Electromagnetic shielding camouflage coating and preparation method thereof
By dispersing glass fibers in electromagnetic shielding coatings and synthesizing Cr-MOF on carbon nanotubes, forming a conductive network, the problem of insufficient mechanical properties and thermal stability of the coating is solved, and the effect of high electromagnetic shielding ability and rapid drying and film formation is achieved. .
Patent Information
- Application Number
- CN202410735345.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-06-07
AI Technical Summary
The existing electromagnetic shielding coatings have shortcomings in mechanical properties and thermal stability, which leads to their prone to cracking when impacted or exposed to sunlight, affecting the electromagnetic shielding ability.
By dispersing glass fibers in the coating and synthesizing Cr-MOF on carbon nanotubes, a conductive network is formed to improve the mechanical properties and thermal stability of the coating while maintaining high electromagnetic shielding capabilities.
It realizes the high mechanical strength, thermal stability and rapid drying of the paint, and improves the service life and scope of application of electromagnetic shielded camouflage paint.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-performance coatings, and in particular relates to an electromagnetic shielding camouflage coating and a preparation method thereof. Background Art
[0002] With the rapid development of information technology, various electronic equipment and instruments will cause electromagnetic wave pollution and interference. Many buildings, vehicles and objects need to be coated with electromagnetic shielding materials to prevent interference. Electromagnetic shielding coatings are mainly used in electronics, electrical appliances, aviation, military industry, medical and chemical industries. Electromagnetic shielding coatings can be applied to the surface of substrates of various shapes and materials by spraying or brushing. They can form a conductive coating on the surface of the substrate that effectively shields electromagnetic waves. They have the main characteristics of thin coating, high absorption rate, absorption bandwidth, light weight and good thermal stability.
[0003] At present, the common electromagnetic shielding coatings are thermoplastic coatings and thermosetting coatings. Thermoplastic coatings generally use thermoplastic resins with relatively large molecular weight, dissolve them in organic solvents, and then apply them on the substrate. After the solvent evaporates and dries, the thermoplastic coating will form a uniform film and adhere to the substrate. Its disadvantages are that due to the lack of a curing process, the mechanical properties are weak and it is easy to be damaged by external forces. In addition, most organic solvents are toxic solvents, which are harmful to the environment and need to be sprayed in a fixed workshop.
[0004] Patent CN107236421A discloses an electromagnetic shielding coating, which is prepared from conductive agent, silicone resin, silane coupling agent and alcohol organic solvent. The obtained electromagnetic shielding coating can be cured naturally, has good adhesion, non-toxic solvent and less environmental damage. However, its physical strength is poor, and it will crack when hit or exposed to sunlight, which will reduce the effect of electromagnetic shielding coating or even make it ineffective.
[0005] Patent CN115746644A discloses a super weather-resistant camouflage coating and its preparation method, wherein a modified additive and polyacrylate are mixed to obtain an anti-ultraviolet resin, and then a homemade additive and a metal pigment are mixed to obtain a pigment, and finally a super weather-resistant camouflage coating with anti-ultraviolet, anti-oxidation, heat insulation and anti-cracking properties is obtained by mixing. The performance of the coating is enhanced by adding fillers to the coating.
[0006] However, in electromagnetic shielding coatings, if fillers are added to improve the mechanical properties of the coating, the fillers will occupy the space of the conductive network, causing the conductive network to be broken and the conductive performance to decrease, thereby reducing the electromagnetic shielding capability of the electromagnetic shielding coating; and camouflage coatings usually require spraying in multiple colors and areas, which takes more time for the coating to dry and form a film. Over-baking will also cause the coating to age and crack easily, resulting in reduced performance.
[0007] Therefore, there is no electromagnetic shielding camouflage coating which has high mechanical properties and thermal stability and does not affect the high electromagnetic shielding capability of the electromagnetic shielding camouflage coating so as to be suitable for the needs of corresponding fields. Summary of the invention
[0008] The purpose of the present invention is to solve the problem of how to make the camouflage paint have high electromagnetic shielding ability while having high-strength mechanical properties and thermal stability, so as to improve the mechanical strength, coating speed and service life of the camouflage paint.
[0009] The present invention improves the mechanical properties and thermal stability of the coating by dispersing glass fibers in the coating, and improves the electromagnetic shielding capability by synthesizing Cr-MOF on carbon nanotubes.
[0010] The purpose of the present invention can be achieved through the following technical solutions:
[0011] An electromagnetic shielding camouflage paint comprises the following raw materials in parts by mass:
[0012] 45-55 parts of functionalized glass fiber, 0.5-1.5 parts of silane coupling agent, 30-40 parts of organic solvent and 20-25 parts of film-forming resin.
[0013] The silane coupling agent is any one of 3-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane and aminopolydimethylsiloxane.
[0014] The organic solvent is any one of methanol, ethanol, isopropanol, propylene glycol methyl ether, dipropylene glycol methyl ether, n-butanol and isobutanol.
[0015] Functionalized glass fiber is prepared by the following steps:
[0016] Step 1: Add the Cr-MOF / carbon nanotube composite material to a mixture of thionyl chloride and N,N-dimethylformamide in a reaction kettle, and then react for 18-24 hours under a nitrogen atmosphere at 65-75° C., filter and vacuum dry at 45-55° C. to obtain an acylated composite material.
[0017] Step 2: Ultrasonic dispersion of the acylated composite material in tetrahydrofuran in a reaction kettle to obtain a dispersion, adding the amino glass fiber to the dispersion to react for 30-40 minutes, then filtering to obtain a precipitate, and vacuum drying the precipitate at 75-85° C. for 18-24 hours to obtain functionalized glass fiber.
[0018] Furthermore, in step 1, the dosage ratio of the Cr-MOF / carbon nanotube composite material to the mixed solution is 10-12 mg: 12-15 mL; and the volume ratio of thionyl chloride to N,N-dimethylformamide in the mixed solution is 20-25:1.
[0019] Furthermore, the concentration of the dispersion in step 2 is 0.1-0.15 mg / mL.
[0020] Further, the Cr-MOF / carbon nanotube composite material is prepared by the following steps:
[0021] S1. Carboxylated carbon nanotubes, CrCl3·6H2O, 2-aminoterephthalic acid and NaCl are mixed and ground at room temperature for 5-10 minutes to obtain a preligand, and then the preligand is transferred to an autoclave, heated to 148-152°C, reacted for 4-5 hours, the product is washed with ethanol and deionized water, and vacuum dried at 150°C for 10-12 hours to obtain the preligand.
[0022] S2. Add the preligand into sufficient chloroform, add 1,3-propanesulfonate after ultrasonic dispersion, stir for 12-16 hours, filter and wash with chloroform, and dry at 70-80°C to obtain a Cr-MOF / carbon nanotube composite material.
[0023] Furthermore, the mass ratio of carboxylated carbon nanotubes, CrCl3·6H2O, 2-aminoterephthalic acid and NaCl in S1 is 10-12:8-10:5-5.5:0.15-0.2.
[0024] Furthermore, the mass ratio of the preligand to 1,3-propane sultone in S2 is 5-6:0.65-0.8.
[0025] Further, the amino glass fiber is prepared by the following steps:
[0026] In a reaction kettle, the glass fiber is placed in an activation solution at 60-70° C. for activation for 2-3 hours, then filtered, and vacuum dried at 70-80° C. for 6-8 hours. Then, γ-aminopropyltriethoxysilane and anhydrous toluene are mixed in a mass ratio of 1-2:100 and added into the reaction kettle. The mixture is heated at 70-80° C. for 24-36 hours under a nitrogen atmosphere. After the reaction is completed, the precipitate is filtered to obtain a precipitate. The precipitate is washed with toluene, acetone, anhydrous ethanol and water in sequence. The precipitate is vacuum dried at 70-80° C. for 5-6 hours to obtain an amino glass fiber.
[0027] Furthermore, the activation solution is prepared by mixing ammonia water, deionized water and hydrogen peroxide in a volume ratio of 1:1:1.
[0028] Furthermore, the film-forming resin is at least one of epoxy resin, acrylic resin, silicone resin, alkyd resin, phenolic resin, polyurethane, and polyester resin.
[0029] A method for preparing an electromagnetic shielding camouflage coating, the method comprising the following steps:
[0030] The organic solvent and the film-forming resin are mixed and stirred evenly, and a silane coupling agent is added. After stirring evenly, the mixture is allowed to stand for a pre-reaction for 12-16 hours, and then functionalized glass fibers are added and ultrasonically dispersed to obtain an electromagnetic shielding camouflage coating.
[0031] Beneficial effects of the present invention:
[0032] (1) In the electromagnetic shielding camouflage paint prepared by the present invention, the glass fibers are evenly distributed in the paint, which improves the mechanical properties of the paint. By dispersing carbon nanotubes and Cr-MOF in the paint to form a conductive network, the paint has a high electromagnetic shielding ability. By evenly distributing the conductive network on the surface of the glass fibers, the connection between the conductive networks is enhanced, and the spatial influence of the glass fibers on the conductive network is reduced. At the same time, the paint has high thermal stability and can be quickly dried at high temperature to form a film in a short time. The film forming speed is fast and the practicality is high.
[0033] (2) The electromagnetic shielding camouflage paint prepared by the present invention improves the dispersibility of carbon nanotubes in the resin by carboxylating carbon nanotubes, and improves the interface bonding strength between the glass fiber and the resin matrix by compounding the carbon nanotubes with glass fiber, thereby improving the mechanical properties and physical strength of the paint. At the same time, by compounding the carboxylated carbon nanotubes with Cr-MOF, the carboxylated carbon nanotubes are evenly distributed on the glass fiber. The glass fiber serves as a connecting carrier, and the carbon nanotubes and Cr-MOF on the surface of the glass fiber form a conductive network, thereby improving the conductivity of the conductive network and allowing the paint to maintain excellent electromagnetic shielding capabilities.
[0034] (3) The preparation method of the present invention is simple. Camouflage pigments can be added to the resin to prepare camouflage coatings of different colors. The drying and film formation of the coating can be accelerated by heating. The Cr-MOF in the coating is synthesized by sulfonic acid ligands, has high stability, and can withstand high temperatures. The synergistic effect with glass fiber improves the thermal stability of the coating, so that the high-temperature drying and film-forming process does not affect the performance of the coating, and the coating has a wide range of applications. DETAILED DESCRIPTION
[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example
[0036] A method for preparing an electromagnetic shielding camouflage coating comprises the following steps:
[0037] Step 1: 10 g of carboxylated carbon nanotubes, 8 g of CrCl3·6H2O, 5 g of 2-aminoterephthalic acid and 0.15 g of NaCl were mixed and ground at room temperature for 5 min to obtain a preligand, and then the preligand was transferred to an autoclave, heated to 148°C, reacted for 4 h, the product was washed with ethanol and deionized water, and vacuum dried at 150°C for 10 h to obtain a preligand;
[0038] Step 2: Add 5 g of the preligand into sufficient chloroform and disperse by ultrasonic to obtain a preligand dispersion. Then add 0.65 g of 1,3-propanesulfonate into the preligand dispersion, stir for 12 h, filter and wash with chloroform, and dry at 70 ° C to obtain a Cr-MOF / carbon nanotube composite material.
[0039] Step 3: Add 5 g of Cr-MOF / carbon nanotube composite material to 6 L of thionyl chloride and N,N-dimethylformamide mixed solution in a reactor, wherein the volume ratio of thionyl chloride to N,N-dimethylformamide is 25:1, react for 18 h at 65 ° C in an argon atmosphere, filter and vacuum dry at 45 ° C, then ultrasonically disperse in tetrahydrofuran, add amino glass fiber and react for 30 min, filter and vacuum dry the precipitate at 75 ° C for 18 h to obtain functionalized glass fiber;
[0040] Step 4: Mix 300g of ethanol and 200g of epoxy resin, stir evenly, add 5g of 3-aminopropyltriethoxysilane, stir evenly and let stand for pre-reaction for 12h, then add 450g of functionalized glass fiber and ultrasonically disperse evenly to obtain electromagnetic shielding camouflage coating.
[0041] Aminated glass fiber is prepared by the following steps:
[0042] In a reactor, 450 g of glass fiber was placed in an activation solution and activated at 60° C. for 2 hours, then filtered and vacuum dried at 70° C. for 6 hours. Then, γ-aminopropyltriethoxysilane and anhydrous toluene were mixed in a mass ratio of 1:100 and added into the reactor. The mixture was heated at 70° C. for 24 hours under a nitrogen atmosphere. After the reaction was completed, the precipitate was filtered to obtain the precipitate. The precipitate was washed with toluene, acetone, anhydrous ethanol and water in turn. The precipitate was vacuum dried at 70° C. for 5 hours to obtain amino glass fiber.
[0043] The activation solution is prepared by mixing ammonia water, deionized water and hydrogen peroxide in a volume ratio of 1:1:1. Example
[0044] A method for preparing an electromagnetic shielding camouflage coating comprises the following steps:
[0045] Step 1: 11 g of carboxylated carbon nanotubes, 9 g of CrCl3·6H2O, 5.2 g of 2-aminoterephthalic acid and 0.18 g of NaCl were mixed and ground at room temperature for 8 min to obtain a preligand, and then the preligand was transferred to an autoclave, heated to 150°C, reacted for 4.5 h, the product was washed with ethanol and deionized water, and vacuum dried at 150°C for 11 h to obtain a preligand;
[0046] Step 2: Add 5.5 g of the preligand into sufficient chloroform, disperse by ultrasonication to obtain a preligand dispersion, then add 0.7 g of 1,3-propanesulfone into the preligand dispersion, stir for 14 h, filter and wash with chloroform, and dry at 75 °C to obtain a Cr-MOF / carbon nanotube composite material.
[0047] Step 3, in a reactor, add 5.5g of Cr-MOF / carbon nanotube composite material to 7L of a mixed solution of thionyl chloride and N,N-dimethylformamide, the volume ratio of thionyl chloride to N,N-dimethylformamide is 22:1, react for 21h at 70°C in an argon atmosphere, filter and vacuum dry at 50°C, then ultrasonically disperse in tetrahydrofuran, add amino glass fiber and react for 35min, filter and vacuum dry the precipitate at 80°C for 21h to obtain functionalized glass fiber;
[0048] Step 4: Mix 350g of n-butanol and 225g of phenolic resin, stir evenly, add 10g of 3-aminopropyltrimethoxysilane, stir evenly and let stand for pre-reaction for 14h, then add 500g of functionalized glass fiber and ultrasonically disperse evenly to obtain electromagnetic shielding camouflage coating.
[0049] Aminated glass fiber is prepared by the following steps:
[0050] In a reactor, 500 g of glass fiber was placed in an activation solution and activated at 65° C. for 2.5 hours, then filtered and vacuum dried at 75° C. for 7 hours. Then, γ-aminopropyltriethoxysilane and anhydrous toluene were mixed in a mass ratio of 1.5:100 and added into the reactor. The mixture was heated at 75° C. for 30 hours under a nitrogen atmosphere. After the reaction was completed, the precipitate was filtered to obtain a precipitate. The precipitate was washed with toluene, acetone, anhydrous ethanol and water in turn. The precipitate was vacuum dried at 75° C. for 5.5 hours to obtain amino glass fiber.
[0051] The activation solution is prepared by mixing ammonia water, deionized water and hydrogen peroxide in a volume ratio of 1:1:1. Example
[0052] A method for preparing an electromagnetic shielding camouflage coating comprises the following steps:
[0053] Step 1: 12 g of carboxylated carbon nanotubes, 10 g of CrCl3·6H2O, 5.5 g of 2-aminoterephthalic acid and 0.2 g of NaCl were mixed and ground at room temperature for 10 min to obtain a preligand, and then the preligand was transferred to an autoclave, heated to 152°C, reacted for 5 h, the product was washed with ethanol and deionized water, and vacuum dried at 150°C for 12 h to obtain a preligand;
[0054] Step 2: Add 6 g of the preligand into sufficient chloroform and disperse by ultrasonic to obtain a preligand dispersion. Then add 0.8 g of 1,3-propanesulfonate into the preligand dispersion, stir for 16 h, filter and wash with chloroform, and dry at 80 ° C to obtain a Cr-MOF / carbon nanotube composite material.
[0055] Cr-MOF is formed using 2-aminoterephthalic acid as a ligand. The amino group in the Cr-MOF ligand reacts with carboxylated carbon nanotubes to generate Cr-MOF on the surface of the carboxylated carbon nanotubes. 1,3-propane sultone undergoes a ring-opening reaction with the amino group on the Cr-MOF to obtain sulfonic acid-functionalized Cr-MOF. The Cr-MOF containing sulfonic acid has stronger conductive properties and stronger electromagnetic shielding capabilities.
[0056] Step 3: Add 6 g of Cr-MOF / carbon nanotube composite material to 7.5 L of a mixed solution of thionyl chloride and N,N-dimethylformamide in a reaction kettle, wherein the volume ratio of thionyl chloride to N,N-dimethylformamide is 20:1, react for 24 h at 75 ° C in an argon atmosphere, filter and vacuum dry at 55 ° C, then ultrasonically disperse in tetrahydrofuran, add amino glass fiber and react for 40 min, filter and vacuum dry the precipitate at 85 ° C for 24 h to obtain functionalized glass fiber;
[0057] The acyl groups on the surface of the carbon nanotubes combine with the amino groups on the surface of the glass fibers to form amide bonds, so that the Cr-MOF / carbon nanotube composite material and the amino-treated glass fibers are chemically bonded together and evenly distributed; the carbon nanotubes attached to the surface of the glass fibers can fill the grooves and defects on the surface of the glass fibers, improving the bending and tensile properties of the fibers.
[0058] Step 4: Mix 400g of isobutyl alcohol and 250g of acrylic resin, stir evenly, add 15g of amino polydimethylsiloxane, stir evenly and let stand for pre-reaction for 16h, then add 550g of functionalized glass fiber and disperse evenly by ultrasonic to obtain electromagnetic shielding camouflage coating.
[0059] Glass fiber can improve the mechanical properties and heat resistance of the coating and has corrosion resistance. The carbon nanotubes on the surface of the functionalized glass fiber can enhance the dispersion of the functionalized glass fiber in the film-forming resin, and also disperse the Cr-MOF, thereby improving the electromagnetic shielding capability of the coating. The ligand of Cr-MOF is a sulfonic acid group, which makes Cr-MOF highly stable and heat-resistant, further improving the heat resistance of the coating and allowing the organic solvent to evaporate quickly at high temperatures, so that the coating can be quickly formed.
[0060] Aminated glass fiber is prepared by the following steps:
[0061] In a reactor, 550 g of glass fiber was placed in an activation solution and activated at 70°C for 3 hours, then filtered and vacuum dried at 80°C for 8 hours. Then, γ-aminopropyltriethoxysilane and anhydrous toluene were mixed in a mass ratio of 2:100 and added into the reactor. The mixture was heated at 80°C for 36 hours under a nitrogen atmosphere. After the reaction was completed, the precipitate was filtered to obtain the precipitate. The precipitate was washed with toluene, acetone, anhydrous ethanol and water in turn. The precipitate was vacuum dried at 80°C for 6 hours to obtain amino glass fiber.
[0062] The activation solution is prepared by mixing ammonia water, deionized water and hydrogen peroxide in a volume ratio of 1:1:1.
[0063] Because MOF has high conductivity, it can improve electromagnetic shielding ability, but MOF has high agglomeration in resin and cannot be dispersed in coating. Therefore, by combining MOF with carbon nanotubes, carbon nanotubes have good dispersion in the resin matrix, which improves the dispersion of functionalized glass fibers in the resin, and improves the electromagnetic shielding ability of electromagnetic shielding coatings and mechanical strength. The thermal stability of the material is improved, and the drying time of the coating can be accelerated by higher temperature.
[0064] Comparative Example 1
[0065] The difference from Example 1 is that carboxylated carbon nanotubes are used instead of functionalized glass fibers;
[0066] The ethanol and epoxy resin were mixed and stirred evenly, 3-aminopropyltriethoxysilane was added, stirred evenly and allowed to stand for pre-reaction for 12 hours, and then carboxylated carbon nanotubes were added and ultrasonically dispersed to obtain an electromagnetic shielding camouflage coating.
[0067] Comparative Example 2
[0068] The difference from Example 1 is that the functionalized glass fiber is replaced by an equal mass of glass fiber and an equal mass of carboxylated carbon nanotubes;
[0069] The ethanol and epoxy resin were mixed and stirred evenly, 3-aminopropyltriethoxysilane was added, stirred evenly and allowed to stand for pre-reaction for 12 hours, and then glass fiber and carboxylated carbon nanotubes were added and ultrasonically dispersed to obtain an electromagnetic shielding camouflage coating.
[0070] Comparative Example 3
[0071] The difference from Example 1 is that graphene oxide is used instead of the functionalized glass fiber;
[0072] The ethanol and epoxy resin were mixed and stirred evenly, 3-aminopropyltriethoxysilane was added, stirred evenly and allowed to stand for a pre-reaction for 12 hours, and then graphene oxide was added and ultrasonically dispersed to obtain an electromagnetic shielding camouflage coating.
[0073] In the examples and comparative examples, the glass fibers were purchased from Hangzhou Gaoke Composite Materials Co., Ltd., and the fiber length was 3 mm.
[0074] The carboxylated carbon nanotubes are carboxylated multi-walled carbon nanotubes with a diameter of 50-100 nm, purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.
[0075] Silane coupling agent, organic solvent, film-forming resin, hydrogen peroxide, anhydrous ethanol, acetone, anhydrous toluene, and graphene oxide were all purchased from Sigma-Aldrich.
[0076] Performance tests were performed on Examples 1 to 3 and Comparative Examples 1 to 3. According to GJB6190-2008, the shielding effectiveness of the electromagnetic shielding materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3 was tested in the range of 100 MHz to 10 GHz. The results are shown in Table 1.
[0077]
[0078] It can be seen from Table 1 that the electromagnetic shielding materials prepared in Examples 1 to 3 have good shielding effectiveness in the range of 100MHz-10GHz; in Comparative Example 1, the carboxylated carbon nanotubes have good dispersion in the numerical value, so that Example 1 has good electromagnetic shielding ability, but the ability is worse than that of Examples 1 to 3. In Comparative Example 2, the glass fiber has poor dispersion in the resin and affects the dispersion of the carboxylated carbon nanotubes, occupying a large amount of conductive network space formed by the carboxylated carbon nanotubes, and has poor electrostatic shielding ability; Comparative Example 3 has poor electrostatic shielding ability than Comparative Example 1 due to the poor dispersion of graphene oxide in the resin.
[0079] Performance tests were performed on Examples 1 to 3 and Comparative Examples 1 to 3. According to GB / T1732-2020, the electromagnetic shielding materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were respectively subjected to coating impact strength tests, and crack conditions were checked. The results are shown in Table 2:
[0080]
[0081] It can be seen from the data in Table 2 that the electromagnetic shielding camouflage coatings prepared in Examples 1 to 3 of the present invention have excellent impact resistance and strong mechanical properties, and no cracks appear after testing; since only electrostatic shielding materials are added to the coatings in Comparative Examples 1 and 3, the impact resistance of the coatings is not enhanced. Since the glass fibers in Comparative Example 2 agglomerate in the coating, the filler distribution in the coating is uneven, and the coating is prone to cracking when subjected to external force, Comparative Example 2 has the lowest impact resistance.
[0082] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0083] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An electromagnetic shielding camouflage paint, characterized in that: The following raw materials are included by mass: 45-55 parts of functionalized glass fiber, 0.5-1.5 parts of silane coupling agent, 30-40 parts of organic solvent and 20-25 parts of film-forming resin; Camouflage pigments are added to the resin to produce camouflage paints of different colors; The functionalized glass fiber is prepared by the following steps: Step 1, adding the Cr-MOF / carbon nanotube composite material to a mixed solution of thionyl chloride and N,N-dimethylformamide in a reaction kettle, and then reacting for 18-24 hours under a nitrogen atmosphere at 65-75° C., filtering and vacuum drying at 45-55° C. to obtain an acylated composite material; Step 2: ultrasonically disperse the acylated composite material in tetrahydrofuran in a reaction kettle to obtain a dispersion, add the amino glass fiber to the dispersion to react for 30-40 minutes, then filter to obtain a precipitate, and vacuum dry the precipitate at 75-85° C. for 18-24 hours to obtain the functionalized glass fiber; The Cr-MOF / carbon nanotube composite material is prepared by the following steps: S1, mixing carboxylated carbon nanotubes, CrCl3·6H2O, 2-aminoterephthalic acid and NaCl and grinding at room temperature for 5-10 minutes to obtain preligand 1, then transferring preligand 1 to an autoclave, heating to 148-152°C, reacting for 4-5 hours, washing the product with ethanol and deionized water, and vacuum drying at 150°C for 10-12 hours to obtain preligand 2; S2, adding preligand 2 to a sufficient amount of chloroform, adding 1,3-propane sultone after ultrasonic dispersion, stirring for 12-16 hours, filtering and washing with chloroform, and drying at 70-80° C. to obtain a Cr-MOF / carbon nanotube composite material; The amino glass fiber is prepared by the following steps: In a reaction kettle, the glass fiber is placed in an activation solution at 60-70° C. for activation for 2-3 hours, filtered, and vacuum dried at 70-80° C. for 6-8 hours. Then, γ-aminopropyltriethoxysilane and anhydrous toluene are mixed in a mass ratio of 1-2:100 and added into the reaction kettle. The mixture is heated at 70-80° C. for 24-36 hours under a nitrogen atmosphere. After the reaction is completed, the precipitate is filtered to obtain a precipitate. The precipitate is washed with toluene, acetone, anhydrous ethanol and water in sequence. The precipitate is vacuum dried at 70-80° C. for 5-6 hours to obtain an amino glass fiber. The activation solution is prepared by mixing ammonia water, deionized water and hydrogen peroxide in a volume ratio of 1:1:
1.
2. The method for preparing an electromagnetic shielding camouflage coating according to claim 1, characterized in that: In step 1, the dosage ratio of the Cr-MOF / carbon nanotube composite material to the mixed solution is 10-12 mg: 12-15 mL; the volume ratio of thionyl chloride to N,N-dimethylformamide in the mixed solution is 20-25:
1.
3. The method for preparing an electromagnetic shielding camouflage coating according to claim 1, characterized in that: The concentration of the dispersion in step 2 is 0.1-0.15 mg / mL.
4. The method for preparing an electromagnetic shielding camouflage coating according to claim 1, characterized in that: The mass ratio of the carboxylated carbon nanotubes, CrCl3·6H2O, 2-aminoterephthalic acid and NaCl in S1 is 10-12:8-10:5-5.5:0.15-0.
2.
5. The method for preparing an electromagnetic shielding camouflage coating according to claim 1, characterized in that: The mass ratio of the preligand 2 to 1,3-propane sultone in S2 is 5-6:0.65-0.
8.
6. The electromagnetic shielding camouflage paint according to claim 1, characterized in that: The silane coupling agent is any one of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, and aminopolydimethylsiloxane; The organic solvent is any one of methanol, ethanol, isopropanol, propylene glycol methyl ether, dipropylene glycol methyl ether, n-butanol, and isobutanol; The film-forming resin is at least one of epoxy resin, acrylic resin, silicone resin, alkyd resin, phenolic resin, polyurethane and polyester resin.
7. The method for preparing an electromagnetic shielding camouflage coating according to claim 1, characterized in that: The method comprises the following steps: The organic solvent and the film-forming resin are mixed and stirred evenly, and a silane coupling agent is added. After stirring evenly, the mixture is allowed to stand for a pre-reaction for 12-16 hours, and then functionalized glass fibers are added and ultrasonically dispersed to obtain an electromagnetic shielding camouflage coating.
Citation Information
Patent Citations
Electromagnetic shielding coating
CN107236421A
Aminated glass fibers, preparation method and applications thereof
CN110590186A
Glass fiber surface modification method and application thereof in PA66 / GF composite material
CN113929937A