High-purity selenium bottom blowing compensation oxidation device and method
By designing a high-purity selenium bottom-blown compensated oxidation device during the preparation process of high-purity selenium, and using bottom-blown oxidation technology and a compensated oxidation mechanism, the problem of incomplete oxidation in the pre-oxidation section is solved, and the oxidation efficiency and purity of the selenium material are improved. .
Patent Information
- Application Number
- CN202410787381.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-01
AI Technical Summary
In the preparation process of high-purity selenium, the contact area between oxygen and molten selenium liquid in the pre-oxidation section is small, resulting in a slow oxidation rate and incomplete oxidation, which affects the purity and production efficiency of the selenium material.
A high-purity selenium bottom-blown compensated oxidation device is designed, including a furnace body, a combustion chamber, a compensated oxidation mechanism and a condensation chamber. Oxygen is input into the selenium liquid through the air inlet pipe for bottom-blown oxidation, and the mixed gas is compensated in the buffer chamber and protection chamber. Oxidation, increasing the content of selenium dioxide and condensation in the condensation chamber, ensuring more complete oxidation and purity.
By increasing the oxidation space and the residence time of the mixed gas, the oxidation efficiency of the selenium material is improved, the escape of unoxidized selenium and the entry of impurities are reduced, and the yield and purity of high-purity selenium are improved.
Smart Images

Figure CN118718904A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of chemical purification, and in particular to a high-purity selenium bottom blowing compensation oxidation device and method. Background Art
[0002] As an important scientific research and industrial raw material, high-purity selenium is widely used in semiconductors, high-end medical fields, etc. due to its excellent photosensitivity and biological activity. The purity of selenium directly determines the performance of related semiconductor materials, photosensitive materials, and the effect and safety of medical drugs.
[0003] At present, in the preparation process of high-purity selenium, the purification technology of pre-oxidation-reduction-vacuum distillation is valued by people because of its significant advantages in product purity. As an important link in this purification technology, pre-oxidation has a crucial impact on the product purity and production efficiency of high-purity selenium. On the one hand, the pre-oxidation technology converts selenium, tellurium and other single substances in the selenium material into corresponding dioxides to achieve the removal of tellurium impurities in subsequent steps; on the other hand, impurities with lower saturated vapor pressure remain in the residue, while impurities with higher saturated vapor pressure escape with the airflow.
[0004] However, in the pre-oxidation section, the contact area between oxygen and the molten selenium liquid is small, the oxidation rate is slow, and a portion of selenium enters the condensation section for condensation without being oxidized, resulting in incomplete oxidation. Summary of the invention
[0005] In view of the above problems, one of the purposes of the present invention is to provide a high-purity selenium bottom blowing compensation oxidation device to solve the problem of low oxidation efficiency and incomplete oxidation of selenium materials in the pre-oxidation section. Another purpose of the present invention is to provide a high-purity selenium bottom blowing compensation oxidation method to improve the oxidation effect of selenium materials in the pre-oxidation section.
[0006] A first aspect of the present invention provides a high-purity selenium bottom blowing compensation oxidation device, comprising a furnace body, wherein the furnace body is provided with an air inlet pipe and an air outlet pipe;
[0007] The furnace body is provided with:
[0008] A combustion chamber, wherein a crucible is arranged inside, and the crucible is used to fill the selenium material;
[0009] The compensating oxidation mechanism comprises a buffer chamber and a protection chamber, wherein the combustion chamber is arranged in communication between the buffer chamber and the protection chamber;
[0010] a condensation chamber, communicated with the buffer chamber;
[0011] A heating mechanism, arranged on the combustion chamber and the compensating oxidation mechanism;
[0012] The air inlet pipe extends into the crucible in the combustion chamber, and the air outlet pipe is in communication with the condensation chamber;
[0013] Among them, the heating mechanism heats the combustion chamber and the compensating oxidation mechanism, burns and melts the selenium material in the crucible into selenium liquid, the air inlet pipe inputs oxygen into the selenium liquid, performs bottom blowing oxidation to obtain a mixed gas, and the mixed gas is divided into two airflows and enters the buffer chamber and the protection chamber respectively to be compensated oxidized, so that the selenium dioxide content in the mixed gas is increased to obtain a target gas rich in selenium dioxide; the target gas flows into the condensation chamber, at least the selenium dioxide is condensed to obtain a condensation product and a non-target gas; the non-target gas is discharged from the furnace body through the air outlet pipe.
[0014] As one of the preferred schemes, a back-blowing pipe is also provided on the furnace body, and the back-blowing pipe is connected to the protection chamber to blow oxygen into the protection chamber, so that the target gas in the protection chamber flows back into the combustion chamber and flows to the condensation chamber through the buffer chamber.
[0015] As one of the preferred solutions, the outlet sleeve of the air inlet pipe in the crucible is provided with a microporous sleeve, and the microporous sleeve is spaced apart from the bottom of the crucible.
[0016] As one of the preferred solutions, the microporous sleeve is cylindrical, and a plurality of through holes are evenly spaced on the cylindrical wall.
[0017] As one of the preferred solutions, along the flow direction of the mixed gas, the areas of the cavities of the protection chamber and the buffer chamber decrease in steps; along the flow direction of the target gas, the area of the cavity of the condensation chamber decreases in steps.
[0018] As one of the preferred solutions, the protection chamber, the buffer chamber and the condensation chamber are all composed of at least one quartz collector, the interior of each quartz collector is hollow to form the cavity, and the cavity is trumpet-shaped.
[0019] As one of the preferred solutions, the heating mechanism is a heating sleeve, the interior of the heating sleeve is filled with resistance wire, and the heating sleeve is sleeved on the outer circumference of the combustion chamber and the compensating oxidation mechanism.
[0020] As one of the preferred solutions, the bottom projection of the heating mechanism overlaps with the bottom projections of the combustion chamber and the compensating oxidation mechanism.
[0021] As one of the preferred solutions, the device further comprises an outlet valve, a first air inlet valve, a second air inlet valve, a pressure gauge and two furnace covers, all of which are located outside the furnace body; wherein,
[0022] The air outlet valve is arranged on the air outlet pipe;
[0023] The first air intake valve and the pressure gauge are respectively arranged on the air intake pipe;
[0024] The second air intake valve is arranged on the blowback pipe;
[0025] The two furnace covers seal the openings at both ends of the furnace body, and the air inlet pipe, the air outlet pipe and the blowback pipe respectively penetrate the corresponding furnace covers and enter the furnace body;
[0026] Wherein, the furnace cover is detachably connected to the furnace body.
[0027] The second aspect of the present invention further provides a high-purity selenium bottom blowing compensation oxidation method, which is implemented by relying on the high-purity selenium bottom blowing compensation oxidation device provided by the first aspect of the present invention, and the method comprises:
[0028] Fill the selenium material into the crucible in the combustion chamber and seal the furnace body;
[0029] Expelling air from the furnace body;
[0030] The heating mechanism heats the combustion chamber and the compensating oxidation mechanism to a target temperature, and burns and melts the selenium material in the crucible into selenium liquid;
[0031] The air inlet pipe transmits oxygen into the selenium liquid for bottom blowing oxidation to obtain mixed gas and high boiling point impurities;
[0032] The mixed gas is divided into two gas streams which enter the buffer chamber and the protection chamber respectively to be compensated for oxidation, thereby obtaining a target gas rich in selenium dioxide, and the high boiling point impurities remain in the crucible;
[0033] The target gas in the buffer chamber enters the condensation chamber for condensation, and the target gas in the protection chamber flows back into the combustion chamber and flows through the buffer chamber to the condensation chamber for condensation, thereby obtaining condensation products and non-target gas, which is discharged from the furnace body through the gas outlet pipe;
[0034] The condensed product is collected and passed through a reduction section and a vacuum distillation section to obtain high-purity selenium.
[0035] Compared with the prior art, this application has the following advantages:
[0036] The embodiment of the present invention provides a high-purity selenium bottom blowing compensation oxidation device, comprising a furnace body, on which an air inlet pipe and an air outlet pipe are arranged; the furnace body is provided with: a combustion chamber, inside which a crucible is arranged, and the crucible is used to fill selenium material; a compensation oxidation mechanism, comprising a buffer chamber and a protection chamber, the combustion chamber is connected and arranged between the buffer chamber and the protection chamber; a condensation chamber, which is connected to the buffer chamber; a heating mechanism, which is arranged on the combustion chamber and the compensation oxidation mechanism; the air inlet pipe extends into the crucible in the combustion chamber, and the air outlet pipe is connected to the condensation chamber;
[0037] Among them, the heating mechanism heats the combustion chamber and the compensating oxidation mechanism, burns and melts the selenium material in the crucible into selenium liquid, the air inlet pipe inputs oxygen into the selenium liquid, performs bottom blowing oxidation to obtain a mixed gas, and the mixed gas is divided into two airflows and enters the buffer chamber and the protection chamber respectively to be compensated oxidized, so that the selenium dioxide content in the mixed gas is increased to obtain a target gas rich in selenium dioxide; the target gas flows into the condensation chamber, at least the selenium dioxide is condensed to obtain a condensation product and a non-target gas; the non-target gas is discharged from the furnace body through the air outlet pipe.
[0038] By adopting the technical solution of the present application, the setting of the compensating oxidation mechanism provides an additional oxidation space for gaseous selenium, so that the flow path of the mixed gas carrying selenium dioxide and gaseous selenium in the furnace body becomes longer, and the reciprocating flow of the mixed gas in the buffer chamber and the protection chamber increases the residence time of the mixed gas in the furnace body, ensuring more thorough oxidation; the gaseous selenium that is not completely oxidized in the buffer chamber and the protection chamber continues to react with oxygen and is further oxidized to selenium dioxide, so that the selenium dioxide can be fully condensed in the condensation chamber, reducing the escape of unoxidized selenium element, and reducing the entry of impurities into the final product, thereby improving the yield and purity of high-purity selenium in subsequent stages.
[0039] The high-purity selenium bottom blowing compensating oxidation method provided in the embodiment of the present invention has the same advantages as the above-mentioned high-purity selenium bottom blowing compensating oxidation device over the prior art, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the description of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0041] Figure 1 It is a schematic diagram of the overall structure of a high-purity selenium bottom blowing compensation oxidation device according to an embodiment of the present application;
[0042] Figure 2 is a side view of a quartz collector according to an embodiment of the present application;
[0043] Figure 3 1 is a front view and a bottom view of a microporous casing according to an embodiment of the present application;
[0044] Figure 4 It is a flow chart of the steps of the high-purity selenium bottom blowing compensation oxidation method described in one embodiment of the present application.
[0045] Description of reference numerals:
[0046] 1. Furnace body; 2. Furnace cover; 3. Exhaust pipe; 4. Exhaust valve; 5. Graphite crucible; 6. Quartz collector; 7. First air inlet valve; 8. Pressure pipe; 9. Pressure gauge; 10. Air inlet pipe; 11. Back-blow pipe; 12. Second air inlet valve; 13. Heating device; 14. Resistance wire; 15. Microporous sleeve; 16. Condensation chamber; 17. Buffer chamber; 18. Combustion chamber; 19. Protection chamber; 20. Narrow mouth; 21. Through hole. DETAILED DESCRIPTION
[0047] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0048] It should be noted that selenium materials usually contain tellurium, and selenium and tellurium have similar physical and chemical properties. It is difficult to directly use vacuum distillation or zone melting to remove trace tellurium in selenium. Therefore, it is necessary to convert selenium and tellurium in the selenium material into dioxide, and then separate them using their saturated vapor pressure difference. The present invention is mainly aimed at improving the deficiencies of the pre-oxidation section in the high-purity selenium purification process. After the pre-oxidation section, it needs to be further purified through the reduction section and the vacuum distillation section to finally obtain high-purity selenium. More descriptions about the reduction section and the vacuum distillation section can be obtained from related processes, and the present invention does not elaborate on this.
[0049] The deficiencies in the pre-oxidation section are mainly reflected in:
[0050] During the pre-oxidation process, the contact area between oxygen and selenium liquid is small, and tellurium and selenium cannot be fully converted into dioxide, volatilized and separated. This not only affects the removal effect of tellurium, reduces the recovery rate of selenium, and further affects the purity of high-purity selenium, but also leads to low overall oxidation efficiency.
[0051] Traditional technologies all use stirring, adding additional oxidation time or increasing the oxidation temperature to increase the contact area between oxygen and selenium liquid, but this will increase energy consumption and cost.
[0052] At the same time, when the dioxide enters the condensation section for condensation, the oxides of selenium and tellurium still contain unreacted elemental selenium and tellurium, so that the selenium dioxide content in the condensation product cannot reach the expected level, resulting in selenium loss during the purification process and waste of resources.
[0053] In the related art, there is still a blank in the means for improving the conversion rate of elemental selenium in selenium materials.
[0054] In view of this, for the phenomenon that low oxidation efficiency and incomplete oxidation together lead to low production efficiency of high-purity selenium, an embodiment of the present invention provides a high-purity selenium bottom blowing compensation oxidation device, Figure 1 An exemplary high-purity selenium bottom blowing compensation oxidation device according to some embodiments of the present disclosure is shown, and the internal structure of the device is shown, the device includes a furnace body 1, and the furnace body 1 is provided with an air inlet pipe 10 and an air outlet pipe 3; the furnace body 1 is provided with: a combustion chamber 18, in which a crucible is provided, and the crucible is used to fill selenium material; a compensation oxidation mechanism, including a buffer chamber 17 and a protection chamber 19, the combustion chamber 18 is connected and arranged between the buffer chamber 17 and the protection chamber 19; a condensation chamber 16 is connected to the buffer chamber 17; a heating mechanism is arranged on the combustion chamber 18 and the compensation oxidation mechanism; the air inlet pipe 10 extends into the crucible in the combustion chamber 18, and the air outlet pipe 3 is connected to the condensation chamber 16;
[0055] Among them, the heating mechanism heats the combustion chamber 18 and the compensating oxidation mechanism, burns and melts the selenium material in the crucible into selenium liquid, the air inlet pipe 10 inputs oxygen into the selenium liquid, performs bottom blowing oxidation to obtain a mixed gas, and the mixed gas is divided into two air flows and enters the buffer chamber 17 and the protection chamber 19 respectively to be compensated oxidized, so that the content of selenium dioxide in the mixed gas is increased to obtain a target gas rich in selenium dioxide; the target gas flows into the condensation chamber 16, at least the selenium dioxide is condensed to obtain a condensation product and a non-target gas; the non-target gas is discharged from the furnace body 1 through the outlet pipe 3.
[0056] Specifically, selenium materials can include pure selenium and low-purity selenium. Pure selenium has a higher content of selenium, while low-purity selenium has a lower content of selenium. For example, pure selenium includes products that have undergone preliminary purification and have a purity of 3N-5N, where N represents purity. Low-purity selenium includes industrial selenium and selenium minerals.
[0057] Specifically, Figure 1As shown, the furnace body 1 is a tubular furnace with openings at both ends and a hollow interior. The openings at both ends of the tubular furnace are sealed by two furnace covers 2 to form a closed furnace body 1. Specifically, the two furnace covers 2 are a left furnace cover and a right furnace cover. The right furnace cover seals the right opening of the furnace body 1 and allows the air inlet pipe 10 to pass through; the left furnace cover seals the left opening of the furnace body 1 and allows the air outlet pipe 3 to pass through.
[0058] The furnace body 1 is provided with a condensation chamber 16, a buffer chamber 17, a combustion chamber 18 and a protection chamber 19 from left to right. A crucible, such as a graphite crucible 5, is provided in the combustion chamber 18, which has high temperature resistance and oxidation resistance and is responsible for the high temperature oxidation reaction of the selenium material in the crucible. Among them, one end of the air inlet pipe 10 extends horizontally through the right furnace cover 2 of the furnace body 1 and the protection chamber 19 to enter the combustion chamber 18, and the other end extends out of the furnace body 1 to be connected to the oxygen output device, and oxygen is input into the air inlet pipe 10 through the oxygen output device. One end of the air outlet pipe 3 extends horizontally through the left furnace cover 2 of the furnace body 1 to extend into the furnace body 1, and the other end extends out of the furnace body 1 to be connected to the tail gas tank.
[0059] In some embodiments, an oxygen preheating device is provided on the pipe connecting the air inlet pipe 10 and the oxygen output device. The oxygen preheating device may include an electric heater or a heat exchanger to allow the oxygen to reach a desired temperature before entering the furnace body 1. The combustion chamber 18 is the main reaction area, and the heating device 13 is arranged on the combustion chamber 18 to heat the combustion chamber 18 to maintain a high temperature environment. Therefore, the preheated oxygen is passed into the preheated combustion chamber 18, which can improve the reactivity and combustion efficiency of the oxygen and accelerate the reaction rate. In addition, the heating mechanism is arranged on the compensating oxidation mechanism, and the buffer chamber 17, the combustion chamber 18 and the protection chamber 19 are heated to the set temperature at the same time, so as to further ensure the efficiency and purity of the reaction.
[0060] More specifically, during the purification process of selenium materials, possible impurities include sulfur, tellurium, bismuth, silver, copper, lead, cadmium, arsenic, zirconium, antimony, iron and other elements. The device of the present invention is described by taking pure selenium carrying trace amounts of lead, bismuth, antimony, sulfur and arsenic as an example.
[0061] The selenium material is heated and melted in the crucible in the combustion chamber 18 to form a selenium material. The selenium material undergoes an oxidation reaction with the preheated oxygen to obtain a mixed gas and high-boiling impurities. The high-boiling impurities (lead, tellurium, bismuth, etc.) remain in the graphite crucible 5. The mixed gas includes selenium dioxide, tellurium dioxide, oxygen, gaseous selenium, etc. The mixed gas is divided into two streams and enters the buffer chamber 17 and the protection chamber 19 respectively to be compensated for oxidation. The buffer chamber 17 maintains a high temperature state under the heating mechanism. It itself serves as a second line of defense to capture incompletely oxidized gas, so that selenium is further oxidized in this area, thereby obtaining a target gas rich in selenium dioxide. The target gas flows from the buffer chamber 17 to the condensation chamber 16 to be condensed, and a condensation product and non-target gas, that is, low-boiling impurities (sulfur, arsenic, chlorine and some compounds thereof) are obtained. At the same time, the protection chamber 19 is maintained at a high temperature under the heating mechanism, and the buffer chamber 17 serves as the third line of defense to capture the incompletely oxidized gas, so that selenium is further oxidized in the area, thereby obtaining a target gas rich in selenium dioxide. When the target gas flows back to the combustion chamber 18, it is oxidized again in the combustion chamber 18, and then flows to the buffer chamber 17 to be further oxidized, and the selenium dioxide content in the target gas is further increased, and finally flows to the condensation chamber 16 and condenses together with the target gas flowing out of the buffer chamber 17 to obtain condensation products and non-target gas. The non-target gas escapes with the air flow and is discharged to the tail gas tank through the outlet pipe 3.
[0062] In some embodiments, the furnace cover 2 is detachably connected to the furnace body 1, and the furnace cover 2 is opened when the selenium material is filled in the crucible, and the furnace cover 2 is closed to carry out the oxidation reaction, and the furnace cover 2 is opened after the oxidation reaction is completed to collect the condensed product.
[0063] In some embodiments, a back-blowing pipe 11 is further provided on the furnace body 1, and the back-blowing pipe 11 is connected to the protection chamber 19 to blow oxygen into the protection chamber 19, so that the target gas in the protection chamber 19 flows back into the combustion chamber 18 and is oxidized again in the combustion chamber 18.
[0064] It is understandable that the types and contents of impurities of selenium materials vary depending on their sources, so selenium materials of different purities and compositions will produce different mixed gases during the oxidation combustion process, thereby producing different high-boiling point impurities and low-boiling point impurities. The device of the present invention is suitable for pre-oxidation of selenium materials of different compositions, so the embodiments of the present invention do not limit the specific composition of the selenium material and the mixed gas formed during the combustion process of the selenium material.
[0065] In this way, the setting of the compensating oxidation mechanism provides an additional oxidation space for gaseous selenium, so that the flow path of the mixed gas carrying selenium dioxide and gaseous selenium in the furnace body 1 becomes longer, and the reciprocating flow of the mixed gas in the buffer chamber 17 and the protection chamber 19 increases the residence time of the mixed gas in the device, ensuring more thorough oxidation. The gaseous selenium that is not completely oxidized in the buffer chamber 17 and the protection chamber 19 continues to react with oxygen and is further oxidized to selenium dioxide, so that the selenium dioxide can be fully condensed in the condensation chamber 16, reducing the escape of unoxidized selenium and reducing impurities from entering the final product, thereby improving the yield and purity of high-purity selenium in the subsequent process.
[0066] In a further technical solution, the condensation chamber 16, the buffer chamber 17, the combustion chamber 18 and the protection chamber 19 are connected in sequence and arranged in the furnace body 1. The condensation chamber 16 on the left side has a space with the left end cover, and the non-target gas is discharged from the furnace body 1 through the outlet pipe 3 in the space; the protection chamber 19 on the right side has a space with the right end cover, and oxygen is mixed in the space through the back-blowing pipe 11 and then blown into the protection chamber 19, so that the target gas in the protection chamber 19 is completely blocked by the back-blown oxygen before it flows out of the protection chamber 19, and then flows back into the combustion chamber 18.
[0067] Furthermore, the inlet of the air outlet pipe 3 is located in the first space between the condensation chamber 16 and the left end cover, the backblowing pipe 11 is located in the second space between the protection chamber 19 and the right end cover, and the outlet of the air inlet pipe 10 extends horizontally through the right furnace cover 2, the second space, and the protection chamber 19 into the combustion chamber 18, and bends toward the direction of the crucible, and continues to extend vertically close to the bottom of the crucible, and has a distance from the bottom, so as to directly guide the oxygen into the interior of the molten selenium liquid, and allow the oxygen to pass through the selenium liquid from the bottom of the selenium liquid upward to perform bottom blowing oxidation, thereby improving the rate and efficiency of the oxidation reaction.
[0068] In a preferred embodiment, the outlet of the air inlet pipe 10 is sleeved with a microporous sleeve 15, and the microporous sleeve 15 is spaced apart from the bottom of the crucible. In this embodiment, the microporous sleeve 15 disperses the oxygen flowing out of the air inlet pipe 10, so that the oxygen enters the selenium liquid in the form of oxygen microbubbles, and the oxygen is evenly distributed and blown upward from the bottom into the molten selenium liquid, thereby ensuring that the oxygen can penetrate into every part of the selenium liquid, reducing the problem of incomplete oxidation in the combustion chamber 18.
[0069] For a detailed explanation of this embodiment, please refer to Figure 3 , Figure 3The three views are the front view and the bottom view of the microporous sleeve, wherein (a) represents the front view and (b) represents the bottom view. The microporous sleeve 15 is cylindrical, and a plurality of through holes 21 are evenly spaced on the cylindrical wall. In this embodiment, one end of the microporous sleeve 15 is connected to the air inlet pipe 10, and the other end is immersed in the molten selenium liquid. The surface of the microporous sleeve 15 is covered with evenly distributed tiny holes, and oxygen enters the selenium liquid evenly through the multiple micropores. Preferably, the cylindrical microporous sleeve 15 makes the multiple through holes 21 face all around and contact with the selenium liquid in all directions. The multiple through holes 21 disperse the oxygen into small and dense oxygen microbubbles, which greatly increases the contact area between oxygen and the selenium liquid. The larger contact area can improve the utilization efficiency of oxygen and make the oxygen more evenly distributed in the selenium liquid, thereby increasing the rate of the oxidation reaction.
[0070] Specifically, the cylindrical wall surface includes a top wall surface, a bottom wall surface and a circumferential side wall surface. The top wall surface of the microporous sleeve 15 has a positioning hole, and the outlet of the air inlet pipe 10 is installed in the positioning hole. The circumferential side wall surface of the microporous sleeve 15 is evenly spaced to open a plurality of through holes 21, and the bottom wall surface of the microporous sleeve 15 is opened with one or more through holes 21 to evenly blow oxygen into the selenium liquid.
[0071] It can be understood that the shape, size and distribution density of the micropores determine the size and number of the oxygen microbubbles, which is not limited in this embodiment.
[0072] In another embodiment, along the flow direction of the mixed gas, the area of the cavity of the protection chamber 19 and the buffer chamber 17 decreases in steps, and along the flow direction of the target gas, the area of the cavity of the condensation chamber 16 decreases in steps. In this embodiment, the mixed gas flows out of the combustion chamber 18 in two streams, and the flow directions are from right to left from the combustion chamber 18 into the buffer chamber 17, and from left to right from the combustion chamber 18 into the protection chamber 19. The mixed gas is supplemented and oxidized in the buffer chamber 17 and the protection chamber 19 to become the target gas. The difference between the target gas and the mixed gas is that the gas components are the same but the content of the components is different. More specifically, the content of selenium and tellurium oxide in the target gas is greater than that in the mixed gas. The target gas in the buffer chamber 17 and the target gas in the protection chamber 19 eventually flow from the buffer chamber 17 to the condensation chamber 16 from right to left.
[0073] Therefore, the area of the cavity of each chamber is reduced along the direction of gas flow, and when the gas passes through the narrow cavity, it can intercept the mixed gas and the target gas from escaping from the small opening, and confine the mixed gas in the quartz collector 6 for further oxidation, and confine the target gas in the quartz collector 6 for full condensation. Therefore, the contact time and area between the gas and oxygen are significantly increased, so that the elemental selenium in the mixed gas has more time to be oxidized into selenium dioxide, and the selenium and tellurium oxide in the target gas have more time to condense and settle, thereby improving the collection efficiency.
[0074] Along the direction of gas flow, the cavity areas of the protection chamber 19, the buffer chamber 17 and the condensation chamber 16 are reduced in steps. Specifically, the protection chamber 19, the buffer chamber 17 and the condensation chamber 16 are all composed of at least one quartz collector 6, and the interior of each quartz collector 6 is hollow to form the cavity, and the cavity is trumpet-shaped.
[0075] In this embodiment, if Figure 2 As shown, Figure 2 is a side view of the quartz collector shown in this application.
[0076] The quartz collector 6 is made of high-purity silicon dioxide material and has good chemical stability and thermal stability. A trumpet-shaped cavity is formed inside the quartz collector 6, and the protection chamber 19, the buffer chamber 17 and the condensation chamber 16 are all composed of one or more quartz collectors 6, and multiple quartz collectors 6 are connected to form a channel for gas circulation. The trumpet-shaped space has a conical inner wall, and the contact area between the mixed gas and oxygen in the protection chamber 19 and the buffer chamber 17 increases, and the elemental selenium in the mixed gas has more opportunities to contact with oxygen, which promotes the further oxidation of the elemental selenium; when the target gas flows through the quartz collector 6, the contact area with the inner wall of the quartz collector 6 increases, thereby improving the heat exchange efficiency between the target gas and the inner wall of the quartz collector 6, thereby improving the condensation efficiency.
[0077] Exemplarily, the buffer chamber 17 and the condensation chamber 16 are both composed of two quartz collectors 6, the trumpet flares of the two quartz collectors 6 face the direction of the combustion chamber 18, that is, the direction in which the mixed gas comes in, and the narrow opening 20 faces the direction of the left furnace cover 2, that is, the direction in which the mixed gas goes out. The protection chamber 19 is composed of two quartz collectors 6, the trumpet flares of the two quartz collectors 6 face the direction of the combustion chamber 18, that is, the direction in which the mixed gas comes in, and the narrow opening 20 faces the direction of the right furnace cover 2, that is, the direction in which the mixed gas goes out, and the narrow opening 20 blocks the gas from directly flowing out of the corresponding quartz collector 6. Among them, the narrow opening 20 of the first quartz collector 6 is connected to the flared opening of the second quartz collector 6, so the buffer chamber 17, the condensation chamber 16 and the protection chamber 19 are a stepped diameter-reducing structure formed by the combination of two quartz collectors 6.
[0078] Similarly, three or more quartz collectors 6 are combined to form a two-step diameter reduction structure and a multi-step diameter reduction structure. Taking the condensation chamber 16 as an example, in the step diameter reduction structure, the mixed gas is fully condensed by the first stage in the first quartz collector 6, and slowly flows from the narrow mouth 20 to the second quartz collector 6 to be fully condensed by the second stage. Since the narrow mouth 20 of the first quartz collector 6 is connected to the expanded mouth of the second quartz collector 6, the mixed gas is easier to mix evenly during the diffusion process, and the inner surface area of the next quartz collector 6 is expanded again to be consistent with the first quartz collector 6, and the inner diameter is gradually reduced to form a cone, which not only increases the contact area with the mixed gas itself, but also maximizes the contact area between the mixed gas and all quartz collectors 6, and significantly improves the heat exchange efficiency.
[0079] In some embodiments, the number of quartz collectors 6 of the condensation chamber 16 may be different from the number of quartz collectors 6 of the buffer chamber 17 and the protection chamber 19, while the number of quartz collectors 6 of the buffer chamber 17 and the protection chamber 19 may be the same. Similarly, the shapes and sizes (including height, diameter and capacity) of the quartz collectors 6 of the condensation chamber 16, the quartz collectors 6 of the buffer chamber 17 and the quartz collectors 6 of the protection chamber 19 may be different from each other. In some embodiments, the size of the quartz collector 6 of the protection chamber 19 toward the narrow opening 20 of the right furnace cover 2 may be smaller to further prevent the mixed gas and the target gas from escaping from the narrow opening 20 and flowing back into the combustion chamber 18 with the blown back oxygen.
[0080] It can be understood that the characteristic parameters of the quartz collector 6 constituting the condensation chamber 16, the buffer chamber 17 and the protection chamber 19 do not necessarily need to be exactly the same, and can be reasonably designed and configured according to their respective functions and working conditions to achieve the best oxidation and condensation effects. This embodiment does not make specific limitations on this.
[0081] In summary, the present application realizes the bottom blowing function through the air inlet pipe 10 and the microporous sleeve 15 at the end, and blows a large number of small and dense oxygen microbubbles into the molten selenium liquid, which increases the contact area between oxygen and selenium liquid, greatly improves the rate of oxidation reaction, and makes oxidation more thorough. On the other hand, bubbling stirs the liquid, making the internal oxidation reaction more uniform. Through the conical surface inside the quartz collector 6, the contact area between the mixed gas mainly composed of selenium dioxide and the buffer chamber 17, the protection chamber 19 and the quartz collector 6 of the condensation chamber 16 is increased, and heat exchange is better realized. On the one hand, the gaseous selenium element that has not been completely oxidized is more completely oxidized in the buffer chamber 17, and on the other hand, the condensation efficiency of the condensation chamber 16 is improved.
[0082] In combination with the above embodiments, the first air intake valve 7 and the pressure gauge 9 are provided on the air intake pipe 10 extending out of the furnace body 1, the air outlet valve 4 is provided on the air outlet pipe 3 extending out of the furnace body 1, and the second air intake valve 12 is provided on the blowback pipe 11 extending out of the furnace body 1. The heating mechanism is a heating sleeve, the interior of which is filled with a resistance wire 14, and is sleeved on the combustion chamber 18 and the outer periphery of the compensation oxidation mechanism.
[0083] In some embodiments, the air inlet pipe 10 may be connected to a pressure pipe 8, and a pressure gauge 9 may be installed on the pressure pipe 8. In the pre-oxidation section, the oxygen flow rate and flow velocity may be controlled by the first air inlet valve 7, the second air inlet valve 12, and the air outlet valve 4, the oxygen pressure may be monitored by the pressure gauge 9, and the temperature of the molten selenium liquid may be controlled by the heating resistor 14 to control the oxidation reaction process.
[0084] Furthermore, the bottom projection of the heating mechanism overlaps with the bottom projection of the combustion chamber 18 and the compensating oxidation mechanism, that is, the heating sleeve is just arranged on the periphery of the buffer chamber 17, the combustion chamber 18 and the protection chamber 19, and the edge is flush with the edge of the buffer chamber 17 and the protection chamber 19, wrapping the cavity that needs to be heated for heat dissipation, improving the heating effectiveness, and separating from the condensation chamber 16, improving the condensation effectiveness.
[0085] The present invention also proposes a high-purity selenium bottom blowing compensation oxidation method, such as Figure 4 The step flow chart of the high-purity selenium bottom blowing compensation oxidation method shown is implemented by relying on the high-purity selenium bottom blowing compensation oxidation device as described above, and the method includes the following steps:
[0086] S1, filling the selenium material into the crucible in the combustion chamber 18, and sealing the furnace body 1;
[0087] In this step, block selenium material is loaded into the graphite crucible 5, the purity of the selenium material can be 3N-5N, and the furnace cover 2 is closed and sealed.
[0088] S2, exhausting the air in the furnace body 1;
[0089] In this step, the second air inlet valve 12 and the air outlet valve 4 are opened to introduce oxygen into the tubular furnace at an oxygen flow rate of 0.9 L / min-1 L / min to exhaust the air in the tubular furnace.
[0090] S3, the heating mechanism heats the combustion chamber 18 and the compensating oxidation mechanism to the target temperature, and burns and melts the selenium material in the crucible into selenium liquid;
[0091] In this step, the heating device 13 is turned on, and the buffer chamber 17, the combustion chamber 18 and the protection chamber 19 are heated to between 300°C and 600°C respectively through the resistance wire 14 inside the heating device 13; the oxygen preheating device is turned on to preheat the oxygen in the intake pipe 10 and the blowback pipe 11 to between 300°C and 600°C; after the temperature of the combustion chamber 18 rises to 220°C-230°C, the selenium material begins to melt.
[0092] S4, the air inlet pipe 10 transmits oxygen into the selenium liquid for bottom blowing oxidation to obtain a mixed gas and high boiling point impurities;
[0093] In this step, when the temperature of the combustion chamber 18 rises to between 300°C and 600°C, the first air intake valve 7 is opened, and oxygen preheated to between 300°C and 600°C is blown into the selenium liquid through the microporous sleeve 15 at the end of the air intake pipe 10, and the oxygen flow rate is set to between 0.3L / min and 2L / min, and bottom blowing oxidation is performed, and then the timing starts. The elemental selenium in the raw material is oxidized into gaseous selenium dioxide under the action of a large number of tiny bubbles generated by the oxygen flow blown into the air intake pipe 10 and the oxygen on the surface of the melt, and a mixed gas mainly composed of selenium dioxide is obtained.
[0094] S5, the mixed gas is divided into two streams and enters the buffer chamber 17 and the protection chamber 19 respectively to be compensated for oxidation, thereby obtaining a target gas rich in selenium dioxide, and the high boiling point impurities remain in the crucible;
[0095] In this step, the mixed gas enters the buffer chamber 17 and the protection chamber 19 in turn, and the high-boiling-point impurities remain in the graphite crucible 5; the gaseous selenium element that is not completely oxidized is further oxidized in the buffer chamber 17 and the protection chamber 19, and the mixed gas such as gaseous selenium dioxide and selenium element that flows back into the protection chamber 19 returns to the combustion chamber 18 under the action of the oxygen flow introduced by the backblowing pipe 11.
[0096] S6, the target gas in the buffer chamber 17 enters the condensation chamber 16 for condensation, and the target gas in the protection chamber 19 flows back into the combustion chamber 18, and flows through the buffer chamber 17 to the condensation chamber 16 for condensation, thereby obtaining condensation products and non-target gas, and the non-target gas is discharged from the furnace body 1 through the gas outlet pipe 3;
[0097] In this step, the target gas is further oxidized to be rich in selenium dioxide and enters the condensation chamber 16 ; the condensation product is collected by the quartz collector 6 of the condensation chamber 16 , and the low-boiling impurities are discharged through the outlet pipe 3 for treatment.
[0098] S7. Collect the condensed product and obtain high-purity selenium through a reduction section and a vacuum distillation section.
[0099] In this step, the selenium material is completely burned in about 0.5h-2h, the heating device 13 and the oxygen preheating device are turned off, the first air inlet valve 7 is closed, and the temperature in the furnace is lowered to room temperature. The second air inlet valve 12 is closed, the oxygen supply is stopped, the furnace cover 2 is opened, the quartz collector 6 is taken out, and the condensed product is collected.
[0100] In this embodiment, the 3N-5N selenium material still contains a certain amount of impurities. These impurities will affect the performance and quality of the product in the application of high-purity selenium (such as semiconductors, solar cells, electronic components, etc.), and further purification is required to remove the residual impurities to obtain higher purity selenium to meet the needs of specific applications. The composition of the 3N-5N selenium material is mainly elemental selenium, which contains trace amounts of impurities.
[0101] As for the method embodiment, since it is basically similar to the device embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.
[0102] The following embodiments take 3N-5N selenium material as an example, and use a high-purity selenium bottom blowing compensation oxidation device to perform pre-oxidation of high-purity selenium. The device comprises: a tubular furnace, both ends of which are sealed by a left furnace cover 2 and a right furnace cover 2 respectively, the left side of the tubular furnace is connected to an air outlet pipe 3, and an air outlet valve 4 is arranged on the air outlet pipe 3; quartz collectors 6 numbered 1#-4#, 6#-7# and a graphite crucible 5 numbered 5# are respectively installed in the tubular furnace in the order of numbers, and form a condensation chamber 16, a buffer chamber 17, a combustion chamber 18 and a protection chamber 19 from left to right; the right side of the tubular furnace is connected to an air inlet pipe 10 and a blowback pipe 11, and a first air inlet valve 7 and a second air inlet valve 12 are respectively arranged on the air inlet pipe 10 and the blowback pipe 11, the end of the air inlet pipe 10 is connected to a microporous sleeve 15, the bottom wall of the microporous sleeve 15 is arranged at 1 / 10 of the pipe diameter from the bottom of the graphite crucible 5, and a pressure pipe 8 is connected to the air inlet pipe 10, and a pressure gauge 9 is arranged on the pressure pipe 8.
[0103] The present invention is described in detail below through specific examples.
[0104] Embodiment 1:
[0105] A high-purity selenium bottom blowing compensation oxidation method comprises the following steps:
[0106] S101, 200 g of block selenium material with a purity of 4N is loaded into the graphite crucible 5, the furnace cover 2 is closed and sealed, the second air inlet valve 12 and the air outlet valve 4 are opened, oxygen is introduced into the tubular furnace at an oxygen flow rate of 0.9 L / min, and the air in the tubular furnace is exhausted;
[0107] S102, turn on the heating device 13, and heat the buffer chamber 17 to about 345° C., the combustion chamber 18 and the protection chamber 19 to about 300° C. respectively through the resistance wire 14 inside the heating device 13; turn on the oxygen preheating device to preheat the oxygen in the intake pipe 10 and the blowback pipe 11 to about 300° C.;
[0108] S103, when the temperature of the combustion chamber 18 rises to about 220°C, the selenium material begins to melt; when the temperature of the combustion chamber 18 rises to about 300°C, the first air intake valve 7 is opened, and oxygen preheated to about 300°C is blown into the selenium liquid through the microporous sleeve 15 at the end of the air intake pipe 10, and the oxygen flow rate is set to 0.3L / min, and bottom blowing oxidation is performed, and timing is started at the same time;
[0109] S104, the selenium material is completely burned after about 1.5 hours, the heating device 13 and the oxygen preheating device are turned off, the first air inlet valve 7 is closed, and the temperature in the furnace is lowered to room temperature, the second air inlet valve 12 is closed, the oxygen is stopped, the furnace cover 2 is opened, the quartz collector 6 is taken out, and about 262.03g of condensed product is collected. The main component of the condensed product is selenium dioxide, and the yield of elemental selenium is 93.23%, and the oxidation rate is 133.33g / h.
[0110] Embodiment 2:
[0111] A high-purity selenium bottom blowing compensation oxidation method comprises the following steps:
[0112] S201, 200 g of block selenium material with a purity of 4N is loaded into the graphite crucible 5, the furnace cover 2 is closed and sealed, the second air inlet valve 12 and the air outlet valve 4 are opened, oxygen is introduced into the tubular furnace at an oxygen flow rate of 1.0 L / min, and the air in the tubular furnace is exhausted;
[0113] S202, turn on the heating device 13, and heat the buffer chamber 17 to about 550° C., the combustion chamber 18 and the protection chamber 19 to about 500° C. respectively through the resistance wire 14 inside the heating device 13; turn on the oxygen preheating device to preheat the oxygen in the intake pipe 10 and the blowback pipe 11 to about 500° C.;
[0114] S203, when the temperature of the combustion chamber 18 rises to about 220°C, the selenium material begins to melt; when the temperature of the combustion chamber 18 rises to about 300°C, the first air intake valve 7 is opened, and oxygen preheated to about 500°C is blown into the selenium liquid through the microporous sleeve 15 at the end of the air intake pipe 10, and the oxygen flow rate is set to 1L / min, and bottom blowing oxidation is performed, and timing is started at the same time;
[0115] S204, the selenium material is completely burned in about 0.5h, the heating device 13 and the oxygen preheating device are turned off, the first air inlet valve 7 is closed, and the temperature in the furnace is lowered to room temperature, the second air inlet valve 12 is closed, the oxygen is stopped, the furnace cover 2 is opened, the quartz collector 6 is taken out, and about 238.93g of condensed product is collected. The main component of the condensed product is selenium dioxide, and the yield of elemental selenium is 85.01%, and the oxidation rate is 400g / h.
[0116] Embodiment three:
[0117] A high-purity selenium bottom blowing compensation oxidation method comprises the following steps:
[0118] S301, 2 kg of block selenium material with a purity of 4N is loaded into the graphite crucible 5, the furnace cover 2 is closed and sealed, the second air inlet valve 12 and the air outlet valve 4 are opened, oxygen is introduced into the tubular furnace, and the oxygen flow rate is 0.9 L / min, and the air in the tubular furnace is exhausted;
[0119] S302, turn on the heating device 13, and heat the buffer chamber 17 to about 650°C, the combustion chamber 18 and the protection chamber 19 to about 600°C respectively through the resistance wire 14 inside the heating device 13; turn on the oxygen preheating device to preheat the oxygen in the intake pipe 10 and the blowback pipe 11 to about 600°C;
[0120] S303, when the temperature of the combustion chamber 18 rises to about 230°C, the selenium material begins to melt; when the temperature of the combustion chamber 18 rises to about 600°C, the first air intake valve 7 is opened, and oxygen preheated to about 600°C is blown into the selenium liquid through the microporous sleeve 15 at the end of the air intake pipe 10, the oxygen flow rate is set to 2L / min, bottom blowing oxidation is performed, and timing is started at the same time;
[0121] S304, the selenium material is completely burned in about 2 hours, the heating device 13 and the oxygen preheating device are turned off, the first air inlet valve 7 is closed, and the temperature in the furnace is lowered to room temperature, the second air inlet valve 12 is closed, the oxygen is stopped, the furnace cover 2 is opened, the quartz collector 6 is taken out, and about 2339.21g of condensed product is collected. The main component of the condensed product is selenium dioxide, and the yield of elemental selenium is 83.23%, and the oxidation rate is 1kg / h.
[0122] It can be seen from Examples 1 to 3 that pre-oxidation of high-purity selenium by using the high-purity selenium bottom blowing compensating oxidation device provided in the present application can improve the oxidation efficiency and promote the conversion of more elemental selenium into selenium dioxide, thereby improving the yield and purity of high-purity selenium.
[0123] It should be noted that the various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0124] It should also be noted that, in this article, the orientation or position relationship indicated by the terms "upper", "lower", "left", "right", "inside", "outside", etc. is based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. In addition, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations, nor can they be understood as indicating or implying relative importance. Moreover, the term "include" or any other variant thereof is intended to cover non-exclusive inclusion, so that a process, method, article or terminal device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or terminal device.
[0125] The above is a detailed introduction to a high-purity selenium bottom blowing compensation oxidation device and method provided by the present application. This article uses specific examples to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the present application, and the content of this specification should not be understood as a limitation on the present application. At the same time, for those of ordinary skill in the art, according to the present application, there will be different forms of changes in the specific implementation methods and application scopes. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived from this are still within the scope of protection of the present application.
Claims
1. A high-purity selenium bottom blowing compensation oxidation device, characterized in that: It comprises a furnace body, on which an air inlet pipe and an air outlet pipe are arranged; The furnace body is provided with: A combustion chamber, wherein a crucible is arranged inside, and the crucible is used to fill the selenium material; The compensating oxidation mechanism comprises a buffer chamber and a protection chamber, wherein the combustion chamber is arranged in communication between the buffer chamber and the protection chamber; a condensation chamber, communicated with the buffer chamber; A heating mechanism, arranged on the combustion chamber and the compensating oxidation mechanism; The air inlet pipe extends into the crucible in the combustion chamber, and the air outlet pipe is in communication with the condensation chamber; Among them, the heating mechanism heats the combustion chamber and the compensating oxidation mechanism, burns and melts the selenium material in the crucible into selenium liquid, the air inlet pipe inputs oxygen into the selenium liquid, performs bottom blowing oxidation to obtain a mixed gas, and the mixed gas is divided into two airflows and enters the buffer chamber and the protection chamber respectively to be compensated oxidized, so that the selenium dioxide content in the mixed gas is increased to obtain a target gas rich in selenium dioxide; the target gas flows into the condensation chamber, at least the selenium dioxide is condensed to obtain a condensation product and a non-target gas; the non-target gas is discharged from the furnace body through the air outlet pipe.
2. A high-purity selenium bottom blowing compensation oxidation device according to claim 1, characterized in that: The furnace body is also provided with a back-blowing pipe, which is connected to the protection chamber to blow oxygen into the protection chamber so that the target gas in the protection chamber flows back into the combustion chamber and flows to the condensation chamber through the buffer chamber.
3. A high-purity selenium bottom blowing compensation oxidation device according to claim 1, characterized in that: The outlet sleeve of the air inlet pipe in the crucible is provided with a microporous sleeve, and the microporous sleeve is spaced apart from the bottom of the crucible.
4. A high-purity selenium bottom blowing compensation oxidation device according to claim 3, characterized in that: The microporous sleeve is cylindrical, and a plurality of through holes are evenly spaced on the cylindrical wall.
5. A high-purity selenium bottom blowing compensation oxidation device according to claim 1, characterized in that: Along the flow direction of the mixed gas, the areas of the cavities of the protection chamber and the buffer chamber decrease in steps; along the flow direction of the target gas, the area of the cavity of the condensation chamber decreases in steps.
6. A high-purity selenium bottom blowing compensation oxidation device according to claim 5, characterized in that: The protection chamber, the buffer chamber and the condensation chamber are all composed of at least one quartz collector, and the interior of each quartz collector is hollow to form the cavity, and the cavity is trumpet-shaped.
7. A high-purity selenium bottom blowing compensation oxidation device according to claim 1, characterized in that: The heating mechanism is a heating sleeve, the interior of which is filled with resistance wires and is sleeved around the combustion chamber and the compensating oxidation mechanism.
8. A high-purity selenium bottom blowing compensation oxidation device according to claim 7, characterized in that: A bottom projection of the heating mechanism overlaps with bottom projections of the combustion chamber and the compensating oxidation mechanism.
9. A high-purity selenium bottom blowing compensation oxidation device according to claim 2, characterized in that: The device also includes an air outlet valve, a first air inlet valve, a second air inlet valve, a pressure gauge and two furnace covers, all of which are located outside the furnace body; wherein, The air outlet valve is arranged on the air outlet pipe; The first air intake valve and the pressure gauge are respectively arranged on the air intake pipe; The second air intake valve is arranged on the blowback pipe; The two furnace covers seal the openings at both ends of the furnace body, and the air inlet pipe, the air outlet pipe and the blowback pipe respectively penetrate the corresponding furnace covers and enter the furnace body; Wherein, the furnace cover is detachably connected to the furnace body.
10. A high-purity selenium bottom blowing compensation oxidation method, characterized in that: The method is implemented by using the high-purity selenium bottom blowing compensation oxidation device according to any one of claims 1 to 9, and the method comprises: Fill the selenium material into the crucible in the combustion chamber and seal the furnace body; Expelling air from the furnace body; The heating mechanism heats the combustion chamber and the compensating oxidation mechanism to a target temperature, and burns and melts the selenium material in the crucible into selenium liquid; The air inlet pipe transmits oxygen into the selenium liquid for bottom blowing oxidation to obtain mixed gas and high boiling point impurities; The mixed gas is divided into two gas streams which enter the buffer chamber and the protection chamber respectively to be compensated for oxidation, thereby obtaining a target gas rich in selenium dioxide, and the high boiling point impurities remain in the crucible; The target gas in the buffer chamber enters the condensation chamber for condensation, and the target gas in the protection chamber flows back into the combustion chamber and flows through the buffer chamber to the condensation chamber for condensation, thereby obtaining condensation products and non-target gas, which is discharged from the furnace body through the gas outlet pipe; The condensed product is collected and passed through a reduction section and a vacuum distillation section to obtain high-purity selenium.