear in the terms are merely descriptions used to distinguish the same or similar components and should not be understood as emphasizing or implying the relative importance of specific components.

[0032] In addition, in the description of the embodiments of the present invention, "several", "plurality" and "a number" represent at least 2. It can be any number such as 2, 3, 4, 5, 6, 7, 8, 9, and even more than 9.

[0033] In addition, in the description of the technical solution of the present invention, unless otherwise clearly specified / defined / restricted, the terms "set", "install", "connect", "connected", "provided with", "laid", and "arranged" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection, and can be welding, riveting, bolting, threading, and other commonly used connection means in the field. This connection can be a mechanical connection, an electrical connection, or a communication connection; it can be a direct connection, or an indirect connection through an intermediate medium, and it can be the internal connection of two elements.

[0034] Unless otherwise specified, in the description of the specific embodiments of the present invention, the mesh number refers to the number of holes on the screen per square inch. 50 mesh means 50 holes per square inch, and 500 mesh means 500 holes. The higher the mesh number, the more holes there are. In addition to indicating the holes of the screen, it is also used to indicate the particle size of particles that can pass through the screen. The higher the mesh number, the smaller the particle size. The present invention uses the US standard mesh number for comparison. For ease of use, an empirical conversion formula can also be used: particle size d (mm) = 16 / mesh number.

[0035] Example 1 like Figure 1A schematic diagram of the material of the new high-efficiency sound insulation layer 100 provided in this embodiment, the sound insulation layer 100 includes glass fiber 5 and a resin mixture mixed with the glass fiber 5. The resin mixture includes a first rubber particle 1 with a larger particle size, a phase change particle 3 with a second larger particle size, and a second rubber particle 2 with a smallest particle size, and the resin mixture also includes a resin 4. The particle size of the first rubber particle 1 is 40-60 mesh; the particle size of the second rubber particle 2 is 400-600 mesh; the sum of the mass of the first rubber particle 1 and the second rubber particle 2 accounts for 10wt%-30wt% of the whole material; the mass ratio of the first rubber particle 1 and the second rubber particle 2 is (0-2):5; the particle size of the phase change particle 3 is 90-110 mesh; the mass of the phase change particle 3 accounts for 35wt%-45wt% of the whole material; the mass of the resin 4 accounts for 5wt%-15wt% of the whole material.

[0036] In this embodiment, the preferred phase change particles 3 can be paraffin wrapped in a silica shell. Paraffin itself is a good phase change material. The introduction of the silica shell layer realizes the encapsulation of the phase change core material to prevent its leakage, while improving the overall thermal conductivity of the composite material, enhancing the thermal stability of the phase change material, and making the material have advantages such as flame retardancy, which greatly enhances the safety of the phase change particles 3.

[0037] In this embodiment, the resin 4 is preferably epoxy resin or polyurethane.

[0038] Furthermore, the sound insulation layer 100 provided in this embodiment is in the form of a long coiled material, and the width of the sound insulation layer 100 is 0.8m~1.2m, and more preferably the width of the sound insulation layer 100 is 1m. This arrangement is convenient for construction personnel to operate on the one hand, and can also cover the construction area to the maximum extent on the other hand, and achieve efficient laying. The length of the sound insulation layer 100 can be determined according to the actual construction situation; the thickness of the sound insulation layer 100 is 10mm~20mm, and more preferably the thickness of the sound insulation layer 100 is 10mm. This arrangement further optimizes the relationship between the thickness, sound insulation performance, and heat storage performance of the sound insulation layer 100, and can meet the sound insulation and heat insulation functions while not causing the total thickness of the entire floor heating system to be too high and affecting the indoor space utilization. The long coiled material design allows the sound insulation layer 100 to be rolled up and stored, with a small volume and convenient transportation. It can also be gradually unfolded and laid during on-site construction, and the operation is simple.

[0039] The sound insulation and heat preservation layer 100 provided in this embodiment is based on a glass fiber skeleton, and rubber particles (first rubber particles 1, second rubber particles 2) and organic phase change materials (phase change particles 3) are filled in the gaps of the glass fiber 5, wherein the first rubber particles 1 have a larger particle size and can fill the pores of the glass fiber skeleton over a large area, but in some small gaps, the second rubber particles 2 and phase change particles 3 with smaller particle sizes are required to be filled. The damping, shock absorption and sound insulation characteristics of rubber particles can effectively reduce the noise generated by the collision between floor slabs, and the phase change particles 3 can act as phase change energy storage materials, providing heat storage and heat release functions, thereby achieving the purpose of sound insulation and heat preservation at the same time. By specially limiting the particle sizes and ratios of the first rubber particles 1, the second rubber particles 2 and the phase change particles 3, the rubber particles and the phase change particles 3 are dispersed in the middle of the glass fiber 5 skeleton in an optimal ratio. That is, by adopting the particle size combination and ratio provided in this embodiment, it is possible to dissipate vibration energy to a greater extent and reduce the amount and cost of resin 4, thereby enabling the sound insulation layer 100 to have both sound insulation performance and heat storage performance within a relatively low thickness range.

[0040] It can be foreseen that the sound insulation and thermal insulation layer provided in this embodiment is not limited to floor heating applications, but can also be made into plates or coils and used as interlayers between building partitions or floor slabs to exert its excellent sound insulation and thermal insulation effects. For example, the sound insulation and thermal insulation layer can be directly pressed into plates as a component of dry partitions. Since it integrates sound insulation and thermal insulation functions, it can achieve better acoustic and thermal performance at the same thickness compared to traditional masonry partitions or gypsum board partitions; the sound insulation and thermal insulation layer can also be made into a coil form, which can be laid between floor structures, inside walls, etc., to act as an interlayer with composite functions. The coil is flexible, light in weight, and easy to construct; the sound insulation and thermal insulation are integrated to avoid the bloated structure caused by multi-layer superposition; of course, the material can also be used as a sound insulation and thermal insulation layer for floors. It can play the role of vibration isolation and noise reduction, and can effectively reduce the interference of walking noise upstairs on the downstairs. At the same time, the thermal insulation effect can create a more comfortable environment indoors. The sound insulation layer can also be made into ceiling or suspended ceiling sound-absorbing panels, which can not only have a beautifying effect, but also absorb indoor noise, improve the acoustic environment, and realize the integration of sound insulation and thermal insulation.

[0041] Example 2 The present embodiment provides a method for preparing a sound insulation layer, which is used to prepare the sound insulation layer 100 provided in Example 1. The method is improved from the traditional glass fiber wool preparation method, and comprises the following steps: spraying a resin mixture while spinning the glass fiber 5, and then pressing the glass fiber 5 mixed with the resin mixture into an integral body to form the sound insulation layer 100.

[0042] The traditional preparation method of glass fiber wool can be produced by the centrifugal technology commonly used in the industry. For example, glass fiber wool can use quartz sand or recycled glass as the main raw material, and add certain auxiliary materials, such as silicates, phosphates, etc. The main material and auxiliary materials are mixed in a certain proportion and stirred evenly, and then put into a kiln at about 1375℃ to melt them into liquid, cool them down and transport them to the centrifuge. Under the centrifugal force, the molten mixture will be thrown out into filaments, that is, the spinning process. At the same time, resin glue and a small amount of water are added, and the traditional glass fiber wool is obtained.

[0043] The method for preparing the sound insulation layer 100 provided in this embodiment is based on a glass fiber skeleton, and rubber particles (first rubber particles 1, second rubber particles 2) and organic phase change materials (phase change particles 3) are filled in the gaps between the glass fibers 5, so that the sound insulation layer 100 has both sound insulation performance and heat storage performance within a relatively low thickness range.

[0044] Example 3 like Figure 2 As shown, this embodiment provides a floor heating system, including the sound insulation layer 100 provided in Embodiment 1, the sound insulation layer 100 is laid on the floor 500, the electric heating film layer 200 is laid on the sound insulation layer 100, the heat absorbing layer 300 is laid on the electric heating film layer 200, and the finishing layer 400 is laid on the heat absorbing layer 300. In this embodiment, the heat absorbing layer 300 can be an aluminum plate heat absorbing layer, and the finishing layer 400 can be a wooden floor, a tile, a gypsum board, etc.

[0045] In the floor heating system provided in this embodiment, the sound insulation and thermal insulation layer 100 can be laid on the floor 500 and used as the sound insulation and thermal insulation layer of the electric floor heating. The rubber particles therein can effectively dissipate the noise energy generated by the impact of the floor 500 and reduce noise; the phase change particles 3 can store heat energy when the power is on, and slowly release heat after the power is off to maintain the temperature of the room. The entire system can continue to release the originally stored heat after the power is off to maintain the set temperature. Since the floor heating system has a small thickness and a simple structure, it can save the use area and achieve a rapid temperature response. Taking into account the peak and valley electricity prices, an intermittent electric heating method can be used to effectively reduce the cost of users. Example 4 Based on Example 1, this example provides the best particle size combination and ratio of the first rubber particles 1, the second rubber particles 2, and the phase change particles 3.

[0046] In this embodiment, the particle size of the first rubber particles 1 is 50 mesh, the particle size of the second rubber particles 2 is 500 mesh, the sum of the mass of the first rubber particles 1 and the second rubber particles 2 accounts for 30wt% of the whole material, and the mass ratio of the first rubber particles 1 to the second rubber particles 2 is 2:5; The particle size of the phase change particles 3 is 100 mesh, and the mass of the phase change particles 3 accounts for 40wt% of the whole material; The mass of the resin 4 accounts for 5wt% to 15wt% of the whole material, preferably the mass of the resin 4 accounts for 5wt% of the whole material, and the resin 4 is specifically epoxy resin; In the resin mixture, the mass ratio of the sum of the mass of the first rubber particles 1 and the second rubber particles 2 : the phase change particles 3 : the resin 4 is 6:8:1.

[0047] In this embodiment, the sound insulation layer 100 is in the form of a long coiled material, the width of the sound insulation layer 100 is 1 m, and the thickness of the sound insulation layer 100 is 10 mm.

[0048] This embodiment further optimizes the mass proportion of resin 4 and the mass ratio of rubber particles, phase change particles 3, and resin 4, dissipates vibration energy to the maximum extent, minimizes the amount of resin 4 and cost investment, and achieves the optimization among the thickness, sound insulation performance, and heat storage performance of the sound insulation layer 100.

[0049] Example 5 This embodiment is a variation of Embodiment 4: The particle size of the first rubber particles 1 is 50 meshes, the particle size of the second rubber particles 2 is 500 meshes, the sum of the mass of the first rubber particles 1 and the second rubber particles 2 accounts for 30wt% of the whole material, and the mass ratio of the first rubber particles 1 to the second rubber particles 2 is 1:5, that is, this embodiment focuses on adjusting the ratio of the first rubber particles 1 to the second rubber particles 2, and reducing the ratio of the first rubber particles 1; The particle size of the phase change particles 3 is 100 mesh, and the mass of the phase change particles 3 accounts for 40wt% of the whole material; The mass of resin 4 accounts for 10wt% of the whole material. The amount of resin 4 in this embodiment is increased. Resin 4 is specifically epoxy resin. In the resin mixture, the mass ratio of the sum of the mass of the first rubber particles 1 and the second rubber particles 2: the phase change particles 3: the resin 4 is 3:4:1.

[0050] Example 6 This embodiment is a variation of Embodiment 4: The particle size of the first rubber particles 1 is 50 meshes, the particle size of the second rubber particles 2 is 500 meshes, the sum of the mass of the first rubber particles 1 and the second rubber particles 2 accounts for 30wt% of the whole material, and the mass ratio of the first rubber particles 1 to the second rubber particles 2 is 0:5, that is, this embodiment focuses on adjusting the ratio of the first rubber particles 1 to the second rubber particles 2, and further reduces the ratio of the first rubber particles 1; The particle size of the phase change particles 3 is 100 mesh, and the mass of the phase change particles 3 accounts for 40wt% of the whole material; The mass of resin 4 accounts for 15wt% of the whole material. In this embodiment, the amount of resin 4 is further increased. Resin 4 is specifically epoxy resin. In the resin mixture, the mass ratio of the sum of the mass of the first rubber particles 1 and the second rubber particles 2: the phase change particles 3: the resin 4 is 6:8:3.

[0051] Example 7 This embodiment is a variation of Embodiment 4: The particle size of the first rubber particles 1 is 50 meshes, the particle size of the second rubber particles 2 is 500 meshes, and the sum of the mass of the first rubber particles 1 and the second rubber particles 2 accounts for 20wt% of the whole material, that is, the amount of rubber used is reduced in this embodiment, and the mass ratio of the first rubber particles 1 to the second rubber particles 2 is 2:5; The particle size of the phase change particles 3 is 100 mesh, and the mass of the phase change particles 3 accounts for 40wt% of the whole material; The mass of resin 4 accounts for 15wt% of the whole material, and resin 4 is specifically epoxy resin; In the resin mixture, the mass ratio of the sum of the mass of the first rubber particles 1 and the second rubber particles 2: the phase change particles 3: the resin 4 is 4:8:3.

[0052] Example 8 This embodiment is a variation of Embodiment 4: The particle size of the first rubber particles 1 is 50 meshes, the particle size of the second rubber particles 2 is 500 meshes, the sum of the mass of the first rubber particles 1 and the second rubber particles 2 accounts for 30wt% of the whole material, and the mass ratio of the first rubber particles 1 to the second rubber particles 2 is 2:5; The particle size of the phase change particles 3 is 100 meshes, and the mass of the phase change particles 3 accounts for 30wt% of the whole material, that is, the amount of the phase change particles 3 is reduced in this embodiment; The mass of resin 4 accounts for 5wt% of the whole material, and resin 4 is specifically epoxy resin; In the resin mixture, the mass ratio of the sum of the mass of the first rubber particles 1 and the second rubber particles 2 : the phase change particles 3 : the resin 4 is 6:6:1.

[0053] Example 9 This embodiment is a variation of Embodiment 4: The particle size of the first rubber particles 1 is 50 meshes, the particle size of the second rubber particles 2 is 500 meshes, the sum of the mass of the first rubber particles 1 and the second rubber particles 2 accounts for 30wt% of the whole material, and the mass ratio of the first rubber particles 1 to the second rubber particles 2 is 2:5; The particle size of the phase change particles 3 is 100 meshes, and the mass of the phase change particles 3 accounts for 50wt% of the whole material, that is, the amount of the phase change particles 3 is increased in this embodiment; The mass of resin 4 accounts for 10wt% of the whole material, that is, the amount of resin 4 is increased in this embodiment, and resin 4 is specifically epoxy resin; In the resin mixture, the mass ratio of the sum of the mass of the first rubber particles 1 and the second rubber particles 2 : the phase change particles 3 : the resin 4 is 3:5:1.

[0054] Example 10 This embodiment is a variation of Embodiment 4. The difference from Embodiment 4 is that in this embodiment, the thickness of the sound insulation layer 100 is 15 mm.

[0055] Embodiment 11 This embodiment is a variation of Embodiment 4. The difference from Embodiment 4 is that in this embodiment, the thickness of the sound insulation layer 100 is 20 mm.

[0056] Comparative Example 1 In this comparative example, only the first rubber particles 1 are provided, and the second rubber particles 2 are not provided. Specifically: The particle size of the first rubber particles 1 is 50 meshes, and the total mass of the first rubber particles 1 accounts for 30wt% of the entire material; The particle size of the phase change particles 3 is 100 mesh, and the mass of the phase change particles 3 accounts for 40wt% of the whole material; The mass of resin 4 accounts for 10wt% of the whole material, and resin 4 is specifically epoxy resin; In the resin mixture, the mass ratio of the sum of the mass of the first rubber particles 1: the phase change particles 3: the resin 4 is 3:4:1.

[0057] The sound insulation layer 100 is in the form of a long coiled material, the width of the sound insulation layer 100 is 1 m, and the thickness of the sound insulation layer 100 is 10 mm.

[0058] Comparative Example 2 In this comparative example, no sound insulation material is provided, that is, the first rubber particles 1 and the second rubber particles 2 are not provided in the resin mixture, and only the phase change particles 3 are added. Specifically: The particle size of the phase change particles 3 is 100 mesh, and the mass of the phase change particles 3 accounts for 40wt% of the whole material; The mass of resin 4 accounts for 5wt% of the whole material, and resin 4 is specifically epoxy resin.

[0059] The sound insulation layer 100 is in the form of a long coiled material, the width of the sound insulation layer 100 is 1 m, and the thickness of the sound insulation layer 100 is 10 mm.

[0060] Comparative Example 3 In this comparative example, no phase change material is provided, that is, no phase change particles 3 are provided in the resin mixture, and only the first rubber particles 1 and the second rubber particles 2 are added. Specifically: The particle size of the first rubber particles 1 is 50 meshes, the particle size of the second rubber particles 2 is 500 meshes, the sum of the mass of the first rubber particles 1 and the second rubber particles 2 accounts for 30wt% of the whole material, and the mass ratio of the first rubber particles 1 to the second rubber particles 2 is 2:5; The mass of resin 4 accounts for 5wt% of the whole material, and resin 4 is specifically epoxy resin.

[0061] In this embodiment, the sound insulation layer 100 is in the form of a long coiled material, the width of the sound insulation layer 100 is 1 m, and the thickness of the sound insulation layer 100 is 10 mm.

[0062] Comparison of sound insulation performance: In the same room, floor heating systems with sound insulation layers 100 provided by Examples 4 to 7, Examples 10 to 11, and Comparative Examples 1 to 2 are respectively laid, and the structure of the floor heating system adopts the floor heating structure provided by Example 3.

[0063] The floor impact sound insulation test was carried out in accordance with the fixed microphone position measurement method when the impactor is used as the impact source in "Acoustic Building and Building Component Sound Insulation Measurement Part 7: Field Measurement of Impact Sound Insulation" GB / T 19889.7-2022 / ISO 16283-2:2020. The experimental system is mainly composed of B&K2270 acoustic analyzer and microphone, B&K3207 standard impactor, B&K4231 acoustic calibrator and balloons. The sound insulation performance of the floor heating system corresponding to each sound insulation layer 100 is shown in Table 1. For the convenience of observation, we define the floor heating systems corresponding to the sound insulation layers 100 provided in Examples 4-7, 10-11 as Group A, Group B, Group C, Group D, Group E, and Group F respectively; the floor heating systems corresponding to the sound insulation layers 100 provided in Comparative Examples 1-2 are called Group A and Group B respectively.

[0064] Table 1 Sound insulation performance of floor heating system corresponding to each sound insulation layer 100 Group A Group B Group C Group D Group E Group F Group A Group B Impact sound pressure level (dB) 68 67 65 71 66 65 70 74 From the analysis of Table 1, it can be seen that whether or not rubber particles are added to the sound insulation layer 100 has a significant impact on the sound insulation effect of the entire system (for example, Group B corresponding to Comparative Example 2, which does not have the first rubber particles 1 and the second rubber particles 2, has the worst sound insulation performance). Because rubber has elasticity, when the sound insulation layer 100 is impacted, the energy can be dissipated through the damping effect of the rubber particles, thereby eliminating the noise generated by the impact vibration.

[0065] By comparing the results of Group A corresponding to Example 4, Group B corresponding to Example 5, and Group C corresponding to Example 6, it can be seen that as the amount of large rubber particles (first rubber particles 1) decreases, the sound insulation effect becomes better. The main reason for this is that when the rubber particles are impacted and vibrate, they compress and dissipate part of the energy, and friction also occurs between the rubber particles, further dissipating energy. Therefore, the smaller the rubber particle size, the more friction is generated between the rubber particles, and the more energy can be consumed. The final effect presented is better sound insulation performance. However, the smaller the particle size of the rubber particles, the more resin 4 is needed to bond it to the glass fiber 5 into a plate-like structure, resulting in a significant increase in the amount of resin 4 (for example, the amount of resin 4 in Group A to Group C gradually increases), and the fire resistance of the material decreases.

[0066] The sound insulation effect of group B is the best, but the amount of resin 4 in Example 5 corresponding to group B is increased, and the fireproof performance of the material is reduced.

[0067] By comparing the results of Group A and Group D, it can be seen that the reduction in the total amount of rubber (first rubber particles 1, second rubber particles 2) will reduce the vibration energy generated by the impact that can be dissipated, which will also lead to a reduction in the sound insulation effect.

[0068] By comparing Group A corresponding to Example 4, Group E corresponding to Example 10, and Group F corresponding to Example 11, it can be seen that as the thickness of the sound insulation layer 100 increases, the sound insulation performance of the entire system is improved. However, even if the sound insulation layer 100 with a thickness of 10 mm has met the current national requirements, it can also meet the high standards of developed countries. If the thickness of the sound insulation layer 100 is further increased, on the one hand, unnecessary costs will be increased, and on the other hand, the total thickness of the entire floor heating system will be too high, affecting the utilization of indoor space.

[0069] Therefore, Group A corresponding to Example 4 is the best group in terms of comprehensive cost, space, and sound insulation performance.

[0070] Comparison of thermal insulation performance: In the same room, floor heating systems with the sound insulation layer 100 provided by Example 4, Example 8 to Example 11, and Comparative Example 3 are respectively laid, and the structure of the floor heating system adopts the floor heating structure provided by Example 3.

[0071] The outdoor ambient temperature is 10℃, and the heating is turned on intermittently for 4 hours. Considering the peak and valley electricity prices, the power is turned on from 22:00-2:00, 6:00-10:00, and 14:00-18:00, and the power is turned off from 2:00-6:00, 10:00-14:00, and 18:00-22:00. The temperature is set to 22℃, and the indoor temperature changes are monitored. Figure 3-Figure 8 The temperature variation over time of the floor heating system corresponding to different sound insulation layers 100 is shown.

[0072] from Figure 3-Figure 6 It can be seen that when a phase change material is added to the sound insulation layer 100 (for example Figure 3 , Figure 5 As shown in the figure, the temperature drops slowly after power failure and can be maintained near the set temperature. When power is restored, the temperature can rise quickly. Since the temperature difference changes little after power failure, when power is restored, only a small amount of electricity is needed to return to the set temperature.

[0073] When there is no phase change material (e.g. Figure 6 As shown, in comparative example 3, no phase change material is provided, that is, no phase change particles 3 are provided in the resin mixture, and its thermal insulation performance is the worst) or there is less phase change material (for example Figure 4 The sound insulation layer 100 provided in the embodiment 8 shown reduces the amount of phase change particles 3 used. When the power is turned off, the temperature drops rapidly to near room temperature. When the power is turned on, it can rise rapidly. However, the temperature difference during this period is large, so the power consumption doubles.

[0074] from Figure 3 , Figure 7-Figure 8 It can be seen that the change in the thickness of the sound insulation layer 100 has little effect on the temperature change after power failure and can be ignored to a certain extent.

[0075] therefore Figure 3 The floor heating system with the sound insulation layer 100 provided in the fourth embodiment shown is the best one in terms of comprehensive cost, space, sound insulation and thermal insulation performance.

[0076] The above-mentioned intermittent power-on mode can be uniformly controlled by a control panel, and the heating power can vary with the temperature difference (in order to quickly heat up to the set temperature, the greater the temperature difference, the higher the heating power and the greater the power consumption).

[0077] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A sound insulation layer (100), It is characterized in that It comprises glass fibers (5) and a resin mixture mixed with the glass fibers (5), wherein the resin mixture comprises first rubber particles (1), second rubber particles (2), phase change particles (3), and resin (4); The particle size of the first rubber particles (1) is 40-60 mesh; The particle size of the second rubber particles (2) is 400-600 mesh; The sum of the mass of the first rubber particles (1) and the second rubber particles (2) accounts for 10wt% to 30wt% of the entire material; The mass ratio of the first rubber particles (1) to the second rubber particles (2) is 0-2:5; The particle size of the phase change particles (3) is 90-110 mesh; The mass of the phase change particles (3) accounts for 35wt% to 45wt% of the entire material; The mass of the resin (4) accounts for 5wt% to 15wt% of the entire material.

2. The sound insulation layer (100) according to claim 1, It is characterized in that The particle size of the first rubber particles (1) is 50 mesh, the particle size of the second rubber particles (2) is 500 mesh, the sum of the mass of the first rubber particles (1) and the second rubber particles (2) accounts for 30wt% of the whole material, the mass ratio of the first rubber particles (1) to the second rubber particles (2) is 2:5, the particle size of the phase change particles (3) is 100 mesh, the mass of the phase change particles (3) accounts for 40wt% of the whole material, and the mass of the resin (4) accounts for 5wt%~15wt% of the whole material.

3. The sound insulation layer (100) according to claim 2, It is characterized in that The mass of the resin (4) accounts for 5wt% of the entire material. In the resin mixture, the mass ratio of the sum of the mass of the first rubber particles (1) and the second rubber particles (2): the phase change particles (3): the resin (4) is 6:8:

1.

4. The sound insulation layer (100) according to claim 1, It is characterized in that The phase change particles (3) are paraffin wrapped in a silicon dioxide shell.

5. The sound insulation layer (100) according to claim 1, It is characterized in that The resin (4) is epoxy resin or polyurethane.

6. The sound insulation layer (100) according to claim 1, It is characterized in that The sound insulation and thermal insulation layer (100) is in the form of a long coiled material, the width of the sound insulation and thermal insulation layer (100) is 0.8m-1.2m, and the thickness of the sound insulation and thermal insulation layer (100) is 10mm-20mm.

7. The sound insulation layer (100) according to claim 6, It is characterized in that The width of the sound insulation and thermal insulation layer (100) is 1 m, and the thickness of the sound insulation and thermal insulation layer (100) is 10 mm.

8. A method for preparing a sound insulation layer, It is characterized in that A method for manufacturing a sound insulation layer (100) as claimed in any one of claims 1 to 7 comprises the following steps: While the glass fibers (5) are being spinned, the resin mixture is sprayed, and then the mixture is pressed into an integral shape.

9. A floor heating system, It is characterized in that The invention comprises a sound insulation and heat preservation layer (100) as claimed in any one of claims 1 to 7, wherein an electric heating film layer (200) is laid on the sound insulation and heat preservation layer (100), a heat equalization layer (300) is laid on the electric heating film layer (200), and a finishing layer (400) is laid on the heat equalization layer (300).

10. A floor heating system according to claim 9, It is characterized in that The heat-spreading layer (300) is an aluminum plate heat-spreading layer.

Citation Information

Cited By

  • High-thermal-conductivity glass fiber reinforced phase change laminated plate and preparation method thereof

    CN120756156A