Lost foam casting method for square ram of machine tool part

Through vertical pouring, segmented processing and back exhaust pipe design, combined with CAE software simulation and pouring system optimization, the problem of slag inclusion and shrinkage cavities in the lost foam casting of the square ram of the machine tool part was solved, and the quality and quality of the castings were improved. processing effect.

CN118720055AInactive Publication Date: 2024-10-01WUHU RUYHOO CASTING

Patent Information

Application Number
CN202410859142.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The square ram of machine tool parts is prone to problems such as slag inclusion and end surface shrinkage during the lost foam casting process. The existing vertical casting method is difficult to effectively solve, resulting in poor quality castings and scrapping.

Method used

The lost foam casting method of vertical pouring and segmented processing is adopted. By making a foam model and setting a stepped direct exhaust pipe on the back, combined with CAE software simulation and pouring system optimization, the pouring temperature and composition are controlled, and the insulation riser is used. Feeding to ensure casting quality.

Benefits of technology

It effectively reduces the slag inclusion on the machined surface caused by gasified slag, reduces the problem of end-face shrinkage cavities, and improves the guide rail surface quality and overall processing effect of the casting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720055A_ABST
    Figure CN118720055A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lost foam casting, in particular to a machine tool part square ram lost foam casting method which comprises the following steps: S1, manufacturing a foam model; s2, vertical casting is conducted, and segmented treatment is conducted; s3, a pouring system is arranged, simulation is conducted through casting CAE software, technological parameters and the pouring speed are set, the pouring temperature is selected, and direct exhaust is arranged on the back; s4, coating, drying, reinforcing the model and modeling; s5, pouring is conducted; s6, cooling, taking out the casting, and machining to remove the sticking amount; the stepped direct exhaust pipe is designed on the back face of the pouring position, part of gasified slag can be directly discharged through the exhaust pipe, slag inclusion of a machining face caused by the gasified slag is reduced, and the problem of end face shrinkage can be effectively controlled by controlling components and inoculation according to the HT300 component requirement range, controlling the pouring temperature to be 1400 DEG C and reducing the pouring temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lost foam casting, in particular to a lost foam casting method for a square ram of a machine tool part. Background Art

[0002] The square slide of machine tool parts has very high requirements on casting quality. This part is 2550mm long, 420mm wide and 420mm high. This part has strict usage requirements. All four sides are guide surfaces, and the surface quality requirements are high. Slag and sand inclusions are not allowed during processing, and the wall thickness needs to be guaranteed according to the drawing dimensions.

[0003] At present, when the square ram is cast in full mold, the model can only be cast in vertical steps to ensure the processing quality of its guide surface. However, due to the large shrinkage of the molten iron during vertical casting, large shrinkage holes and slag inclusion defects on the end face of the square ram and the defect of the guide surface are easily caused. As the defect area is too large, it cannot be repaired and the part is scrapped.

[0004] Although the stepped pouring method is beneficial to the rapid filling of molten iron and the corresponding shrinkage compensation of the casting, the height of the model itself reaches more than 1800mm. In vertical casting, turbulence of molten iron is prone to occur, and the foam pyrolysis products are drawn into the molten iron. When the molten iron rises to the top surface, it cannot be discharged in time and accumulates on the side guide surface, resulting in slag inclusion defects on the surrounding guide surfaces.

[0005] Although vertical casting is beneficial to the processing quality of most of the guide rail surfaces around, a large amount of molten iron is required to compensate for shrinkage during the solidification of the molten iron in the lower part of the cavity after casting, which leads to shrinkage holes on the upper end surface of the casting. Therefore, a lost foam casting method for square ram of machine tool parts is urgently needed to solve the above problems. Summary of the invention

[0006] In view of this, the purpose of the present invention is to provide a lost foam casting method for a square ram of a machine tool part, so as to solve the problem of slag inclusion on the machining surface and shrinkage cavity on the end surface caused by gasified slag.

[0007] Based on the above purpose, the present invention provides a lost foam casting method for a square slide of a machine tool part, comprising the following steps: S1, making a foam model; S2, vertical casting and segmentation processing; S3, setting a pouring system and simulating it through casting CAE software, setting process parameters, pouring speed, selecting pouring temperature, and setting direct exhaust on the back; S4, coating, drying, reinforcing the model, and shaping; S5, pouring; S6, cooling, taking out the casting, and machining to remove the sticking.

[0008] Preferably, in step S1, a low-density copolymer foam board with a density of less than 20 Kg / m³ is used when making the foam model, and the internal structure of the foam is a honeycomb structure. At the same time, the square slide rail surface is increased in normal volume according to the lost foam casting through CNC machining, and the end slag discharge surface is increased by 20 mm to directly process the model.

[0009] Preferably, in step S2, the foam mold is made into three sections, each section is stood up and buried in sand, and a box is used for molding. When the three sections of the foam mold are matched together during the molding process, two φ34 round holes with a depth of 40 mm are opened on the matching surfaces respectively, and then a foam round rod with a size of φ33.5 and a length of 80 mm is made. During molding, after the first section is buried, the foam round rod is placed into the φ34 round hole, and then the φ34 round hole on the bottom surface of the end of the second section is bridged by the foam round rod, so that the second section of the foam mold is matched with the first section of the foam mold.

[0010] Preferably, in step S2, the box shape size is 1400mm*2300mm.

[0011] Preferably, in step S3, a stepped pouring system is selected, the guide surface is placed on the side, the thicker side at the end is used as the molding surface, and the thinner side at the end is used as the slag discharge surface. A paper tube is used for the inner runner, and multi-point dispersed injection is performed. A 500mm pot table is placed at the straight runner position. After the pouring system is set up, it is simulated on the casting CAE software. During the process, the position of the gate is adjusted until all the displayed defects are eliminated. Through the simulation of the casting CAE software, the position where shrinkage cavities and shrinkage may occur in the casting is located, and two insulation risers are placed at the bottom to compensate for shrinkage, and a stepped direct exhaust pipe is set on the back of the pouring position.

[0012] Preferably, in step S4, the three-stage foam model is first matched with each other and marked, and cloth-based tape is pasted on all the joints between the product model segments. After the product model is processed, the product model is coated with paint, and the Baume degree of the water-based paint is 55-75. The minimum thickness of the model coating is controlled to be 1.0-2.0 mm after three times of coating. Before molding, the inner gate on the three-stage foam mold and the direct exhaust pipe on the back are preset in advance, and alcohol paint is applied. The non-turnover molding process is adopted. When the buried sand molding starts, the resin addition ratio of the molding sand is 1.0%, and the molding sand strength is greater than 1.5 MPa. First, a layer of 200 mm molding sand is placed in the frame. After scraping and leveling, put in the first section of the foam mold after pouring coating, tamp it while burying sand, put a steel pipe with an outer diameter of 30mm and an inner diameter of 20mm on the inside, and wrap an air rope on the steel pipe. When molding, after the first section is buried, put the foam round rod into the φ34 round hole, and then use the foam round rod to bridge the φ34 round hole on the bottom surface of the second section end, so that the second section of the foam mold can be matched with the first section of the foam mold, and the gap is pasted with tape. After the third section of the foam mold is connected and buried in turn, two insulation risers are set on the bottom according to the process plan. After burying the sand, wait for the molding sand to solidify and gain strength. Turn the box over after 5-6 hours. After the molding is completed, fix the upper and lower molding sand boxes with clips, and hoist them to the pouring area after complete solidification.

[0013] Preferably, in step S5, iron weights are placed on the surface of the sand box before pouring, the weight of the iron weights is about 7 times the weight of the pouring, the composition and inoculation are controlled within the HT300 composition requirement range, and the pouring temperature is controlled to be 1400°C.

[0014] Preferably, in step S6, after pouring is completed, measurement is performed every 10 hours, and every 5 hours in the later period. The temperature of the casting in the sand mold is measured and recorded by a thermocouple pasted during molding. When the temperature drops to about 350°C, the sand is removed and the casting is lifted out. After cooling to room temperature, the pouring system, riser, etc. are removed and polished, and the excess 10 mm amount at the end of the casting is removed by machining.

[0015] The beneficial effects of the present invention are as follows: by vertical casting and vertical pouring, segmented processing can facilitate fixation to prevent dislocation during the sand burial process, thereby ensuring the quality of the square slide rail surface; at the same time, by designing a stepped direct exhaust pipe on the back of the pouring position, part of the gasified slag can be directly discharged through the exhaust pipe, thereby reducing slag inclusion on the machined surface caused by the gasified slag; and by controlling the composition and inoculation according to the HT300 composition requirement range and controlling the pouring temperature to 1400°C, lowering the pouring temperature can effectively control the end face shrinkage problem. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0017] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0018] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0019] like Figure 1 As shown, a lost foam casting method for a square slide of a machine tool part comprises the following steps: S1, making a foam model; S2, vertical casting and segmentation processing; S3, setting a pouring system and simulating it through casting CAE software, setting process parameters, pouring speed, selecting pouring temperature, and setting direct exhaust at the back; S4, spraying paint, drying, reinforcing the model, and shaping; S5, pouring; S6, cooling, taking out the casting, and machining to remove the sticking.

[0020] In step S1, in order to reduce the probability of slag inclusion defects in the casting process of the square slide rail surface, a low-density copolymer foam board with a density of less than 20Kg / m³ is used when making the foam model. The low-density copolymer has a low carbon content and contains oxygen atoms in the molecular structure. The internal structure of the foam is a honeycomb structure, which burns more fully than ordinary EPS foam and has less carbon residue. At the same time, the square slide rail surface is increased in normal volume according to the lost foam casting through CNC machining, and the end slag discharge surface is increased by 20mm to directly process the model.

[0021] In step S2, flat casting and parting and plate removal are adopted, long square bars are used as core bones, and round steel core supports are placed after the box is turned over. However, the core supports have color difference, which affects the use of the mold surface, and one of the guide surfaces of the square slide is used as the slag discharge surface, which easily leads to slag inclusion defects on the guide surface.

[0022] The method of flat casting and vertical pouring is also to separate the mold and remove the plate. First, lay the mold flat and bury the sand. After the mold and box are combined, stand the sand box up. The pouring basin is set on the side of the sand box. This solution is convenient for modeling, but there are safety risks in standing the sand box up, and a set of sand boxes needs to be redesigned and welded. This solution is not advisable.

[0023] Finally, vertical casting and segmented processing were adopted. The foam mold was made into three sections, each section was stood up and buried with sand, and box molding was used. The box molding size was 1400mm*2300mm. When the three sections of foam molds were matched together during the molding process, in order to ensure that the three sections of foam molds were well matched together during the molding process, two φ34 round holes with a depth of 40mm were opened on the matching surfaces respectively, and then foam round rods with a size of φ33.5 and a length of 80mm were made. During molding, after the first section was buried, the foam round rod was placed into the φ34 round hole, and then the φ34 round hole on the bottom surface of the end of the second section was bridged by the foam round rod, so that the second section of the foam mold was matched with the first section of the foam mold, which was convenient for fixation to prevent dislocation during the sand burying process and ensure the quality of the square slide rail surface.

[0024] In step S3, since the height of the square slide of the machine tool reaches 2550mm, which is a relatively tall casting, a stepped pouring system is selected, the guide surface is placed on the side, the thicker side at the end is used as the molding surface, and the thinner side at the end is used as the slag discharge surface. The inner runner adopts a paper tube and is injected at multiple points to ensure that the molten iron quickly fills the mold layer by layer, and the flow of the molten iron is fully considered to avoid other defects such as cold shut and insufficient pouring. Finally, a 500mm pot table is placed at the sprue position to increase the filling speed of the molten iron during pouring, so that the foam is quickly gasified and decomposed to ensure that the casting is well filled. After the pouring system is set up, it is simulated on the casting CAE software. The casting CAE software is a conventional existing simulation software and does not belong to the requirements of this application. Within the scope of protection sought, no further explanation is given. During the process, the position of the gate is adjusted until all the displayed defects are eliminated. Through the simulation of the casting CAE software, the position where shrinkage cavities and shrinkage may occur in the casting is located. Two insulation risers are placed on the bottom for shrinkage compensation. From the defect + liquid phase CAE analysis, it can be seen that the shrinkage cavities defects are moved to the upper part of the insulation riser, and the lower molten iron is well compensated for shrinkage during the solidification process. At the same time, because this piece is made and poured vertically, the foam gasification stroke is large, and the difficulty of gasified slag floating is increased. In order to facilitate exhaust and reduce the probability of box expansion, a stepped direct exhaust pipe is set on the back of the pouring position, which can allow part of the gasified slag to be directly discharged through the exhaust pipe to reduce the black slag on the machining surface caused by the gasified slag.

[0025] In step S4, the three sections of foam models are first matched with each other and marked, and cloth-based tapes are pasted at all the joints between the product model segments so that the tape can be torn off to remove the paint at that position and then the product model can be assembled. After the product model is processed, the product model is coated with paint. The Baume degree of the water-based paint is 55-75. The minimum thickness of the model coating is 1.0-2.0 mm after three coats of coating to prevent the thin coating in the hole from causing sand sticking. Before molding, the inner gates on the three sections of foam molds and the direct exhaust pipe on the back are preset in advance, and alcohol paint is applied. The non-turnover molding process is adopted. When starting buried sand molding, the resin addition ratio of the molding sand is 1.0%, and the molding sand strength is greater than 1.5 MPa. First, a layer of 200 is placed in the frame. After the mm molding sand is scraped flat, put in the first section of the foam mold after spraying, tamp the sand while burying it, put a steel pipe with an outer diameter of 30mm and an inner diameter of 20mm on the inside, and wrap an air rope on the steel pipe to fix the molding sand and reduce the heat dissipation of the molding sand in the hole to prevent core drift. During molding, after the first section is buried, put the foam round rod into the φ34 round hole, and then bridge the φ34 round hole on the bottom surface of the second section end with the foam round rod to make the second section of the foam mold fit together with the first section of the foam mold, and tape the gap, connect the third section of the foam mold in turn, and set two insulation risers on the bottom according to the process plan. After burying the sand, wait for the molding sand to solidify and gain strength, turn the box over after 5-6 hours, and after the molding is completed, fix the upper and lower molding sand boxes with clips, and hoist them to the pouring area after complete solidification.

[0026] In step S5, iron weights are placed on the surface of the sand box before pouring, and the weight of the iron weights is about 7 times the weight of the pouring weight to resist the pressure of molten iron pouring, the pressure formed after the foam gasification, and the expansion force of the ductile iron during the graphitization expansion process, so as to maintain the strength of the sand mold and make the casting self-expanding, so as to achieve the purpose of internal shrinkage compensation. The composition and inoculation are controlled according to the HT300 composition requirement range, and the pouring temperature is controlled to 1400°C. Lowering the pouring temperature can effectively control the shrinkage problem.

[0027] In step S6, after pouring is completed, measurement is performed every 10 hours, and every 5 hours in the later stage. The temperature of the casting in the sand mold is measured and recorded by the thermocouple pasted during molding. When the temperature drops to about 350°C, the sand is removed and the casting is lifted out. After cooling to room temperature, the pouring system, riser, etc. are removed and polished, and the excess 10mm amount at the end of the casting is removed by machining to ensure the quality of the square slide.

[0028] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention (including the claims) is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0029] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A lost foam casting method for square ram of machine tool parts, It is characterized in that The method comprises the following steps: S1, making a foam model; S2, vertical casting and segmented processing; S3, setting a pouring system and simulating it through casting CAE software, setting process parameters, pouring speed, selecting pouring temperature, and setting direct exhaust on the back; S4, coating, drying, reinforcing the model, and shaping; S5, pouring; S6, cooling, taking out the casting, and machining to remove the sticker.

2. A lost foam casting method for a square ram of a machine tool part according to claim 1, It is characterized in that In step S1, a low-density copolymer foam board with a density of less than 20 Kg / m³ is used to make the foam model. The internal structure of the foam is a honeycomb structure. At the same time, the square slide rail surface is increased in accordance with the normal lost foam casting through CNC machining, and the end slag discharge surface is increased by 20 mm to directly process the model.

3. A lost foam casting method for a square ram of a machine tool part according to claim 2, It is characterized in that In step S2, the foam mold is made into three sections, each section is stood up and buried in sand, and a box is used for molding. When the three sections of the foam mold are matched together during the molding process, two φ34 round holes with a depth of 40mm are opened on the matching surfaces respectively, and then a foam round rod with a size of φ33.5 and a length of 80mm is made. During molding, after the first section is buried, the foam round rod is placed into the φ34 round hole, and then the φ34 round hole on the bottom surface of the end of the second section is bridged by the foam round rod, so that the second section of the foam mold is matched with the first section of the foam mold.

4. A lost foam casting method for a square ram of a machine tool part according to claim 3, It is characterized in that In step S2, the box size is 1400mm*2300mm.

5. A lost foam casting method for a square ram of a machine tool part according to claim 3, It is characterized in that In step S3, a stepped pouring system is selected, the guide surface is placed on the side, the thicker side at the end is used as the molding surface, and the thinner side at the end is used as the slag discharge surface. A paper tube is used for the inner runner, and multi-point dispersed injection is performed. A 500mm pot table is placed at the straight runner position. After the pouring system is set up, it is simulated on the casting CAE software. During the process, the position of the gate is adjusted until all the displayed defects are eliminated. Through the simulation of the casting CAE software, the position where shrinkage cavities and shrinkage may occur in the casting is located, and two insulation risers are placed at the bottom to compensate for shrinkage, and a stepped direct exhaust pipe is set on the back of the pouring position.

6. A lost foam casting method for a square ram of a machine tool part according to claim 5, It is characterized in that In step S4, the three sections of foam models are first matched with each other and marked, and cloth-based tapes are pasted on all the joints between the product model segments. After the product model is processed, the product model is coated with paint, and the Baume degree of the water-based paint is 55-75. The minimum thickness of the model coating is controlled to be 1.0-2.0 mm after three coats of coating. Before molding, the inner gates on the three sections of foam molds and the direct exhaust pipe on the back are preset in advance, and alcohol paint is applied. The non-turnover molding process is adopted. When starting the buried sand molding, the resin addition ratio of the molding sand is 1.0%, and the molding sand strength is greater than 1.5 MPa. First, a layer of 200 mm molding sand is placed in the frame and then scraped flat. Finally, put in the first section of foam mold after pouring coating, tamp it while burying sand, put a steel pipe with an outer diameter of 30mm and an inner diameter of 20mm on the inside, and wrap an air rope on the steel pipe. When molding, after the first section is buried, put the foam round rod into the φ34 round hole, and then bridge the φ34 round hole on the bottom surface of the second section end with the foam round rod to make the second section of the foam mold fit together with the first section of the foam mold, and stick the gap with tape, and then connect and bury the third section of the foam mold in turn. Set two insulation risers on the bottom according to the process plan, wait for the molding sand to solidify and gain strength after burying the sand, turn over the box after 5-6 hours, and fix the upper and lower molding sand boxes with clips after the molding is completed. After it is completely solidified, lift it to the pouring area.

7. A lost foam casting method for a square ram of a machine tool part according to claim 6, It is characterized in that In step S5, iron weights are placed on the surface of the sand box before pouring. The weight of the iron weight is about 7 times the weight of the pouring. The composition and inoculation are controlled according to the HT300 composition requirement range, and the pouring temperature is controlled to be 1400°C.

8. A lost foam casting method for a square ram of a machine tool part according to claim 7, It is characterized in that In step S6, after pouring is completed, measurements are taken every 10 hours, and then every 5 hours in the later stage. The temperature of the casting in the sand mold is measured and recorded by the thermocouple pasted during molding. When the temperature drops to about 350°C, the sand is removed and the casting is lifted out. After cooling to room temperature, the pouring system, riser, etc. are removed and polished, and the excess 10 mm amount at the end of the casting is removed by machining.

Citation Information

Patent Citations

  • FMC (full mould casting) modeling method

    CN104070137A

  • Manufacturing method for machine tool castings

    CN113182493A

  • Casting process for full mold casting machine tool body

    CN115106501A

  • Casting process method for moving table of full-mold casting planer type milling machine

    CN116352044A

  • Lost foam of rotating shaft of wind driven generator and casting method of lost foam

    CN116765332A

Cited By

  • Lost foam casting method

    CN119681207A