Synthesis method of S-modulated Cu monatomic loaded red carbon nitride

The synthesis method of Cu single atom-loaded red carbon nitride modulated by S solves the stability and product type problems of red carbon nitride in photocatalytic CO2 reduction, improves the photocatalytic activity and CO2 reduction efficiency, and achieves photocatalytic CO2 reduction under visible light. High performance liquid phase product generation.

CN118719113AActive Publication Date: 2024-10-01JIANGSU UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410768854.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

In terms of photocatalytic CO2 reduction, red carbon nitride has problems such as easy recombination of photogenerated electrons and holes, poor stability, and mostly gas phase products. There are few studies on photocatalytic CO2 reduction to liquid phase products.

Method used

The S-modulated Cu single atom supported red carbon nitride is synthesized by mixing and grinding melamine, 2,4,6-triaminopyrimidine, thiocyanate and potassium chloride in a mortar, followed by programmed temperature rise and calcination. It was cooled under N2 atmosphere, then stirred with CuCl in ultrapure water, evaporated to dryness, and vacuum dried to prepare a Cu single atom-supported red carbon nitride photocatalyst.

Benefits of technology

It improves the photocatalytic activity and stability of red carbon nitride, promotes the separation of photogenerated electrons and holes, enhances the efficiency of CO2 reduction to ethanol, and achieves efficient reduction of CO2 to liquid products under visible light.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719113A_ABST
    Figure CN118719113A_ABST
Patent Text Reader

Abstract

The invention discloses a synthesis method of S-modulated Cu monatomic loaded red carbon nitride, which comprises the following steps: S1, fully mixing and grinding melamine, 2, 4, 6-triaminopyrimidine, trithiocyanuric acid and potassium chloride; s2, placing the mixed and ground powder in a porcelain boat, heating the porcelain boat to 500-600 DEG C, and then cooling the porcelain boat to room temperature to obtain S-modulated red carbon nitride; s3, adding the red carbon nitride prepared in the step S into a CuCl solution, stirring, and drying by distillation to obtain a product; and carrying out cleaning and vacuum drying on the dried product to obtain the S-modulated Cu monatomic loaded red carbon nitride sample. The method has the characteristics of few raw material types, simple operation method, simple process, environmental protection and the like, and the obtained S-modulated Cu monatomic loaded red carbon nitride can be efficiently reduced into ethanol through CO2 photocatalysis in a water phase.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalytic materials, in particular to a method for synthesizing a S-modulated Cu single-atom-loaded red carbon nitride system. Background Art

[0002] As a special metal-free semiconductor graphite phase carbon nitride material, it has an appropriate bandgap width (E g About 2.7eV), and visible light response ability, so graphite phase carbon nitride has a good prospect in the application of photocatalytic technology. So far, graphite phase carbon nitride semiconductor photocatalysts are mainly used for photocatalytic carbon dioxide reduction in the visible light region, photodecomposition of water to produce hydrogen, removal of pollutants in the environment, etc. However, since pure graphite phase carbon nitride has a relatively narrow visible light absorption range, people have developed a red carbon nitride to broaden the light absorption range. Despite this, red carbon nitride still has the disadvantages of easy recombination of photogenerated electrons and holes and poor stability. At the same time, the reduction products obtained by using red carbon nitride for CO2 reduction are mostly gas phase products such as CO and CH4, and there is little research on photocatalytic CO2 reduction to liquid phase products.

[0003] Therefore, modifying red carbon nitride to promote the photocatalytic reduction of CO2 to liquid products and improve stability has extremely important application value. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for synthesizing a S-modulated Cu single-atom-loaded red carbon nitride system.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] A method for synthesizing S-modulated Cu single-atom-loaded red carbon nitride comprises the following steps:

[0007] S1. Mix melamine, 2,4,6-triaminopyrimidine, thiocyanate and potassium chloride in a mortar and grind them thoroughly according to the proportions;

[0008] S2, placing the mixed and ground powder in a porcelain boat, heating it to the calcination temperature in a N2 atmosphere, calcining it for a period of time and then cooling it to room temperature, and washing it to obtain S-modulated red carbon nitride;

[0009] S3. Based on the mass of the S-modulated red carbon nitride sample, the mass of the added CuCl solid is calculated according to the mass percentage of the added Cu single atom, the S-modulated red carbon nitride and the CuCl solid are mixed and stirred in ultrapure water for a period of time and then evaporated to obtain a product; the evaporated product is washed and vacuum-dried to obtain the S-modulated Cu single atom-loaded red carbon nitride sample.

[0010] In step S1, the mass ratio of melamine, 2,4,6-triaminopyrimidine, thiocyanate and potassium chloride is 10:3:10:20, and the grinding time is 5-20 minutes.

[0011] In step S2, the calcination temperature is 500-600°C, the calcination time is 2-4 hours, the heating rate is 4-6°C / min; and the calcination is cooled to room temperature by natural cooling under N2 atmosphere.

[0012] In step S3, the amount of CuCl solid added is: the mass of Cu single atom is 0.5-3% of the mass of S-modulated red carbon nitride.

[0013] In step S3, the stirring time is 10-20 hours; and the evaporation temperature is 80-100°C.

[0014] In step S3, the cleaning method is: the product is filtered and washed with ultrapure water until the ion concentration is less than 20 ppm.

[0015] In step S3, the vacuum drying temperature is 50-70°C and the drying time is 10-15h.

[0016] In the present invention, by modifying red carbon nitride, the prepared S-modulated Cu single-atom-loaded red carbon nitride photocatalyst can be used to reduce CO2 under simulated sunlight.

[0017] The beneficial effects of the present invention are:

[0018] (1) The present invention prepares a S-modulated Cu single-atom-loaded red carbon nitride material, and the S modulation changes the chemical structure of the red carbon nitride, which is beneficial to the loading of the Cu single atom. The preparation method has the characteristics of simple operation method, simple process, green environmental protection, etc., and the obtained S-modulated Cu single-atom-loaded red carbon nitride has high photocatalytic activity and good stability.

[0019] (2) The catalyst prepared by the present invention is used to reduce CO2 under visible light, absorbs light energy to generate electron-hole pairs, and S acts as an aggregation center for photogenerated holes, thereby improving the separation efficiency of photogenerated electrons and holes and promoting the formation of electron-rich Cu sites, which is beneficial to the reduction of CO2 to produce ethanol. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a high-angle annular dark-field scanning transmission electron microscopy image of the product of Example 1 after spherical aberration correction;

[0021] Figure 2 This is the high-magnification X-ray photoelectron spectrum of the Cu element of the product of Example 1 and the red carbon nitride modulated with S;

[0022] Figure 3 This is the CO2 adsorption spectrum of the product of Example 1 and red carbon nitride modulated with S;

[0023] Figure 4 This is a comparison chart of the reduction performance of CO2 of the product of Example 1 and S-modulated red carbon nitride under simulated sunlight conditions.

[0024] Figure 5 This is a comparison chart of the CO2 reduction performance of the products obtained in Examples 1-3 of the present invention under simulated sunlight conditions. DETAILED DESCRIPTION

[0025] In order to further understand the features, technical means, specific objectives and functions of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0026] Example 1

[0027] A method for synthesizing S-modulated Cu single-atom-loaded red carbon nitride comprises the following steps:

[0028] S1. Weigh 1.0 g of melamine, 0.3 g of 2,4,6-triaminopyrimidine, 1.0 g of thiocyanate and 2.0 g of potassium chloride into a mortar and grind thoroughly for 10 minutes.

[0029] S2. Place the mixed and ground powder in a porcelain boat, heat the porcelain boat to 550°C at a heating rate of 5°C per minute in a N2 atmosphere, maintain for 3 hours, and then naturally cool to room temperature. After washing, S-modulated red carbon nitride is obtained. The room temperature is a temperature in the range of 20-30°C.

[0030] S3, weigh 1.0 g of S-modified red carbon nitride and 1% Cu atomic mass ratio of CuCl (15.6 mg of CuCl solid), disperse them in 80 ml of ultrapure water, stir for 18 hours, and evaporate to dryness in a water bath at 90° C. to obtain the product;

[0031] S4. The product obtained in S3 is filtered and washed with ultrapure water until the ionic strength of the filtered solution is less than 20 ppm, and then placed in a vacuum drying oven at 60° C. for 12 hours to obtain a S-modulated 1% Cu single-atom doped red carbon nitride sample.

[0032] Example 2

[0033] A method for synthesizing S-modulated Cu single-atom-loaded red carbon nitride comprises the following steps:

[0034] S1. Weigh 1.0 g of melamine, 0.3 g of 2,4,6-triaminopyrimidine, 1.0 g of thiocyanate and 2.0 g of potassium chloride into a mortar and grind thoroughly for 10 minutes.

[0035] S2. Place the mixed and ground powder in a porcelain boat, heat the porcelain boat to 550°C at a heating rate of 5°C per minute in a N2 atmosphere, maintain for 3 hours, and then naturally cool to room temperature. After washing, S-modulated red carbon nitride is obtained. The room temperature is a temperature in the range of 20-30°C.

[0036] S3, weigh 1.0 g of S-modified red carbon nitride and 0.5% Cu atomic mass ratio of CuCl (7.8 mg of CuCl solid), disperse them in 80 ml of ultrapure water, stir for 18 hours, and evaporate to dryness in a water bath at 95° C. to obtain the product;

[0037] S4. The product obtained in S3 is filtered and washed with ultrapure water until the ionic strength of the filtered solution is less than 20 ppm, and then placed in a vacuum drying oven at 60° C. for 12 hours to obtain a S-modulated 0.5% Cu single-atom-loaded red carbon nitride sample.

[0038] Example 3

[0039] A method for synthesizing S-modulated Cu single-atom-loaded red carbon nitride comprises the following steps:

[0040] S1. Weigh 1.0 g of melamine, 0.3 g of 2,4,6-triaminopyrimidine, 1.0 g of thiocyanate and 2.0 g of potassium chloride into a mortar and grind thoroughly for 10 minutes.

[0041] S2. Place the mixed and ground powder in a porcelain boat, heat the porcelain boat to 550°C at a heating rate of 5°C per minute in a N2 atmosphere, maintain for 3 hours, and then naturally cool to room temperature. After washing, S-modulated red carbon nitride is obtained. The room temperature is a temperature in the range of 20-30°C.

[0042] S3, weigh 1.0 g of S-modified red carbon nitride and 3% Cu atomic mass ratio of CuCl (46.8 mg of CuCl solid), disperse them in 80 ml of ultrapure water, stir for 18 hours, and evaporate to dryness in a water bath at 100° C. to obtain the product;

[0043] S4. The product obtained in S3 is filtered and washed with ultrapure water until the ionic strength of the filtered solution is less than 20 ppm, and then placed in a vacuum drying oven at 60° C. for 12 hours to obtain a S-modulated 3% Cu single-atom-loaded red carbon nitride sample.

[0044] Comparative Example

[0045] Melamine, 2,4,6-triaminopyrimidine, thiocyanate and potassium chloride are fully ground and calcined in one step to obtain a product, and the obtained product is washed and dried to obtain S-modulated red carbon nitride.

[0046] The performance of the red carbon nitride prepared in Example 1 was tested below.

[0047] The product of Example 1 was characterized by high-precision morphology using a high-angle annular dark-field scanning transmission electron microscope with spherical aberration correction. The red carbon nitride obtained in Example 1 is a Cu single-atom loading system modulated by S, as shown in the attached figure. Figure 1 shown.

[0048] The product obtained in Example 1 and the S-modulated red carbon nitride were characterized by an X-ray photoelectron spectrometer. The high-magnification X-ray photoelectron spectrum of the Cu element showed that the product obtained in Example 1 contained a single Cu atom, as shown in the attached Figure 2 shown.

[0049] The CO2 adsorption of the product obtained in Example 1 and the red carbon nitride modulated with S was analyzed by CO2 adsorption. Figure 3 As shown, the product obtained in Example 1 has higher CO2 adsorption performance. CO2 adsorption is a prerequisite for CO2 reduction. Higher CO2 adsorption performance is conducive to the photocatalytic CO2 reduction reaction.

[0050] The photocatalytic performance of the samples was evaluated by photocatalytic CO2 reduction in a CO2-filled reactor filled with water. The reactor was made of quartz glass and a xenon lamp (0.5 W / cm -2 ). Before the photocatalytic experiment, 10 mg of catalyst was weighed and dispersed in 10 ml of ultrapure water and placed in a reactor. The reactor containing the mixed solution was placed on a magnetic stirrer. Under the condition of no light, the mixed solution was stirred evenly by a magnetic stirrer to reach adsorption and desorption equilibrium with CO2. After 30 minutes, the xenon lamp was turned on to start the test. After five hours of light exposure, the gas phase product was tested by a gas chromatograph, and the liquid phase product was tested by a nuclear magnetic resonance spectrometer.

[0051] The reduction performance of the product obtained in Example 1 and the red carbon nitride modulated by S to CO2 under simulated sunlight is shown in the attached Figure 4 The yields of various products are shown in the figure, from which it can be seen that the products prepared by the present invention have good photocatalytic effect.

[0052] like Figure 5 As shown, the ethanol production in Example 1 reached 50.43 μmol / g / h, the ethanol production in Example 2 was 16.08 μmol / g / h, and the ethanol production in Example 3 was 7.76 μmol / g / h.

Claims

1. A method for synthesizing S-modulated Cu single-atom-supported red carbon nitride, characterized in that: The steps include: S1. Mix melamine, 2,4,6-triaminopyrimidine, thiocyanate and potassium chloride in a mortar and grind them thoroughly according to the proportions; S2, placing the mixed and ground powder in a porcelain boat, heating it to the calcination temperature in a N2 atmosphere, calcining it for a period of time and then cooling it to room temperature, and washing it to obtain S-modulated red carbon nitride; S3, based on the mass of the red carbon nitride sample modulated by S, the mass of the added CuCl solid is calculated according to the mass percentage of the added Cu single atom, the red carbon nitride modulated by S and the CuCl solid are mixed and stirred in ultrapure water for a period of time and then evaporated to dryness to obtain a product; The evaporated product is washed and vacuum dried to obtain a S-modulated Cu single-atom-loaded red carbon nitride sample.

2. The synthesis method according to claim 1, characterized in that In step S1, the mass ratio of melamine, 2,4,6-triaminopyrimidine, thiocyanate and potassium chloride is 10:3:10:20, and the grinding time is 5-20 minutes.

3. The synthesis method according to claim 1, characterized in that In step S2, the calcination temperature is 500-600°C, the calcination time is 2-4 hours, the heating rate is 4-6°C / min; and the calcination is cooled to room temperature by natural cooling under N2 atmosphere.

4. The synthesis method according to claim 1, characterized in that In step S3, the amount of CuCl solid added is: the mass of Cu single atom is 0.5-3% of the mass of S-modulated red carbon nitride.

5. The synthesis method according to claim 1, characterized in that In step S3, the stirring time is 10-20 hours; and the evaporation temperature is 80-100°C.

6. The synthesis method according to claim 1, characterized in that In step S3, the cleaning method is: the product is filtered and washed with ultrapure water until the ion concentration is less than 20 ppm.

7. The synthesis method according to claim 1, characterized in that In step S3, the vacuum drying temperature is 50-70°C and the drying time is 10-15h.

8. Use of the S-modulated Cu single-atom-supported red carbon nitride prepared by the synthesis method according to any one of claims 1 to 7 for reducing CO2 under simulated sunlight.

Citation Information

Patent Citations

  • Nitrogen-defect-containing porous carbon nitride supported monatomic copper catalyst and preparation method and light nitrogen fixation application thereof

    CN115069290A

  • Carbon nitride-loaded bimetallic monatomic catalyst as well as preparation method and application thereof

    CN115400775A

  • Copper monatomic catalyst as well as preparation method and application thereof

    CN116726972A