Lithium cobalt oxide material and preparation method and application thereof

By preparing lithium cobalt oxide materials composited with T2 phase and O2 phase, the problems of low capacity and poor cycle stability of lithium cobalt oxide materials at high voltages are solved, and electrochemical properties of high capacity and long cycle life are achieved.

CN118712376APending Publication Date: 2024-09-27TIANJIN B&M SCI & TECH LTD +1
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410699172.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-30
Publication Date
2024-09-27

AI Technical Summary

Technical Problem

Existing lithium cobalt oxide materials have low capacity and poor cycle stability at high voltages. When charged to a higher potential, the material is easily destroyed, the interface is unstable, and a spinel phase with low electrochemical activity is generated.

Method used

Lithium cobalt oxide composite materials with T2 phase structure and O2 phase structure are prepared through mixed heat treatment, ion exchange treatment and drying treatment of sodium and cobalt sources to obtain lithium cobalt oxide materials with high capacity and excellent cycle stability.

Benefits of technology

Under high voltage, the capacity and cycle stability of lithium cobalt oxide materials are significantly improved, the generation of spinel phase is suppressed, the cycle life of the battery is extended, and the electrochemical performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118712376A
    Figure CN118712376A
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a lithium cobalt oxide material and a preparation method and application thereof. The lithium cobalt oxide material comprises a composite material of lithium cobalt oxide with a T2 phase structure and lithium cobalt oxide with an O2 phase structure, and the mass ratio of the lithium cobalt oxide with the T2 phase structure to the lithium cobalt oxide with the O2 phase structure is smaller than or equal to 0.3; the chemical formula of the lithium cobalt oxide material is LiaNabCoO2, a is more than or equal to 0.6 and less than or equal to 1, and b is more than or equal to 0 and less than or equal to 0.1. The lithium cobalt oxide material provided by the invention takes an O2 phase as a main phase and a T2 phase as an auxiliary phase, and has relatively high capacity, good structural stability and excellent cycling stability under high voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a lithium cobalt oxide material and a preparation method and application thereof. Background Art

[0002] The space group of O3-LiCoO2 is R-3m, Li + and Co 3+ The layers are arranged alternately in a cubic close-packed O 2- In the octahedral position formed, LiO6 and CoO6 octahedra are stacked with shared edges, and the arrangement order of O layers is ABCABC. + It is superior to spinel oxide positive electrode and lithium iron phosphate positive electrode in terms of diffusion. At the same time, its theoretical capacity is as high as 274mAh / g, with a very high volume energy density. However, when charged to 4.5V, the phase transition of O3→H1-3→O1 begins, the reversibility of the slip phase transition of the CoO2 plate layer decreases, and the particles undergo a c-axis contraction of more than 3%. At the same time, due to the Co 3+ / 4+ :3d energy band and O 2- : The top of the 2p band overlaps, resulting in the O 2- It will provide charge compensation and cause an oxidation reaction, and O2 will be released from the lattice, causing damage to the material. In addition, some researchers have found that when charged to a higher potential, the interface of LiCoO2 is unstable and a spinel phase with low electrochemical activity will be generated.

[0003] Therefore, it is crucial to develop cathode materials with stable electrochemical performance at high voltage and higher energy density.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One object of the present invention is to provide a lithium cobalt oxide material to solve the technical problems of low capacity and poor cycle stability of the lithium cobalt oxide material in the prior art under high voltage. The lithium cobalt oxide material of the present invention has high capacity and good cycle stability under high voltage.

[0006] Another object of the present invention is to provide a method for preparing the lithium cobalt oxide material, which is simple and easy to implement, environmentally friendly, and the obtained lithium cobalt oxide material has uniform particles, high crystallinity, and excellent electrochemical properties under high pressure.

[0007] Another object of the present invention is to provide a positive electrode sheet.

[0008] Another object of the present invention is to provide a battery.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] A lithium cobalt oxide material, comprising a composite material of lithium cobalt oxide with a T2 phase structure and lithium cobalt oxide with an O2 phase structure, wherein the mass ratio of the lithium cobalt oxide with the T2 phase structure to the lithium cobalt oxide with the O2 phase structure is less than or equal to 0.3; the chemical formula of the lithium cobalt oxide material is Li a Na b CoO2, where 0.6≤a≤1, 0≤b≤0.1.

[0011] In some embodiments, the mass ratio of the lithium cobalt oxide with T2 phase structure to the lithium cobalt oxide with O2 phase structure is 0.01 to 0.25.

[0012] In some embodiments, the particle size D50 of the lithium cobalt oxide material is 4 to 18 μm.

[0013] In some embodiments, the specific surface area of ​​the lithium cobalt oxide material is 0.14 to 0.68 m 2 / g.

[0014] In some embodiments, the first coulombic efficiency of the battery made of the lithium cobalt oxide material is greater than or equal to 120% under the conditions of 3V to 4.65V and 0.1CC / 0.1CD.

[0015] In some embodiments, the battery made of the lithium cobalt oxide material has an initial discharge capacity of more than 230 mAh / g under the conditions of 3-4.65 V and 0.1 CC / 0.1 CD.

[0016] In some embodiments, the capacity retention rate of a battery corresponding to the lithium cobalt oxide material after 50 cycles at 45° C. is greater than 67%.

[0017] The method for preparing the lithium cobalt oxide material as described above comprises the following steps:

[0018] The mixture of the sodium source and the cobalt source is subjected to a first heat treatment to obtain a first material; the mixture of the first material and the lithium source is subjected to an ion exchange treatment under a second heat treatment condition to obtain a second material; the second material is subjected to a washing treatment and a drying treatment to obtain a lithium cobalt oxide material.

[0019] In some embodiments, the cobalt source includes at least one of cobalt tetroxide, cobalt hydroxide, cobaltous oxide, cobalt nitrate, cobalt sulfate and cobalt oxyhydroxide.

[0020] In some embodiments, the sodium source includes at least one of sodium carbonate, sodium bicarbonate, and sodium hydroxide.

[0021] In some embodiments, the molar ratio of the sodium source to the cobalt source, calculated as sodium element and cobalt element, is (0.65-0.8):1.

[0022] In some embodiments, the sodium source and the cobalt source are mixed multiple times to obtain the mixture, the mixing speed is 10000-18000 rpm, and the mixing time of each time is 0.5-3 min.

[0023] In some embodiments, the temperature of the first heat treatment is 650-850° C., and the time of the first heat treatment is 8-30 hours.

[0024] In some embodiments, the heating rate of the first heat treatment is 2-8° C. / min.

[0025] In some embodiments, the lithium source includes at least one of lithium nitrate, lithium hydroxide, lithium chloride and lithium carbonate.

[0026] In some embodiments, the molar ratio of the lithium source to the sodium source, calculated as lithium element and sodium element, is greater than or equal to 5.

[0027] In some embodiments, the temperature of the second heat treatment is 80 to 250° C., and the time of the second heat treatment is 0.5 to 3 hours.

[0028] In some embodiments, the drying process is carried out at a temperature of 80 to 180° C. and for a time of 10 to 20 hours.

[0029] A positive electrode sheet comprises a positive electrode current collector and a positive electrode layer arranged on at least one side surface of the positive electrode current collector, wherein the positive electrode layer contains a lithium cobalt oxide material, and the lithium cobalt oxide material is the lithium cobalt oxide material described above, or the lithium cobalt oxide material prepared by the preparation method of the lithium cobalt oxide material described above.

[0030] A battery comprises the positive electrode sheet, the negative electrode sheet, the separator and the electrolyte.

[0031] An electrical device comprises the battery.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The lithium cobalt oxide material of the present invention comprises a composite material of lithium cobalt oxide of T2 phase structure and lithium cobalt oxide of O2 phase structure, with O2 phase as the main phase and T2 phase as the auxiliary phase. The O2 phase lithium cobalt oxide has a higher resistivity against proton attack, and the local face sharing configuration between LiO6 and CoO6 octahedra in the O2 phase lithium cobalt oxide can inhibit the migration of Co to the Li site, thereby inhibiting the formation of spinel phase during charge and discharge, so that the O2 phase lithium cobalt oxide has a relatively stable structure and good electrochemical cycle performance; T2 phase lithium cobalt oxide positive electrode material, its structure The structural feature is that the oxygen atomic layers are periodically arranged with the spacing between two transition metal layers as the period, and the lithium is located at the tetrahedral site, which is very different from the lithium at the octahedral site in the traditional commercial O3 phase lithium cobalt oxide. Therefore, T2 phase lithium cobalt oxide has a higher first coulombic efficiency and a huge improvement in specific capacity compared to the mainstream commercial positive electrode materials on the market. Therefore, the composite material prepared in the present application has good structural stability at high voltage, high capacity and excellent cycle stability under the synergistic effect of O2 phase lithium cobalt oxide and T2 phase lithium cobalt oxide.

[0034] (2) The preparation method of the lithium cobalt oxide material of the present invention is simple and easy. The first material having a P2 phase is obtained by solid phase sintering, and then ion exchange treatment is performed to obtain a lithium cobalt oxide material having a composite of a T2 phase and an O2 phase. The lithium cobalt oxide material obtained by this method has uniform particles and high crystallinity, and has a higher capacity and a longer cycle life under high voltage.

[0035] (3) The battery of the present invention has the characteristics of high capacity, high stability and high cycle performance under high voltage. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0037] Figure 1 This is a scanning electron microscope image of the lithium cobalt oxide material in Example 1 of the present invention;

[0038] Figure 2 is an X-ray diffraction pattern of the lithium cobalt oxide material in Example 1 of the present invention;

[0039] Figure 3 The electrical performance diagram of the battery in Example 1 of the present invention and in Comparative Example 1;

[0040] Figure 4 This is a scanning electron microscope image of the lithium cobalt oxide material obtained in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0041] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0042] According to one aspect of the present invention, the present invention relates to a lithium cobalt oxide material, wherein the lithium cobalt oxide material comprises a composite material of lithium cobalt oxide with a T2 phase structure and lithium cobalt oxide with an O2 phase structure, wherein the mass ratio of the lithium cobalt oxide with the T2 phase structure to the lithium cobalt oxide with the O2 phase structure is less than or equal to 0.3; the chemical formula of the lithium cobalt oxide material is Li a Na b CoO2, where 0.6≤a≤1, 0≤b≤0.1.

[0043] The lithium cobalt oxide material of the present invention comprises a composite material of lithium cobalt oxide with a T2 phase structure and lithium cobalt oxide with an O2 phase structure, with the O2 phase as the main phase and the T2 phase as the auxiliary phase, and has a higher capacity at high voltage, good structural stability and excellent cycle stability.

[0044] It should be noted that there will be some residual sodium ions in the lithium cobalt oxide material of the present invention, because the material is prepared by an ion exchange method, and since sodium ions are difficult to be completely replaced by lithium ions, there will still be a very small amount of sodium ions in the material.

[0045] In the present invention, the composition of the lithium cobalt oxide material is detected by an inductively coupled plasma spectrometer.

[0046] In the present invention, the mass ratio of lithium cobalt oxide with a T2 phase structure to lithium cobalt oxide with an O2 phase structure is obtained by XRD calculation.

[0047] In some embodiments, the mass ratio of the lithium cobalt oxide with a T2 phase structure to the lithium cobalt oxide with an O2 phase structure is less than or equal to 0.3, for example, it can be but not limited to 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.15, 0.18, 0.2, 0.22, 0.25, 0.28 or 0.3, or any range between the two. The lithium cobalt oxide with a T2 phase structure and the lithium cobalt oxide with an O2 phase structure have a suitable mass ratio, which can ensure that the lithium cobalt oxide material has the characteristics of high capacity and high cycle life under high pressure. Furthermore, the mass ratio of the lithium cobalt oxide with a T2 phase structure to the lithium cobalt oxide with an O2 phase structure is 0.01 to 0.25.

[0048] In some embodiments, the particle size D50 of the lithium cobalt oxide material is 4 to 18 μm, for example, but not limited to 4 μm, 5 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 15 μm, 16 μm, 18 μm, etc., or any range between the two. The lithium cobalt oxide material of the present invention has a suitable particle size to ensure better electrical properties.

[0049] In some embodiments, the lithium cobalt oxide material of the present invention has a suitable specific surface area, and the specific surface area of ​​the lithium cobalt oxide material is 0.14 to 0.68 m 2 / g, for example, but not limited to 0.14m 2 / g, 0.15m 2 / g, 0.18m 2 / g, 0.2m 2 / g, 0.22m 2 / g, 0.25m 2 / g, 0.3m 2 / g, 0.4m 2 / g, 0.5m 2 / g, 0.6m 2 / g or 0.68m 2 / g, etc., or any range between the two.

[0050] In some embodiments, the first coulombic efficiency of the battery made of the lithium cobalt oxide material under the conditions of 3V~4.65V, 0.1CC / 0.1CD is greater than or equal to 120%, for example, it can be but not limited to 121%, 122%, 123%, 124%, 125%, 128%, 130%, 135%, etc., or any range value between the two.

[0051] In some embodiments, the first discharge capacity of the battery made of the lithium cobalt oxide material under the conditions of 3-4.65V, 0.1CC / 0.1CD is above 230mAh / g, for example, it can be but not limited to 230.2mAh / g, 230.5mAh / g, 231mAh / g, 232mAh / g, 236mAh / g, etc., or any range value between the two.

[0052] In some embodiments, the capacity retention rate of the battery corresponding to the lithium cobalt oxide material after 50 cycles at 45°C is greater than 67%, for example, it can be but not limited to 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, etc., or any range value between the two.

[0053] The lithium cobalt oxide material of the present invention has high first coulombic efficiency, large first discharge capacity in the range of 3 to 4.65 V, and a battery corresponding to the lithium cobalt oxide material has high capacity retention rate after 50 cycles at 45° C. The lithium cobalt oxide material of the present invention has excellent comprehensive performance.

[0054] According to another aspect of the present invention, the present invention also relates to a method for preparing the lithium cobalt oxide material as described above, comprising the following steps:

[0055] Subjecting the mixture of the sodium source and the cobalt source to a first heat treatment to obtain a first material;

[0056] Subjecting the mixture of the first material and the lithium source to an ion exchange treatment under a second heat treatment condition to obtain a second material;

[0057] The second material is washed and dried to obtain a lithium cobalt oxide material.

[0058] The preparation method of the lithium cobalt oxide material of the present invention is simple and easy. The first material with a P2 phase is obtained by solid phase sintering, and then molten salt ion exchange is performed. The exchange of structural Na and Li in the molten salt starts from the Li layer through slip nucleation, and then grows layer by layer to obtain a lithium cobalt oxide material with a composite of a T2 phase and an O2 phase. The lithium cobalt oxide material obtained by the method has uniform particles and high crystallinity, and has a higher capacity and a longer cycle life at high voltage.

[0059] In some embodiments, the cobalt source includes at least one of cobalt trioxide, cobalt hydroxide, cobaltous oxide, cobalt nitrate, cobalt sulfate and cobalt oxyhydroxide. The cobalt source of the present invention can be any one of the above, or a combination of at least two, such as a combination of cobalt hydroxide and cobaltous oxide, a combination of cobaltous oxide, cobalt nitrate and cobalt sulfate, a combination of cobalt sulfate and cobalt oxyhydroxide, etc.

[0060] In some embodiments, the sodium source includes at least one of sodium carbonate, sodium bicarbonate and sodium hydroxide, such as sodium carbonate and sodium bicarbonate, sodium bicarbonate and sodium hydroxide.

[0061] In some embodiments, the molar ratio of the sodium source and the cobalt source, calculated as sodium element and cobalt element, respectively, is (0.65-0.8):1, for example, it can be 0.65:1, 0.66:1, 0.67:1, 0.7:1, 0.72:1, 0.73:1, 0.74:1, 0.75:1, 0.78:1, 0.8:1, etc., or any range value between the two.

[0062] In some embodiments, the sodium source and the cobalt source are mixed multiple times to obtain the mixture, and the mixing speed is 10000-18000rpm, for example, it can be but not limited to 10000rpm, 11000rpm, 12000rpm, 13000rpm, 14000rpm, 15000rpm, 16000rpm, 17000rpm, 18000rpm, etc., or any range between the two. The time of each mixing treatment is 0.5-3min. For example, it can be but not limited to 0.5min, 1min, 1.5min, 2min, 2.5min or 3min, etc., or any range between the two. In some embodiments, the mixing treatment uses a high mixer. The present invention adopts a mixing treatment under suitable conditions to ensure that the materials are mixed more fully and evenly to ensure the electrochemical properties of the obtained lithium cobalt oxide material.

[0063] In some embodiments, the temperature of the first heat treatment is 650-850°C, for example, it can be but not limited to 650°C, 670°C, 680°C, 700°C, 710°C, 720°C, 750°C, 780°C, 800°C, 810°C, 820°C, 840°C, 850°C, etc., or any range between the two. The time of the first heat treatment is 8-30h, for example, it can be but not limited to 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 20h, 25h or 30h, etc., or any range between the two. The heating rate of the first heat treatment is 2-8°C / min, for example, it can be but not limited to 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, etc., or any range between the two. The present invention adopts appropriate first heat treatment conditions to obtain the P2 phase first material.

[0064] In some embodiments, the first heat treatment equipment may be a muffle furnace, a tunnel furnace, a roller kiln, a tube furnace or other types of calcining equipment.

[0065] In some embodiments, the lithium source includes at least one of lithium nitrate, lithium hydroxide, lithium chloride and lithium carbonate. In some embodiments, the lithium source can be selected from one or a combination of at least two, such as a combination of lithium nitrate and lithium hydroxide, a combination of lithium hydroxide and lithium chloride, a combination of lithium hydroxide, lithium chloride and lithium carbonate, etc.

[0066] In some embodiments, the molar ratio of the lithium source to the sodium source, calculated as lithium element and sodium element, is greater than or equal to 5, for example, it can be but not limited to 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 11, 12, 15, 20, 30, 50, 80, etc., or any range between the two. In some embodiments, the molar ratio of the lithium source to the sodium source, calculated as lithium element and sodium element, is greater than or equal to 10. The present invention adopts a suitable material ratio to ensure the effect of ion exchange to obtain a lithium cobalt oxide material with high electrochemical performance.

[0067] In some embodiments, the temperature of the second heat treatment is 80 to 250°C, for example, it can be but not limited to 80°C, 100°C, 150°C, 200°C, 250°C, etc., or any range between the two. The time of the second heat treatment is 0.5 to 3h, for example, it can be but not limited to 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, etc., or any range between the two. The present invention adopts appropriate second heat treatment conditions to ensure the effect of ion exchange treatment and the electrochemical properties of the final lithium cobalt oxide material.

[0068] In some embodiments, the equipment used for ion exchange treatment includes: wet coating reaction equipment, co-precipitation reaction equipment, etc.

[0069] In some embodiments, the drying temperature is 80-180°C, for example, but not limited to 80°C, 100°C, 120°C, 150°C, 160°C, 180°C, etc., or any range between the two. The drying time is 10-20h, for example, but not limited to 10h, 12h, 15h, 18h or 20h, etc., or any range between the two. The drying equipment used can be at least one of a blast oven, a vacuum drying oven, a rotary kiln, a tray dryer and an oven.

[0070] In a preferred embodiment, the method for preparing the lithium cobalt oxide material comprises the following steps:

[0071] (1) The mixture of the sodium source and the cobalt source is mixed multiple times to obtain a mixture, the mixing speed is 10000-18000 rpm, the mixing time of each mixing is 0.5-3 min, and the mixing times are 4-7 times; the molar ratio of the sodium source to the cobalt source in terms of sodium element and cobalt element is (0.65-0.8):1; the mixture is subjected to a first heat treatment, the temperature of the first heat treatment is 650-850°C, the time of the first heat treatment is 8-30 h, and the heating rate of the first heat treatment is 2-8°C / min to obtain a first material.

[0072] (2) subjecting the mixture of the first material and the lithium source to ion exchange treatment under a second heat treatment condition, wherein the temperature of the second heat treatment is 80 to 250° C., and the time of the second heat treatment is 0.5 to 3 hours, to obtain a second material; and subjecting the second material to washing and drying treatment, wherein the temperature of the drying treatment is 80 to 180° C., and the time of the drying treatment is 10 to 20 hours, to obtain a lithium cobalt oxide material.

[0073] According to another aspect of the present invention, the present invention also relates to a positive electrode sheet, comprising a positive electrode current collector and a positive electrode layer arranged on at least one side surface of the positive electrode current collector, wherein the positive electrode layer contains a lithium cobalt oxide material, and the lithium cobalt oxide material is the above-mentioned lithium cobalt oxide material, or the lithium cobalt oxide material prepared by the above-mentioned method for preparing the lithium cobalt oxide material.

[0074] The positive electrode layer of the present invention also includes a binder and a conductive agent. The mass proportion of the lithium cobalt oxide material in the positive electrode layer is 88% to 95%.

[0075] According to another aspect of the present invention, the present invention also relates to a battery, comprising the positive electrode sheet, the negative electrode sheet, the separator and the electrolyte. The battery of the present invention has excellent high temperature and high pressure performance.

[0076] According to another aspect of the present invention, the present invention also relates to an electric device, comprising the battery. The electric device may be an electric car, a portable device, and the like.

[0077] The following is further explained in conjunction with specific embodiments and comparative examples.

[0078] Example 1

[0079] The preparation method of lithium cobalt oxide material comprises the following steps:

[0080] (1) Co3O4 and sodium carbonate were mixed in a high-speed mixer at 18000 r / min for 1 min, and the mixture was repeated 6 times, wherein the molar ratio of sodium carbonate to Co3O4 in terms of sodium and cobalt was 0.75:1. The mixture was heated to 800°C at a heating rate of 3°C / min, kept at a constant temperature for 16 h, and then cooled and crushed to an average particle size of 6.8 μm to obtain a P2 sodium electrode material powder Na 0.72 CoO2.

[0081] (2) Mixing the P2 sodium electrode material and a lithium source, wherein the lithium source is composed of lithium nitrate and lithium chloride, and the mass ratio of lithium nitrate to lithium chloride is 72:28. 0.72The molar ratio of CoO2 to lithium and sodium is 10:1, and the molten salt ion exchange is carried out at 232°C for 0.5h. After the ion exchange treatment, the ion exchanged system is washed and dried at 95°C for 12h to finally obtain a T2 phase structure and O2 phase structure composite lithium cobalt oxide Li 0.717 Na 0.003 The mass ratio of CoO2, T2 phase structure lithium cobalt oxide and O2 phase structure lithium cobalt oxide is 0.22.

[0082] The scanning electron microscope image of the lithium cobalt oxide material in this embodiment is as follows Figure 1 shown.

[0083] The X-ray diffraction pattern of lithium cobalt oxide material is as follows Figure 2 shown.

[0084] Example 2

[0085] The preparation method of lithium cobalt oxide material comprises the following steps:

[0086] (1) Co3O4 and sodium carbonate were mixed in a high-speed mixer at 15000 r / min for 2 min, and the mixture was repeated 4 times, wherein the molar ratio of sodium carbonate to Co3O4 in terms of sodium element and cobalt element was 0.68:1. The mixture was heated to 780°C at a heating rate of 4.5°C / min, kept at a constant temperature for 18 h, and then cooled and crushed to a powder with an average particle size of 7.2 μm to obtain P2 sodium electrode material powder Na 0.71 CoO2.

[0087] (2) Mixing the P2 sodium electrode material and a lithium source, wherein the lithium source is composed of lithium chloride and lithium nitrate, and the mass ratio of lithium chloride to lithium nitrate is 25:75. 0.71 The molar ratio of CoO2 to lithium and sodium is 8:1, and the molten salt ion exchange is carried out at 220°C for 1 hour. After the ion exchange treatment, the system after ion exchange is washed and dried at a temperature of 110°C for 12 hours to finally obtain a composite lithium cobalt oxide Li with a T2 phase structure and an O2 phase structure. 0.708 Na 0.002 The mass ratio of CoO2, T2 phase structure lithium cobalt oxide and O2 phase structure lithium cobalt oxide is 0.08.

[0088] Example 3

[0089] The preparation method of lithium cobalt oxide material comprises the following steps:

[0090] (1) Co(NO3)2·6H2O and sodium carbonate were mixed in a high-speed mixer at 16000 r / min for 1.5 min, and the mixture was repeated 6 times, wherein the molar ratio of sodium carbonate to Co(NO3)2·6H2O was 0.75:1 in terms of sodium and cobalt, respectively. The mixture was heated to 850°C at a heating rate of 8°C / min, kept at a constant temperature for 8 h, and then cooled and crushed to an average particle size of 7.8 μm to obtain a P2 sodium electrode material powder Na 0.74 CoO2.

[0091] (2) Mixing the P2 sodium electrode material and a lithium source, wherein the lithium source is composed of lithium nitrate and lithium chloride, and the mass ratio of lithium nitrate to lithium chloride is 70:30. 0.74 The molar ratio of CoO2 to lithium and sodium is 9:1. The molten salt ion exchange is carried out at 250°C for 0.5h. After the ion exchange treatment, the ion exchange system is washed and dried at a temperature of 130°C for 10h to finally obtain a T2 phase structure and O2 phase structure composite lithium cobalt oxide Li 0.733 Na 0.07 The mass ratio of CoO2, T2 phase structure lithium cobalt oxide and O2 phase structure lithium cobalt oxide is 0.26.

[0092] Example 4

[0093] The preparation method of lithium cobalt oxide material comprises the following steps:

[0094] (1) Co(NO3)2·6H2O and sodium bicarbonate were mixed in a high-speed mixer at 10000 r / min for 3 min, and the mixture was repeated 6 times, wherein the molar ratio of Co(NO3)2·6H2O and sodium bicarbonate was 0.76:1 in terms of sodium and cobalt, respectively. The mixture was heated to 850°C at a heating rate of 8°C / min, kept at a constant temperature for 8 h, and then cooled and crushed to an average particle size of 8.2 μm to obtain a P2 sodium electrode material powder Na 0.75 CoO2.

[0095] (2) Mixing the P2 sodium electrode material and a lithium source, wherein the lithium source is composed of lithium nitrate and lithium hydroxide, and the mass ratio of lithium nitrate to lithium hydroxide is 62:38. 0.75 The molar ratio of CoO2 to lithium and sodium is 8:1, and the molten salt ion exchange is carried out at 170°C for 2.5 hours. After the ion exchange treatment, the ion exchanged system is washed and dried at 80°C for 15 hours to finally obtain a T2 phase structure and O2 phase structure composite lithium cobalt oxide Li 0.748 Na 0.02 The mass ratio of CoO2, T2 phase structure lithium cobalt oxide and O2 phase structure lithium cobalt oxide is 0.20.

[0096] Example 5

[0097] The preparation method of lithium cobalt oxide material is different from that of Example 1 in that:

[0098] In step (1), heat to 780° C. and keep the temperature constant for 30 hours.

[0099] Example 6

[0100] The preparation method of lithium cobalt oxide material is different from that of Example 1 in that:

[0101] In step (1), the molar ratio of Co3O4 and sodium carbonate, calculated as sodium element and cobalt element, is 0.8:1.

[0102] Example 7

[0103] The preparation method of lithium cobalt oxide material is different from that of Example 1 in that:

[0104] In step (1), the molar ratio of Co3O4 and sodium carbonate, calculated as sodium element and cobalt element, is 0.65:1.

[0105] Comparative Example 1

[0106] The preparation method of lithium cobalt oxide material comprises the following steps:

[0107] Co3O4 and Li2CO3 were mixed in a high-speed mixer at 18000r / min for 1min, and repeated 6 times, wherein the lithium-cobalt ratio was 1.05:1, and heated to 780°C at a heating rate of 4°C / min in the first stage, and kept at a constant temperature for 4h, and heated to 1000°C at a heating rate of 3°C / min in the second stage, and kept at a constant temperature for 8h, cooled, and crushed to an average particle size of 4.5μm of lithium cobalt oxide powder to obtain lithium cobalt oxide powder Li 0.996 CoO2.

[0108] The scanning electron microscope image of this comparative example 1 is as follows Figure 4 shown.

[0109] Comparative Example 2

[0110] The preparation method of lithium cobalt oxide material is different from that of Example 1 in that:

[0111] In step (1), the molar ratio of sodium carbonate to Co3O4, calculated as sodium element and cobalt element, is 0.6:1.

[0112] Comparative Example 3

[0113] The preparation method of lithium cobalt oxide material is different from that of Example 1 in that:

[0114] In step (1), the lithium source and Na 0.72 The molar ratio of CoO2 to lithium and sodium is 4:1.

[0115] Experimental example

[0116] The lithium cobalt oxide materials obtained in the embodiments and comparative examples of the present invention are respectively used to prepare batteries, which specifically include:

[0117] Lithium cobalt oxide material is used as the positive electrode active material, acetylene black is used as the conductive agent, polyvinylidene fluoride is used as the binder, the mass ratio of lithium cobalt oxide material, acetylene black and polyvinylidene fluoride is 90:5:5, N-methyl pyrrolidone is added, mixed evenly to form a slurry, applied on the aluminum foil current collector, vacuum dried, taken out and pressed, and cut into the positive electrode sheet of the required size. The button lithium-ion battery is assembled from the above-mentioned positive electrode sheet, lithium sheet negative electrode, separator between the positive and negative electrodes and electrolyte.

[0118] The assembled battery was subjected to capacity test and cycle test, and the test results are shown in Table 1. Figure 3 shown.

[0119] Cycle performance test method: At 45°C, charge and discharge the button cell at 1C for 50 cycles, voltage range: 3V~4.65V.

[0120] The present invention uses a particle size tester to test the particle size D50 of the lithium cobalt oxide material. The specific surface area of ​​the lithium cobalt oxide material is tested using a specific surface area tester, as shown in Table 1.

[0121] Table 1 Battery performance test results

[0122]

[0123]

[0124] As can be seen from Table 1, the lithium cobalt oxide material of the present invention has a suitable D50 particle size and a suitable specific surface area. The obtained battery has a high 0.1C discharge specific capacity of more than 230 mAh / g, a high first coulombic efficiency of more than 120%, and a 50-cycle cycle retention rate at 45°C of more than 67%. The battery obtained by the method of the present invention has excellent capacity, structural stability and cycle stability under high voltage.

[0125] Comparative Example 1 uses Co3O4 and Li2CO3 to directly prepare O3 phase lithium cobalt oxide. The obtained battery has low 0.1C discharge specific capacity, low first coulomb efficiency, and low 50 cycle retention rate at 45°C. The amount of sodium source used in step (1) of Comparative Example 2 is too low; the amount of lithium source used in Comparative Example 3 is too low; the discharge specific capacity, first coulomb efficiency and cycle retention rate of the batteries prepared from the lithium cobalt oxide materials of Comparative Examples 2 and 3 are all reduced.

[0126] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A lithium cobalt oxide material, characterized in that: The lithium cobalt oxide material comprises a composite material of lithium cobalt oxide with a T2 phase structure and lithium cobalt oxide with an O2 phase structure, wherein the mass ratio of the lithium cobalt oxide with a T2 phase structure to the lithium cobalt oxide with an O2 phase structure is less than or equal to 0.3; the chemical formula of the lithium cobalt oxide material is Li a Na b CoO2, where 0.6≤a≤1, 0≤b≤0.

1.

2. The lithium cobalt oxide material according to claim 1, characterized in that: The mass ratio of the lithium cobalt oxide with T2 phase structure to the lithium cobalt oxide with O2 phase structure is 0.01 to 0.

25.

3. The lithium cobalt oxide material according to claim 1, characterized in that: Contains at least one of the following features (1) to (2): (1) The particle size D50 of the lithium cobalt oxide material is 4 to 18 μm; (2) The specific surface area of ​​the lithium cobalt oxide material is 0.14 to 0.68 m 2 / g.

4. The lithium cobalt oxide material according to claim 1, characterized in that: Contains at least one of the following features (1) to (3): (1) The first coulombic efficiency of the battery made of the lithium cobalt oxide material is greater than or equal to 120% under the conditions of 3V to 4.65V and 0.1CC / 0.1CD; (2) The battery made of the lithium cobalt oxide material has an initial discharge capacity of more than 230 mAh / g under the conditions of 3-4.65 V and 0.1 CC / 0.1 CD; (3) The capacity retention rate of the battery corresponding to the lithium cobalt oxide material after 50 cycles at 45° C. is greater than 67%.

5. The method for preparing the lithium cobalt oxide material according to any one of claims 1 to 4, characterized in that: The following steps are involved: Subjecting the mixture of the sodium source and the cobalt source to a first heat treatment to obtain a first material; subjecting the mixture of the first material and the lithium source to an ion exchange treatment under a second heat treatment condition to obtain a second material; The second material is washed and dried to obtain a lithium cobalt oxide material.

6. The method for preparing the lithium cobalt oxide material according to claim 5, characterized in that: Contains at least one of the following features (1) to (6): (1) The cobalt source includes at least one of cobalt tetroxide, cobalt hydroxide, cobaltous oxide, cobalt nitrate, cobalt sulfate and cobalt oxyhydroxide; (2) the sodium source comprises at least one of sodium carbonate, sodium bicarbonate and sodium hydroxide; (3) The molar ratio of the sodium source to the cobalt source, calculated as sodium element and cobalt element, is (0.65-0.8):1; (4) performing multiple mixing treatments on the sodium source and the cobalt source to obtain the mixture, wherein the mixing speed is 10000 to 18000 rpm, and the mixing time of each time is 0.5 to 3 min; (5) The temperature of the first heat treatment is 650 to 850° C., and the time of the first heat treatment is 8 to 30 hours; (6) The heating rate of the first heat treatment is 2 to 8°C / min.

7. The method for preparing the lithium cobalt oxide material according to claim 5, characterized in that: Contains at least one of the following features (1) to (4): (1) The lithium source includes at least one of lithium nitrate, lithium hydroxide, lithium chloride and lithium carbonate; (2) the molar ratio of the lithium source to the sodium source, calculated as lithium element and sodium element, is greater than or equal to 5; (3) The temperature of the second heat treatment is 80 to 250° C., and the time of the second heat treatment is 0.5 to 3 hours; (4) The temperature of the drying treatment is 80 to 180° C., and the time of the drying treatment is 10 to 20 hours.

8. A positive electrode sheet, characterized in that: The invention comprises a positive electrode current collector and a positive electrode layer arranged on at least one side surface of the positive electrode current collector, wherein the positive electrode layer contains a lithium cobalt oxide material, and the lithium cobalt oxide material is the lithium cobalt oxide material according to any one of claims 1 to 4, or the lithium cobalt oxide material prepared by the preparation method of the lithium cobalt oxide material according to any one of claims 5 to 7.

9. A battery, characterized in that: It comprises the positive electrode sheet, negative electrode sheet, separator and electrolyte as described in claim 8.

10. An electrical device comprising the battery according to claim 9.

Citation Information

Cited By

  • Lithium cobalt oxide positive electrode material with composite phase as well as preparation method and application of lithium cobalt oxide positive electrode material

    CN119153682A

  • Preparation method of high-voltage lithium cobalt oxide positive electrode material

    CN119994031A

  • Composite-phase O2 type lithium cobalt oxide positive electrode material and preparation method and application thereof

    CN121149234A

  • Positive electrode material, electrochemical device, and electronic device

    WO2026183671A1