Automobile rear windshield electric heating coating and preparation method thereof
By using combined materials such as polyester resin and modified particles in electric heating coatings, the composite modified particles and microsphere-like structures are formed, which solves the weather resistance and light resistance of the coating on the rear windshield of the automobile, significantly improving the quality of the coating. The waterproof and aging resistance of the paint meet the higher requirements of the automotive industry for the performance of electric heating coatings.
Patent Information
- Application Number
- CN202411109725.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The existing electric heating coatings have insufficient performance in terms of weather resistance, temperature resistance, light resistance and aging resistance in automotive rear windshield applications, which cannot meet the further demand of the automotive industry for electric heating coatings.
Using a combination of polyester resin, modified particles, dispersant, leveling agent, curing agent and functional additive, the formation of composite modified particles and microsphere-like structures will enhance electron flowability and surface roughness, and limit the formation of hydrated layer. , improve the maintenance rate of electrons and holes, and enhance the absorption capacity of light.
On the basis of maintaining the electric heating performance, the light resistance, water resistance and aging resistance of the paint are significantly improved, meeting the higher requirements for the performance of the electric heating coating in the rear gear of the car, and have excellent application prospects.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the field of electric heating coatings, and in particular to an electric heating coating for a rear windshield of an automobile and a preparation method thereof. Background Art
[0002] As an emerging technology, electric heating paint has shown its unique application value in many fields. Such paints usually contain conductive materials and can generate heat when current passes through them. They are widely used in the fields of automobiles, construction, aerospace, etc. to achieve functions such as deicing, anti-fogging, heating, etc.
[0003] Before the emergence of electric heating paint, traditional heating methods mostly relied on metal heating elements or resistance wires, which are not only complicated to install, but also heavy and not suitable for occasions with high demand for lightweight design. In the 1980s, with the discovery and in-depth research of conductive polymers, scientists began to explore the application of such materials in coatings to achieve the heating function of the coating. After entering the 21st century, with the development of nanotechnology, various nanomaterials have been introduced into electric heating paint, significantly improving the electric heating performance and thermal stability of the paint.
[0004] In recent years, with the development of science and technology, especially the continuous improvement of the level of the automobile industry, the functional requirements for electric heating coatings are also constantly changing. For example, in order to meet the requirements of transparency, anti-fog and deicing of automobile rear windshields (referred to as automobile rear windshields), the application of electric heating coatings is becoming more and more frequent. Although the existing electric heating coatings can meet the requirements of transparency and electric heating of automobile rear windshields, they always have performance deficiencies in weather resistance, temperature resistance, light resistance, waterproofness and aging resistance.
[0005] Therefore, in order to solve the above problems, the present application provides an electric heating paint for automobile rear windshield and a preparation method thereof. The electric heating paint for automobile rear windshield prepared in the present application not only has good transparency and electric heating properties, but also can maintain good light resistance, waterproofness, temperature resistance and aging resistance on this basis, which greatly meets the further demand for the performance of electric heating paint for existing automobile rear windshields and has very excellent application prospects. Summary of the invention
[0006] In order to solve the above problems, the first aspect of the present application provides an electric heating paint for the rear windshield of an automobile. The raw materials, calculated by mass, are: 30 to 50 parts of polyester resin, 12 to 25 parts of modified particles, 4 to 8 parts of dispersant, 1 to 2 parts of leveling agent, 2 to 4 parts of curing agent, 5 to 15 parts of functional additives, and 40 to 60 parts of solvent.
[0007] As a preferred solution, the mass ratio of the polyester resin, modified particles and dispersant is (4-5): (1.4-2): (0.5-0.7).
[0008] As a preferred solution, the mass ratio of the polyester resin, the modified particles and the dispersant is (4-4.5): (1.5-1.8): (0.5-0.6).
[0009] As a preferred solution, the mass ratio of the modified particles to the functional additives is (1.4-2): (0.9-1.2).
[0010] As a preferred solution, the polyester resin is an unsaturated polyester resin.
[0011] As a preferred solution, the viscosity of the polyester resin is 2000-4000 cP, and the test condition is 25°C.
[0012] As a preferred solution, the viscosity of the polyester resin is 2500-3500 cP, and the test condition is 25°C.
[0013] As a preferred solution, the light transmittance of the polyester resin is 90-95%, and the test conditions are: wavelength 550nm.
[0014] As a preferred solution, the preparation method of the modified particles comprises the following steps: S1: adding zinc nitrate hexahydrate, 2,5-dihydroxyterephthalic acid and acetic acid to a DMF solution and mixing evenly, first heating to 50-60°C for a short period of 20-25 minutes, then heating to 120-130°C, stirring at 100-150 rpm for 20-24 hours; S2: after the reaction is completed, cooling to 60-70°C, first adding succinic anhydride and silane coupling agent, stirring at 40-80 rpm for 5-6 hours, and adding dropwise a DMF solution mixed with titanium dioxide and nano-graphite powder within 1-1.5 hours after the start of the reaction; S3: after the reaction in S2 is completed, heating to 120-130°C for a second time, stirring at 60-90 rpm for 10-15 hours, cooling naturally to room temperature after the reaction is completed, centrifuging, washing the product with methanol, and vacuum drying at 80-90°C to obtain the product.
[0015] As a preferred solution, the mass ratio of zinc nitrate hexahydrate, 2,5-dihydroxyterephthalic acid, acetic acid and nano-graphite powder is (0.8-1): (1.5-2): (8-10): (3.5-4).
[0016] As a preferred solution, the mass ratio of succinic anhydride, silane coupling agent, titanium dioxide and nano-graphite powder is (1.8-2): (0.5-0.7): (0.8-1.2): (3.5-4).
[0017] As a preferred solution, the silane coupling agent is γ-glycidyloxypropyltrimethoxysilane.
[0018] As a preferred solution, the average particle size of the nano graphite powder is 50-100 nm.
[0019] As a preferred solution, the average particle size of the nano graphite powder is 60-80 nm.
[0020] As a preferred solution, the average particle size of the titanium dioxide is 5-10 nm.
[0021] As a preferred solution, the average particle size of the modified particles is 550-650 nm.
[0022] By adding the above-mentioned modified particles in the present application, the light resistance, water resistance and aging resistance of the electric heating coating can be greatly improved under the premise of effectively maintaining the transparency and electric heating properties of the electric heating coating. Firstly, the composite modified particles prepared in the present application can form a fixed structure with the framework particles as the center, and graphite powder and titanium dioxide attached and adhered. The existence of this structure can form a stable electron path between the three particles through hydrogen bonds and coordination. The existence of this path can greatly increase the length of the flow path of electrons inside the coating, enhance the efficiency of electron flow, and thus strengthen the mobility of electrons in the coating system to a certain extent, and control the resistance range of the overall coating through the overall microsphere-like structure of the composite modified particles, thereby ensuring good electric heating performance.
[0023] Secondly, the formed microsphere-like structure can enhance the surface roughness enhancement effect of the surface particles on the coating system. After the coating is coated and cured, the microsphere-like structure can cause a relatively regular continuous peak-valley structure to form on the coating surface. The existence of this structure can greatly reduce the formation rate of the hydration layer on the coating surface and limit the combination of the local hydration layer on the surface, thereby greatly reducing the hydrophilicity of the coating surface and reducing the efficiency of water molecule invasion, thereby obtaining excellent waterproof and aging resistance. Finally, the composite modified particles form a composite structure to form a similar heterojunction structure. The existence of this structure can greatly help enhance the maintenance rate of electrons and holes in the composite modified particles, thereby reducing its bandgap distance, effectively enhancing its ability to absorb ultraviolet light, and thereby obtaining excellent light resistance.
[0024] As a preferred solution, the dispersant is at least one of acrylates, phosphates, and fatty alcohol polyoxyethylene ethers.
[0025] As a preferred solution, the dispersant is a composition of alkylphenyl phosphate and cetearyl alcohol polyoxyethylene ether.
[0026] As a preferred embodiment, the mass ratio of the alkylphenyl phosphate to the cetearyl alcohol polyoxyethylene ether is (2-3): (1-1.5).
[0027] As a preferred solution, the hydroxyl value of the cetearyl alcohol polyoxyethylene ether is 80-120 mgKOH / g.
[0028] As a preferred solution, the leveling agent is a silicone leveling agent or a polyurethane leveling agent.
[0029] As a preferred solution, the leveling agent is a silicone leveling agent.
[0030] As a preferred solution, the curing agent is at least one of methyl ethyl ketone peroxide, benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, cumene hydroperoxide, diphenylmethane diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, and hexamethylene diisocyanate.
[0031] As a preferred solution, the curing agent is a combination of benzoyl peroxide and diphenylmethane diisocyanate.
[0032] As a preferred solution, the mass ratio of benzoyl peroxide to diphenylmethane diisocyanate is (4-5): (0.5-1).
[0033] As a preferred solution, the functional auxiliary agent is a composition of epoxy block, pullulan and sodium carboxymethyl cellulose.
[0034] As a preferred solution, the mass ratio of the epoxy block, pullulan and sodium carboxymethyl cellulose is (2.5-3.5): (5-7): (1.5-2).
[0035] As a preferred solution, the mass ratio of the epoxy block, pullulan and sodium carboxymethyl cellulose is (2.8-3.2): (6-6.5): (1.6-1.8).
[0036] As a preferred solution, the epoxy block material is an ethylene oxide-propylene oxide block copolymer.
[0037] As a preferred solution, the epoxy block is a composition of an ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 2500-3000 and an ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 7500-8500, and the mass ratio of the two is (5-6.5):(1.1-2.2).
[0038] As a preferred solution, the branched chain content of the amylopectin is 70-75%.
[0039] The epoxy block, pullulan and sodium carboxymethyl cellulose compound added in the present application can help improve the waterproof, aging and light resistance properties of the electric heating coating. The above-mentioned compounding scheme added in the present application can, firstly, effectively remove and preserve the trace moisture remaining in the coating through the water-retaining effect of sodium carboxymethyl cellulose, limit the diffusion of water molecules, and thus help increase the penetration resistance of water molecules to the coating; secondly, the pseudoplastic fluid effect of sodium carboxymethyl cellulose enhances the dispersion effect of epoxy block and branched starch in the coating system, and at this time, epoxy block with different molecular weight can form an overlapping film layer structure on the surface of the modified particles. The presence of this structure reduces the attraction between the modified particles, thereby avoiding the strong agglomeration phenomenon after the surface treatment, and branched starch can work together with sodium carboxymethyl cellulose, through its multi-branched molecular chain structure, to strengthen the connection and entanglement between the internal molecules and the molecular chains of the polyester resin, enhance the intermolecular force, and thus make the heated coating form a more dense internal three-dimensional network structure. The presence of this dense structure reduces the contact frequency of active molecules and groups in the internal system of the coating, reduces the reaction probability, and thus greatly improves the coating performance.
[0040] As a preferred solution, the solvent is isopropanol.
[0041] The second aspect of the present application provides a method for preparing the above-mentioned electric heating coating for the rear windshield of an automobile, which specifically comprises the following steps: S1: mixing the modified particles and the dispersant and adding them to the polyester resin, and dispersing them at a high speed of 400-450 rpm in a high-speed disperser for 15-20 minutes; S2: then adding a solvent containing a leveling agent and a functional additive, and continuing to disperse at a high speed for 40-50 minutes; S3: adding a curing agent after the dispersion is completed, and stirring at a speed of 60-120 rpm for 10-15 minutes to obtain the coating.
[0042] The beneficial effects of this application are:
[0043] 1. The electric heating coating for the rear window of an automobile provided in the present application not only has good transparency and electric heating properties, but also can maintain good light resistance, water resistance, temperature resistance and aging resistance on this basis, which greatly meets the further demand for the performance of the electric heating coating for the rear window of an existing automobile, and has very excellent application prospects.
[0044] 2. The electric heating paint for the rear windshield of an automobile provided in the present application can significantly improve the light resistance, water resistance and aging resistance of the electric heating paint while effectively maintaining the transparency and electric heating properties of the electric heating paint by adding modified particles; the composite modified particles prepared in the present application can form a fixed structure with the framework particles as the center and graphite powder and titanium dioxide attached and adhered. The existence of this structure can form a stable electron path between the three particles through hydrogen bonds and coordination. The existence of this path can significantly increase the length of the flow path of electrons inside the paint and enhance the electron flow efficiency, thereby enhancing the mobility of electrons in the paint system to a certain extent, and the overall resistance range of the paint is controlled by the overall microsphere-like structure of the composite modified particles.
[0045] 3. In the electric heating coating for the rear windshield of an automobile provided in the present application, the microsphere-like structure formed by the modified particles can enhance the surface roughness enhancement effect of the surface particles on the coating system. After the coating is coated and cured, the microsphere-like structure can cause a relatively regular continuous peak-valley structure to form on the coating surface. The existence of this structure can greatly reduce the formation speed of the hydration layer on the coating surface and limit the combination of local hydration layers on the surface, thereby greatly reducing the hydrophilicity of the coating surface and reducing the efficiency of water molecule intrusion, thereby obtaining excellent waterproof and aging resistance.
[0046] 4. The electric heating paint for the rear windshield of an automobile provided in the present application can effectively remove and preserve the trace moisture remaining in the paint through the water-retaining effect of sodium carboxymethyl cellulose, limit the diffusion of water molecules, and thus help increase the penetration resistance of water molecules to the paint; on the other hand, the pseudoplastic fluid effect of sodium carboxymethyl cellulose enhances the dispersion effect of epoxy block and amylopectin in the paint system, and at this time, epoxy block with different molecular weights can form an overlapping film structure on the surface of modified particles. The existence of this structure reduces the attraction between the modified particles, thereby avoiding the strong agglomeration phenomenon after the surface treatment, and amylopectin can work together with sodium carboxymethyl cellulose to strengthen the connection and entanglement between the internal molecules and the molecular chains of the polyester resin through its multi-branched molecular chain structure, thereby enhancing the intermolecular force. DETAILED DESCRIPTION
[0047] The following will further explain and demonstrate the technical solutions in the above invention content of this application in the form of specific implementation schemes. The following embodiments are only practical examples used to illustrate and explain the contents of the technical solutions in the specification, and should not limit the scope of the claims to be protected by this application. All technical products based on the technical solutions described in the invention content of this application should be included in the scope to be protected by this application.
[0048] In the following examples, unless otherwise specified, the raw materials are all commercially available products, or can be prepared by methods well known to those skilled in the art.
[0049] Example 1
[0050] Example 1 The first aspect provides an electric heating paint for the rear windshield of an automobile. The raw materials are, by mass, 44.5 parts of polyester resin, 17.6 parts of modified particles, 6 parts of dispersant, 1.8 parts of leveling agent, 3.2 parts of curing agent, 10.5 parts of functional additives, and 55 parts of solvent.
[0051] The polyester resin is an unsaturated polyester resin, and its viscosity is 3200 cP, and the test condition is 25°C. Its transmittance is 91.2%, and the test condition is a wavelength of 550nm. It is a product with corresponding properties purchased from Tianjin Aobang Resin Co., Ltd.
[0052] The preparation method of the modified particles comprises the following steps, calculated by mass: S1: adding 0.95 parts of zinc nitrate hexahydrate, 1.82 parts of 2,5-dihydroxyterephthalic acid and 10 parts of acetic acid to 80 parts of DMF solution and mixing evenly, first heating to 55°C for a short heat preservation of 25 minutes, then heating to 125°C, stirring at 120 rpm for reaction for 22 hours; S2: after the reaction is completed, cooling to 65°C, first adding 1.85 parts of succinic anhydride and 0.55 parts of γ-glycidyloxypropyltrimethoxysilane, stirring at 60 rpm for heat preservation for 5.5 hours, and within 1 hour after the start of the reaction, adding dropwise 0.9 parts of titanium dioxide and 3.8 parts of nano-graphite powder mixed DMF solution (60 parts in total); S3: after the reaction of S2 is completed, heating to 125°C for a second time, stirring at 80 rpm for reaction for 14 hours, cooling naturally to room temperature after the reaction is completed, centrifugal filtration, washing the product with methanol, and vacuum drying at 90°C to obtain the product.
[0053] The average particle size of nanographite powder is 78 nm, and the corresponding particle size product was purchased from Xuzhou Jie Innovation Materials Technology Co., Ltd.
[0054] The average particle size of titanium dioxide is 5 nm, and the corresponding particle size product was purchased from Hubei Langbowan Biomedicine Co., Ltd.
[0055] The average particle size of the modified particles was 587 nm.
[0056] The dispersant is a composition of alkylphenyl phosphate and cetearyl alcohol polyoxyethylene ether, with a mass ratio of 2.5:1.2; cetearyl alcohol polyoxyethylene ether was purchased from the O-9 product sold by Hai'an Guoyun Chemical Co., Ltd., and its hydroxyl value is 86 mgKOH / g.
[0057] Alkylphenyl phosphate was purchased from dialkylphenyl phosphate products sold by Hubei Chengfeng Chemical Co., Ltd.
[0058] The leveling agent is silicone leveling agent BYK-333.
[0059] The curing agent is a composition of benzoyl peroxide and diphenylmethane diisocyanate, and the mass ratio of the two is 4.2:0.8.
[0060] The functional additive is a composition of epoxy block, pullulan and sodium carboxymethyl cellulose, and the mass ratio of the three is 3:6.2:1.8.
[0061] The epoxy block material is a composition of an ethylene oxide-propylene oxide block copolymer (BASF L64) with a weight average molecular weight of 2900 and an ethylene oxide-propylene oxide block copolymer (BASF L87) with a weight average molecular weight of 7800, and the mass ratio of the two is 5.8:1.5.
[0062] The branched chain content of amylopectin was 72%, and it was purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd.
[0063] The solvent is isopropyl alcohol.
[0064] The second aspect of the present embodiment provides a method for preparing the above-mentioned electric heating coating for the rear windshield of an automobile, which specifically includes the following steps: S1: mixing the modified particles and the dispersant and adding them to the polyester resin, and dispersing them at a high speed of 450 rpm in a high-speed disperser for 20 minutes; S2: then adding a solvent containing a leveling agent and a functional additive, and continuing to disperse at a high speed for 45 minutes; S3: adding a curing agent after the dispersion is completed, and stirring at a speed of 90 rpm for 15 minutes to obtain the coating.
[0065] Example 2
[0066] Example 2 The first aspect provides an electric heating paint for the rear windshield of an automobile. The raw materials, calculated by mass, are: 45 parts of polyester resin, 14.2 parts of modified particles, 5.2 parts of dispersant, 1.5 parts of leveling agent, 3.2 parts of curing agent, 10.5 parts of functional additives, and 55 parts of solvent.
[0067] The polyester resin is an unsaturated polyester resin, and its viscosity is 3200 cP, and the test condition is 25°C. Its transmittance is 91.2%, and the test condition is a wavelength of 550nm. It is a product with corresponding properties purchased from Tianjin Aobang Resin Co., Ltd.
[0068] The preparation method of the modified particles comprises the following steps, calculated by mass: S1: adding 0.95 parts of zinc nitrate hexahydrate, 1.82 parts of 2,5-dihydroxyterephthalic acid and 10 parts of acetic acid to 80 parts of DMF solution and mixing evenly, first heating to 55°C for a short heat preservation of 25 minutes, then heating to 125°C, stirring at 120 rpm for reaction for 22 hours; S2: after the reaction is completed, cooling to 65°C, first adding 1.85 parts of succinic anhydride and 0.55 parts of γ-glycidyloxypropyltrimethoxysilane, stirring at 60 rpm for heat preservation for 5.5 hours, and within 1 hour after the start of the reaction, adding dropwise 0.9 parts of titanium dioxide and 3.8 parts of nano-graphite powder mixed DMF solution (60 parts in total); S3: after the reaction of S2 is completed, heating to 125°C for a second time, stirring at 80 rpm for reaction for 14 hours, cooling naturally to room temperature after the reaction is completed, centrifugal filtration, washing the product with methanol, and vacuum drying at 90°C to obtain the product.
[0069] The average particle size of nanographite powder is 78 nm, and the corresponding particle size product was purchased from Xuzhou Jie Innovation Materials Technology Co., Ltd.
[0070] The average particle size of titanium dioxide is 5 nm, and the corresponding particle size product was purchased from Hubei Langbowan Biomedicine Co., Ltd.
[0071] The average particle size of the modified particles was 587 nm.
[0072] The dispersant is a composition of alkylphenyl phosphate and cetearyl alcohol polyoxyethylene ether, with a mass ratio of 3:1; cetearyl alcohol polyoxyethylene ether was purchased from the O-9 product sold by Hai'an Guoyun Chemical Co., Ltd., and its hydroxyl value is 86 mgKOH / g.
[0073] Alkylphenyl phosphate was purchased from dialkylphenyl phosphate products sold by Hubei Chengfeng Chemical Co., Ltd.
[0074] The leveling agent is silicone leveling agent BYK-333.
[0075] The curing agent is a composition of benzoyl peroxide and diphenylmethane diisocyanate, and the mass ratio of the two is 4:1.
[0076] The functional additive is a composition of epoxy block, pullulan and sodium carboxymethyl cellulose, and the mass ratio of the three is 3.4:5.5:1.5.
[0077] The epoxy block material is a composition of an ethylene oxide-propylene oxide block copolymer (BASF L64) with a weight average molecular weight of 2900 and an ethylene oxide-propylene oxide block copolymer (BASF L87) with a weight average molecular weight of 7800, and the mass ratio of the two is 5.8:1.5.
[0078] The branched chain content of amylopectin was 72%, and it was purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd.
[0079] The solvent is isopropyl alcohol.
[0080] The second aspect of the present embodiment provides a method for preparing the above-mentioned electric heating coating for the rear windshield of an automobile, which specifically includes the following steps: S1: mixing the modified particles and the dispersant and adding them to the polyester resin, and dispersing them at a high speed of 450 rpm in a high-speed disperser for 20 minutes; S2: then adding a solvent containing a leveling agent and a functional additive, and continuing to disperse at a high speed for 45 minutes; S3: adding a curing agent after the dispersion is completed, and stirring at a speed of 90 rpm for 15 minutes to obtain the coating.
[0081] Comparative Example 1
[0082] The specific implementation method of this comparative example is basically the same as that of Example 1, except that: the raw materials of the electric heating paint for the rear windshield of an automobile, in parts by mass, are: 60 parts of polyester resin, 7.5 parts of modified particles, 4.2 parts of dispersant, 1.8 parts of leveling agent, 3.2 parts of curing agent, 10.5 parts of functional additives, and 55 parts of solvent.
[0083] Comparative Example 2
[0084] The specific implementation method of this comparative example is basically the same as that of Example 1, except that: the raw materials of the electric heating paint for the rear windshield of an automobile, in parts by mass, are: 50.5 parts of polyester resin, 28.5 parts of modified particles, 6 parts of dispersant, 1.8 parts of leveling agent, 3.2 parts of curing agent, 4.5 parts of functional additives, and 55 parts of solvent.
[0085] Comparative Example 3
[0086] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified particles comprises the following steps, calculated by mass: S1: 0.35 parts of zinc nitrate hexahydrate, 0.95 parts of 2,5-dihydroxyterephthalic acid and 4.5 parts of acetic acid are added to 60 parts of DMF solution and mixed evenly, first heated to 55°C for a short time for 25 minutes, then heated to 125°C, stirred at 120 rpm for 22 hours; S2: after the reaction is completed, the temperature is lowered to 65°C, 1 .85 parts of succinic anhydride and 0.55 parts of γ-glycidyloxypropyltrimethoxysilane are stirred at 60 rpm for 5.5 hours, and within 1 hour after the start of the reaction, 0.9 parts of titanium dioxide and 3.8 parts of nano-graphite powder mixed DMF solution (60 parts in total) are added dropwise; S3: after the reaction of S2 is completed, the temperature is raised to 125°C for the second time, and the reaction is stirred at 80 rpm for 14 hours. After the reaction is completed, it is naturally cooled to room temperature, centrifuged and filtered, the product is washed with methanol, and vacuum dried at 90°C to obtain S3.
[0087] The average particle size of the modified particles is 324 nm.
[0088] Comparative Example 4
[0089] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified particles comprises the following steps, calculated by mass: S1: 0.95 parts of zinc nitrate hexahydrate, 1.82 parts of 2,5-dihydroxyterephthalic acid and 10 parts of acetic acid are added to 80 parts of DMF solution and mixed evenly, first heated to 55°C for a short time for 25 minutes, then heated to 125°C, stirred at 120 rpm for 22 hours; S2: after the reaction is completed, the temperature is lowered to 65°C, 1.82 parts of 2,5-dihydroxyterephthalic acid and 10 parts of acetic acid are added to 80 parts of DMF solution, and the mixture is ...3: after the reaction is completed, the temperature is lowered to 65°C, 1.82 parts of 2,5-dihydroxyterephthalic acid and 10 parts of acetic acid are added to 80 parts of DMF solution, and the mixture is mixed evenly, first heated to 55°C for a short time for 25 minutes, then heated to 125°C, stirred at 120 rpm for 22 hours; S4: after the reaction is completed, the temperature is lowered to 65°C, 1.82 parts of 2,5- .2 parts of succinic anhydride and 0.2 parts of γ-glycidyloxypropyltrimethoxysilane, stir and keep warm at 60rpm for 5.5h, and within 1h after the start of the reaction, add 0.45 parts of titanium dioxide and 4.5 parts of nano-graphite powder mixed DMF solution (a total of 80 parts) dropwise; S3: after the reaction of S2 is completed, heat it to 125℃ for the second time, stir at 80rpm for 14h, cool it naturally to room temperature after the reaction is completed, centrifuge and filter, wash the product with methanol, and dry it in vacuum at 90℃ to obtain S3.
[0090] The average particle size of the modified particles is 746 nm.
[0091] Comparative Example 5
[0092] The specific implementation of this comparative example is basically the same as that of Example 1, except that the average particle size of the nanographite powder is 120 nm, and the corresponding particle size product is purchased from Xuzhou Jie Innovation Materials Technology Co., Ltd.
[0093] The average particle size of titanium dioxide is 25 nm, and the corresponding particle size product was purchased from Hubei Langbowan Biomedicine Co., Ltd.
[0094] The average particle size of the modified particles was 814 nm.
[0095] Comparative Example 6
[0096] The specific implementation of this comparative example is basically the same as that of Example 1, except that the dispersant is a composition of alkylphenyl phosphate and cetearyl alcohol polyoxyethylene ether, and the mass ratio of the two is 5:0.4.
[0097] Comparative Example 7
[0098] The specific implementation of this comparative example is basically the same as that of Example 1, except that the functional additive is a combination of epoxy block, pullulan and sodium carboxymethyl cellulose, and the mass ratio of the three is 1:8:0.5.
[0099] Comparative Example 8
[0100] The specific implementation of this comparative example is basically the same as that of Example 1, except that the epoxy block material is a composition of an ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 2900 (BASF L64) and an ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 7800 (BASF L87), and the mass ratio of the two is 2:1.
[0101] Performance Evaluation
[0102] Resistance performance: The resistance of the coating of the electric heating coating prepared in the embodiment and the comparative example was tested by a resistance meter. The cured thickness of the electric heating coating was 20 μm. The test environment was 35° C. and the relative humidity was 50%. Stable and good electrical contact was ensured at both ends of the test sample. The test value was the average of 10 tests and recorded in Table 1.
[0103] Waterproofness: The surface water contact angle test of the electric heating coatings prepared in the embodiments and comparative examples was carried out by the sessile drop method. The cured thickness of the electric heating coating was 20 μm, the test water drop size was 2 μL, the test time was 15 s, and the measured water contact angle (°) was recorded. The test value was the average of 10 tests and recorded in Table 1.
[0104] Aging resistance: The electric heating coatings prepared in the embodiments and comparative examples were cured to a coating thickness of 30 μm and aged for 90 days in a constant temperature and humidity chamber at 65°C and 75% relative humidity. After 90 days, the coatings were taken out to observe whether there were yellowing, bubbles, cracks and hydrolysis. If there were any, they were considered unqualified, otherwise they were qualified. 50 groups of samples were tested in each group, and the qualified rate of the samples was recorded in Table 1.
[0105] Light resistance: The electric heating coatings prepared in the embodiments and comparative examples were cured, with a coating thickness of 30 μm. The test environment was exposed to sufficient natural light for 8 hours per day for a total of 180 days. The surface condition of the coating was then observed to see if there was obvious blistering, peeling, damage, cracking, and yellowing. If so, it was recorded as unqualified, otherwise it was qualified. 50 groups of samples were tested in each group, and the qualified rate of the samples was recorded in Table 1.
[0106] Table 1 Performance test results
[0107]
[0108] It can be seen from the examples and comparative examples of the present application and the data results in Table 1 that Examples 1 and 2 of the present application have obvious advantages over comparative examples 1 to 8 in terms of electric heating performance, waterproof performance, aging resistance and light resistance. This is mainly due to the combined effect of the modified particles and compounded functional additives specified in the present application. Comparative examples 1 to 8 did not adopt the technical solution specified in the present application, resulting in obvious disadvantages in the above performance tests. This further proves the necessity of the technical solution specified in the present application for the technical effect of the present application and solving technical problems.
Claims
1. An electric heating paint for the rear windshield of an automobile, characterized in that: The electric heating paint for the rear windshield of an automobile, calculated by weight, comprises the following raw materials: 30-50 parts of polyester resin, 12-25 parts of modified particles, 4-8 parts of dispersant, 1-2 parts of leveling agent, 2-4 parts of curing agent, 5-15 parts of functional additive, and 40-60 parts of solvent; The mass ratio of the polyester resin, modified particles and dispersant is (4-5): (1.4-2): (0.5-0.7); The polyester resin is an unsaturated polyester resin; The viscosity of the polyester resin is 2000-4000 cP, and the test condition is 25°C; The light transmittance of the polyester resin is 90-95%, and the test conditions are: wavelength 550nm; Preparation method of the modified particles The following steps are involved: S1: Add zinc nitrate hexahydrate, 2,5-dihydroxyterephthalic acid and acetic acid to DMF solution and mix evenly, first heat to 50~60℃ and keep warm for 20~25min, then heat to 120~130℃, stir at 100~150rpm for 20~24h; S2: After the reaction is completed, cool to 60~70℃, first add succinic anhydride and silane coupling agent, stir at 40~80rpm for 5~6h, and add titanium dioxide and nano-graphite powder mixed DMF solution dropwise within 1~1.5h after the reaction starts; S3: After the reaction of S2 is completed, heat to 120~130℃ for the second time, stir at 60~90rpm for 10~15h, cool to room temperature naturally after the reaction is completed, centrifuge and filter, wash the product with methanol, and dry in vacuum at 80~90℃ to obtain; The mass ratio of zinc nitrate hexahydrate, 2,5-dihydroxyterephthalic acid, acetic acid and nano-graphite powder is (0.8-1): (1.5-2): (8-10): (3.5-4); The mass ratio of succinic anhydride, silane coupling agent, titanium dioxide and nano-graphite powder is (1.8-2): (0.5-0.7): (0.8-1.2): (3.5-4); The average particle size of the nano graphite powder is 50-100 nm; the average particle size of the titanium dioxide is 5-10 nm; The dispersant is at least one of acrylates, phosphates, and fatty alcohol polyoxyethylene ethers; The leveling agent is a silicone leveling agent or a polyurethane leveling agent; The functional additive is a composition of epoxy block, pullulan and sodium carboxymethyl cellulose; the mass ratio of the epoxy block, pullulan and sodium carboxymethyl cellulose is (2.5-3.5): (5-7): (1.5-2); The epoxy block material is a composition of an ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 2500-3000 and an ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 7500-8500, and the mass ratio of the two is (5-6.5): (1.1-2.2); The automobile rear window is a rear windshield.
2. The electric heating paint for rear windshield of an automobile according to claim 1, characterized in that: The viscosity of the polyester resin is 2500-3500 cP, and the test condition is 25°C.
3. The electric heating paint for automobile rear windshield according to claim 2 is characterized in that: The average particle size of the modified particles is 550-650 nm.
4. The electric heating paint for automobile rear windshield according to claim 3 is characterized in that: The dispersant is a composition of alkylphenyl phosphate and cetearyl alcohol polyoxyethylene ether.
5. The electric heating paint for automobile rear windshield according to claim 4 is characterized in that: The mass ratio of the alkylphenyl phosphate and cetearyl alcohol polyoxyethylene ether is (2-3): (1-1.5); the hydroxyl value of the cetearyl alcohol polyoxyethylene ether is 80-120 mgKOH / g.
6. The electric heating paint for automobile rear windshield according to claim 5, characterized in that: The leveling agent is an organic silicon leveling agent.
7. The electric heating paint for automobile rear windshield according to claim 6, characterized in that: The curing agent is at least one of methyl ethyl ketone peroxide, benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, cumene hydroperoxide, diphenylmethane diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, and hexamethylene diisocyanate.
8. A method for preparing the electric heating paint for the rear windshield of an automobile according to any one of claims 1 to 7, characterized in that: The specific steps include: S1: Mix the modified particles and dispersant and add them to the polyester resin, and disperse them at a high speed of 400-450rpm in a high-speed disperser for 15-20min; S2: Then add the solvent containing the leveling agent and functional additives, and continue to disperse at a high speed for 40-50min; S3: After the dispersion is completed, add the curing agent, stir at a speed of 60-120rpm for 10-15min until uniform, and the product is obtained.