Processing technology of high-strength and corrosion-resistant precision stainless steel strip
By making a composite nano container technology of mesoporous silica and dopamine-modified molybdenum disulfide on stainless steel belts, combined with sustained release agents and aqueous epoxy resins, the problem of insufficient corrosion resistance in extreme environments is solved. It has achieved improvements in high strength and corrosion resistance and is suitable for chemical and marine engineering and other fields.
Patent Information
- Application Number
- CN202411225047.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-03
AI Technical Summary
Traditional stainless steel belts perform poorly in extreme corrosion environments and fail to reach the required level, resulting in insufficient reliability and durability in applications in chemical, marine engineering and other fields.
The homemade mesoporous silica is used as the packaging container, combined with phytic acid, hydroxylamine sulfate/ammonium molybdate as the sustained release agent, and the dopamine-modified molybdenum disulfide is used as the template to grow in situ on the zeolite imidazole skeleton to form multiple layers Structural nanocomposite materials are blended with aqueous epoxy resin to prepare corrosion-resistant coatings, and high-strength corrosion-resistant precision stainless steel belts are prepared through rolling, bright solution annealing, degreasing, coating coating and other processes.
It significantly improves the corrosion resistance of stainless steel strips, provides physical barrier and chemical corrosion resistance, enhances its resistance to corrosive media, and shows excellent corrosion resistance in acidic environments.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of stainless steel strips, in particular to a processing technology for high-strength, corrosion-resistant, precision stainless steel strips. Background Art
[0002] When it comes to the processing of high-strength, corrosion-resistant precision stainless steel strips, corrosion resistance is undoubtedly one of its most attractive features. In many key fields, such as chemical industry, marine engineering, food processing, etc., the corrosion resistance of materials is a crucial consideration. Traditional stainless steel strips often perform poorly in these extreme environments because their corrosion resistance does not reach the required level.
[0003] Therefore, the importance of the processing technology of high-strength, corrosion-resistant, precision stainless steel strips is highlighted. Through a carefully designed process and targeted material engineering methods, the stainless steel strips can maintain their structural integrity and performance stability in a highly corrosive environment. This processing technology can not only improve the corrosion resistance of the stainless steel strips, but also maintain their high strength and precision dimensions, thus meeting the urgent needs of modern industry for high-performance materials.
[0004] Therefore, corrosion resistance, as one of the key characteristics of the high-strength, corrosion-resistant precision stainless steel strip processing technology, not only improves the reliability and durability of the material in specific engineering applications, but also injects new vitality into the technological development and progress in related fields. Summary of the invention
[0005] The object of the present invention is to provide a processing technology for high-strength, corrosion-resistant, precision stainless steel strips to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] The processing technology of high-strength corrosion-resistant precision stainless steel strip includes the following steps:
[0008] S1: Add 2-methylimidazole to deionized water, add encapsulated corrosion inhibitor mesoporous silica and dopamine-modified molybdenum disulfide, ultrasonically disperse, heat to 35-37°C, ultrasonically disperse zinc phytate in deionized water and add thereto, keep warm for 24 hours, centrifuge, wash, and vacuum dry at 60°C for 24 hours to obtain an intermediate; add the intermediate to an aqueous solution composed of cobalt nitrate hexahydrate and 2-methylimidazole, stir for 15-30 minutes, centrifuge, wash, and vacuum dry at 60°C for 24 hours to obtain nanoparticles. Rice composite material; ultrasonically dispersing the nanocomposite material in an ethanol solution of nickel nitrate hexahydrate, stirring evenly, adding a sodium phytate solution, adjusting the pH to 10-10.5, heating to 60-65°C in a nitrogen atmosphere for reaction for 24 hours, centrifuging, and vacuum drying at 80°C for 12-24 hours to obtain a multi-layer structure nanocomposite material; ultrasonically dispersing the multi-layer structure nanocomposite material in deionized water, adding the dispersion into a water-based epoxy resin, ultrasonically dispersing, adding a curing agent, stirring evenly, and obtaining a corrosion-resistant coating;
[0009] S2: The stainless steel strip raw material is sequentially rolled, bright solution annealed, secondary rolled, degreased, coated, tension leveled, and sheared to obtain a high-strength, corrosion-resistant, precision stainless steel strip.
[0010] Furthermore, the stainless steel strip raw material is a 301 stainless steel strip with a thickness of 0.8 mm to 1.0 mm.
[0011] Furthermore, the rolling step includes rolling the stainless steel strip 5-6 times to obtain a stainless steel strip with a thickness of 0.3-0.4 mm.
[0012] Furthermore, the bright solution annealing step includes setting the annealing temperature to 1050-1060° C., setting the production process with a TV value of 8.5, and controlling the final grain size GS No. 9.5-10.0.
[0013] Furthermore, the rollers used in the secondary rolling are subjected to sandblasting and roughening treatment.
[0014] Furthermore, the coating has a coating thickness of 80-100 μm.
[0015] Furthermore, in the intermediate, Zn in zinc phytate 2+ The molar ratio of molybdenum disulfide in 2-methylimidazole: dopamine modified molybdenum disulfide is (45-60): 1: (1.5-2); the mass ratio of zinc phytate: encapsulated corrosion inhibitor mesoporous silica is 1: 1.
[0016] Furthermore, in the nanocomposite material, the mass ratio of the intermediate: cobalt nitrate hexahydrate: 2-methylimidazole is (0.1-0.2):0.1:1.
[0017] Furthermore, in the multi-layer structure nanocomposite material, the mass ratio of the nanocomposite material: nickel nitrate hexahydrate: sodium phytate is 100:80:(230.9-277.1).
[0018] Furthermore, in the corrosion-resistant coating, the multi-layer structure nanocomposite material is added in an amount of 0.6-1.5wt% of the mass of the waterborne epoxy resin.
[0019] Furthermore, the preparation process of the mesoporous silica encapsulating the corrosion inhibitor comprises the following steps:
[0020] Step (1): add hexadecyltrimethylammonium bromide to deionized water, adjust the pH to 12-12.5, heat to 80-85°C, add ethyl silicate, keep warm for 2-3 hours, centrifuge, wash, add the crude product to 0.8mL / 100mL methanol solution of concentrated hydrochloric acid, heat to 65°C, stir overnight, and vacuum dry at 65°C for 12 hours to obtain mesoporous silica;
[0021] Step (2): heat the mesoporous silica to 120°C for activation for 2 hours, place the activated mesoporous silica in a corrosion inhibitor solution, evacuate, stir for 6-8 hours, centrifuge, and vacuum dry at 60°C for 12 hours to obtain the corrosion inhibitor encapsulated mesoporous silica.
[0022] Furthermore, in the mesoporous silica, the mass ratio of hexadecyltrimethylammonium bromide:ethyl silicate is (1-2):(5-10); in the encapsulated corrosion inhibitor mesoporous silica, the sustained-release agent solvent includes any one of a phytic acid-hydroxylamine sulfate solution and a phytic acid-ammonium molybdate solution; in the phytic acid-hydroxylamine sulfate solution, the molar ratio of phytic acid:hydroxylamine sulfate is (2-3):(1-1.5); in the phytic acid-ammonium molybdate solution, the molar ratio of phytic acid:ammonium molybdate is (1.6-2):(1-1.4); the mass ratio of corrosion inhibitor in the mesoporous silica:corrosion inhibitor solution is 1:10.
[0023] Furthermore, the solutes of the phytic acid-hydroxylamine sulfate solution are phytic acid and hydroxylamine sulfate, and the solvent is deionized water; the solutes of the phytic acid-ammonium molybdate solution are phytic acid and ammonium molybdate, and the solvent is deionized water.
[0024] Furthermore, the preparation process of the dopamine-modified molybdenum disulfide comprises the following steps:
[0025] Add molybdenum disulfide to an ethanol solution, perform ultrasonic peeling, centrifuge, collect the upper suspension, rotary evaporate at 40°C, and freeze-dry to obtain a few-layer molybdenum disulfide; ultrasonically disperse the few-layer molybdenum disulfide in anhydrous ethanol, add Tris buffer solution, perform ultrasonic dispersion, add dopamine hydrochloride, stir at room temperature for 24 hours, centrifuge, wash, and vacuum dry at 50°C for 6 hours to obtain polydopamine-modified molybdenum disulfide.
[0026] Furthermore, in the few-layer molybdenum disulfide, the ultrasonic stripping time is 5.5-6.5h; in the polydopamine-modified molybdenum disulfide, the mass ratio of the few-layer molybdenum disulfide: dopamine hydrochloride is 1:(0.5-0.7).
[0027] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0028] The present invention uses homemade mesoporous silica as a layer of packaging container, phytic acid as a corrosion inhibitor, hydroxylamine sulfate / ammonium molybdate as a slow-release promoter, and is encapsulated in mesoporous silica together, followed by corrosion inhibitors phytic acid zinc and hexahydrated cobalt nitrate as metal sources of the MOF framework, 2-methylimidazole as an organic ligand, and dopamine-modified molybdenum dioxide as a template, in situ growth on its surface, and a phytic acid zinc zeolite imidazolate skeleton is prepared, and the MOF framework is used as a two-layer packaging container, encapsulating mesoporous silica loaded with phytic acid and hydroxylamine sulfate / ammonium molybdate to prepare a nanocomposite material; finally, it reacts with hexahydrated nickel nitrate at room temperature to convert part of the zeolite imidazolate skeleton into a layered double hydroxide to obtain a multi-lamellar structure nanocomposite material. It is blended with a water-based epoxy resin and a curing agent to prepare a corrosion-resistant coating, and the stainless steel strip raw material is sequentially rolled, bright solution annealed, secondary rolled, degreased, coated, tension leveled, and sheared to obtain a high-strength corrosion-resistant precision stainless steel strip.
[0029] The present invention uses dopamine-modified molybdenum dioxide as a template, and in situ grows a composite nanocontainer on the surface of the composite nanocontainer with mesoporous silica nanoparticles encapsulated by phytic acid, hydroxylamine sulfate / ammonium molybdate and layered double hydroxide derived from a zeolite imidazolate skeleton as a template. On the one hand, the compatibility of the composite nanocontainer in water-based epoxy resin is utilized to improve the dispersibility and compatibility of the composite nanocontainer in the polymer resin; on the other hand, due to the high band gap of the molybdenum dioxide itself, the composite nanocontainer has a spatial shielding effect of a two-dimensional layered structure similar to that of graphene oxide, and does not cause microgalvanic corrosion. As the first corrosion-resistant barrier, the composite nanocontainer provides a physical barrier effect of corrosive media for the stainless steel strip, thereby improving the corrosion resistance of the stainless steel strip.
[0030] The present invention converts part of the zeolite imidazolate skeleton into a layered double hydroxide, and utilizes the layered double hydroxide and the zeolite imidazolate skeleton intermediate layer to further improve the excellent compatibility and dispersibility of the composite nanocontainer in the waterborne epoxy resin, while giving the composite nanocontainer the ability of pH-responsive controlled release, further improving the barrier properties of the composite coating, and enhancing the resistance to chloride ion penetration. Under the erosion of ordinary neutral salt spray and salt water, phytic acid can form a phytic acid metal conversion film on the surface of the stainless steel strip through complexation with zinc ions. During the long-term corrosion process, part of the phytic acid metal conversion film complex bonds in the film layer are broken, and the P-OH groups in part of the phytic acid molecules are relayed to PO- , complexing with the metal ions in the solution again to achieve the effect of film healing, and the mesoporous silica encapsulated in the layered double hydroxide and zeolite imidazolate skeleton has a sustained release effect, slowly releasing the encapsulated phytic acid, hydroxylamine sulfate / ammonium molybdate, and the released phytic acid can supplement the phosphate groups on the surface of the stainless steel strip. The phosphate groups in the phytic acid molecules can not only form a phytic acid conversion film with the zinc, cobalt, and nickel metal ions in the zeolite imidazolate skeleton through complexation, but also accelerate the partial dissolution of the stainless steel strip surface under the action of the hydroxylamine sulfate promoter, and can also form a dense phytic acid conversion film on the surface of the stainless steel strip through electrostatic action, synergistically enhancing the corrosion resistance of the stainless steel strip. As another promoter, ammonium molybdate can form an ammonium molybdate passivation film on the surface of the stainless steel strip, and promote the phytic acid molecules to further form a phytic acid passivation film on the surface of the film layer, greatly improving the corrosion resistance of the stainless steel strip.
[0031] In order to cope with more severe acidic corrosion environments in addition to neutral conditions, the present invention, when the pH is 4-4.5, the surface of the stainless steel strip is subjected to aggravated corrosion, and the zeolite imidazolate skeleton can respond to the pH and release the internal encapsulated corrosion inhibitor and promoter in advance to achieve the best anti-corrosion and barrier effect. At the same time, when the pH is 4-4.5, the metal dissolution rate of the hydroxylamine sulfate promoter and the film growth rate reach a relative equilibrium state, which can maximize the impedance value of the conversion film and make the film grow completely, and work together to cope with the acidic corrosion environment, greatly improving the application scenario of the stainless steel strip prepared by the present invention. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] In the following examples, zinc phytate CAS: 63903-51-5 was purchased from Hubei Nona Technology Co., Ltd.; molybdenum disulfide was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; dopamine hydrochloride was purchased from Shanghai McLean Biochemical Technology Co., Ltd.; the 301 stainless steel strip specification was 1Cr17Ni7, the nickel content was 6.05%, and the thickness was 0.8 mm; the water-based epoxy resin model was EFD-5601, purchased from Shanghai Di Ai Sheng Trading Co., Ltd.; the curing agent was a water-based epoxy curing agent, BECKOPOX™ EH 613w / 80WA, purchased from Allnex Resins (China) Co., Ltd.; and the remaining raw materials were commercially available.
[0034] The preparation process of mesoporous silica includes the following steps:
[0035] 1 g of hexadecyltrimethylammonium bromide was added to deionized water, and a 2 M sodium hydroxide solution was added to adjust the pH to 12, and the mixture was heated to 80°C, and 5 g of ethyl silicate was added. The mixture was kept warm for 2 h, and the mixture was centrifuged and washed. The crude product was added to a 0.8 mL / 100 mL methanol solution of concentrated hydrochloric acid, and the mixture was heated to 65°C and stirred overnight, and vacuum dried at 65°C for 12 h to obtain mesoporous silica.
[0036] The preparation process of dopamine-modified molybdenum disulfide comprises the following steps:
[0037] Molybdenum disulfide was added to a 45% v / v ethanol solution, ultrasonically stripped for 6 hours, centrifuged, the upper suspension was collected, rotary evaporated at 40°C, and freeze-dried to obtain a few-layer molybdenum disulfide; 100 mg of the few-layer molybdenum disulfide was ultrasonically dispersed in anhydrous ethanol, a Tris buffer solution was added, ultrasonically dispersed, 50 mg of dopamine hydrochloride was added, stirred at room temperature for 24 hours, centrifuged, washed, and vacuum dried at 50°C for 6 hours to obtain polydopamine-modified molybdenum disulfide;
[0038] Example 1: Processing technology of high-strength, corrosion-resistant precision stainless steel strip: S1: 100 mg of mesoporous silica was heated to 120°C for activation for 2 hours, and the activated mesoporous silica was placed in a phytic acid-hydroxylamine sulfate solution containing 1 g of phytic acid-hydroxylamine sulfate, vacuumed, stirred for 6-8 hours, centrifuged, and vacuum dried at 60°C for 12 hours to obtain encapsulated corrosion inhibitor mesoporous silica; wherein, in the phytic acid-hydroxylamine sulfate solution, the molar ratio of phytic acid:hydroxylamine sulfate is 2:1;
[0039] S2: Add 2-methylimidazole to deionized water, add 1g of encapsulated corrosion inhibitor mesoporous silica and dopamine-modified molybdenum disulfide, ultrasonically disperse, heat to 35°C, ultrasonically disperse 1g of zinc phytate in deionized water and add it, keep warm for 24h, centrifuge, wash, and vacuum dry at 60°C for 24h to obtain an intermediate; wherein, Zn in zinc phytate 2+ : The molar ratio of molybdenum disulfide in 2-methylimidazole: dopamine modified molybdenum disulfide is 45:1:1.5;
[0040] S3: Add 0.1 g of the intermediate to an aqueous solution consisting of 0.1 g of cobalt nitrate hexahydrate and 1 g of 2-methylimidazole, stir to react for 15 min, centrifuge, wash, and vacuum dry at 60°C for 24 h to obtain a nanocomposite material; ultrasonically disperse 100 mg of the nanocomposite material in an ethanol solution containing 80 mg of nickel nitrate hexahydrate, stir evenly, add a deionized water solution containing 230.9 mg of sodium phytate, adjust the pH to 10, heat to 60°C under a nitrogen atmosphere, react for 24 h, centrifuge, and vacuum dry at 80°C for 12 h to obtain a multi-layer structure nanocomposite material;
[0041] S4: ultrasonically dispersing the multi-layer structure nanocomposite material in deionized water, adding the dispersion into the waterborne epoxy resin, ultrasonically dispersing, adding a curing agent, and stirring evenly to obtain a corrosion-resistant coating; wherein the amount of the multi-layer structure nanocomposite material added is 0.6wt% of the mass of the waterborne epoxy resin;
[0042] S5: The stainless steel strip raw material is sequentially rolled, bright solution annealed, secondary rolled, degreased, coated, tension leveled, and sheared to obtain a high-strength, corrosion-resistant, precision stainless steel strip.
[0043] Example 2: Processing technology of high-strength, corrosion-resistant precision stainless steel strip: S1: 100 mg of mesoporous silica was heated to 120°C for activation for 2 hours, and the activated mesoporous silica was placed in a phytic acid-ammonium molybdate solution containing 1 g of phytic acid-ammonium molybdate, vacuumed, stirred for 6-8 hours, centrifuged, and vacuum dried at 60°C for 12 hours to obtain encapsulated corrosion inhibitor mesoporous silica; wherein, in the phytic acid-ammonium molybdate solution, the molar ratio of phytic acid:ammonium molybdate is 1.6:1;
[0044] The remaining steps are the same as those in Example 1.
[0045] Example 3: Processing technology of high-strength, corrosion-resistant precision stainless steel strip: S2: Add 2-methylimidazole to deionized water, add 1g of encapsulated corrosion inhibitor mesoporous silica and dopamine-modified molybdenum disulfide, ultrasonically disperse, heat to 35°C, ultrasonically disperse 1g of zinc phytate in deionized water and add it, keep warm for 24h, centrifuge, wash, and vacuum dry at 60°C for 24h to obtain an intermediate; wherein, Zn in zinc phytate 2+ : The molar ratio of molybdenum disulfide in 2-methylimidazole: dopamine modified molybdenum disulfide is 60:1:2;
[0046] The remaining steps are the same as those in Example 1.
[0047] Example 4: Processing technology of high-strength, corrosion-resistant precision stainless steel strip: S4: Ultrasonic dispersion of multi-layer structure nanocomposite material in deionized water, adding the dispersion into water-based epoxy resin, ultrasonic dispersion, adding curing agent, stirring evenly, to obtain corrosion-resistant coating; wherein, the amount of multi-layer structure nanocomposite material added is 1wt% of the mass of water-based epoxy resin;
[0048] The remaining steps are the same as those in Example 3.
[0049] Example 5: Processing technology of high-strength, corrosion-resistant precision stainless steel strip: S4: Ultrasonic dispersion of multi-layer structure nanocomposite material in deionized water, adding the dispersion into water-based epoxy resin, ultrasonic dispersion, adding curing agent, stirring evenly, to obtain corrosion-resistant coating; wherein, the amount of multi-layer structure nanocomposite material added is 1.5wt% of the mass of water-based epoxy resin;
[0050] The remaining steps are the same as those in Example 3.
[0051] Comparative Example 1: Processing technology of high-strength corrosion-resistant precision stainless steel strip: S2: Add 2-methylimidazole to deionized water, add 1g of mesoporous silica encapsulating corrosion inhibitor, ultrasonically disperse, heat to 35°C, ultrasonically disperse 1g of zinc phytate in deionized water and add it, keep warm for 24h, centrifuge, wash, and vacuum dry at 60°C for 24h to obtain an intermediate; wherein, Zn in zinc phytate 2+ : The molar ratio of 2-methylimidazole is 45:1;
[0052] The remaining steps are the same as those in Example 1.
[0053] Comparative Example 2: Processing technology of high-strength, corrosion-resistant precision stainless steel strip: S1: 100 mg of mesoporous silica was heated to 120°C for activation for 2 hours, and the activated mesoporous silica was placed in a phytic acid-hydroxylamine sulfate solution containing 1 g of phytic acid-hydroxylamine sulfate, vacuumed, stirred for 6-8 hours, centrifuged, and vacuum dried at 60°C for 12 hours to obtain encapsulated corrosion inhibitor mesoporous silica; wherein, in the phytic acid-hydroxylamine sulfate solution, the molar ratio of phytic acid:hydroxylamine sulfate is 2:1;
[0054] S2: Add 2-methylimidazole to deionized water, add 1g of encapsulated corrosion inhibitor mesoporous silica and dopamine-modified molybdenum disulfide, ultrasonically disperse, heat to 35°C, ultrasonically disperse 1g of zinc phytate in deionized water and add it, keep warm for 24h, centrifuge, wash, and vacuum dry at 60°C for 24h to obtain an intermediate; wherein, Zn in zinc phytate 2+ : The molar ratio of molybdenum disulfide in 2-methylimidazole: dopamine modified molybdenum disulfide is 45:1:1.5;
[0055] S3: adding 0.1 g of the intermediate to an aqueous solution consisting of 0.1 g of cobalt nitrate hexahydrate and 1 g of 2-methylimidazole, stirring for 15 min, centrifuging, washing, and vacuum drying at 60° C. for 24 h to obtain a multi-layer structure nanocomposite material;
[0056] S4: ultrasonically dispersing the multi-layer structure nanocomposite material in deionized water, adding the dispersion into the waterborne epoxy resin, ultrasonically dispersing, adding a curing agent, and stirring evenly to obtain a corrosion-resistant coating; wherein the amount of the multi-layer structure nanocomposite material added is 0.6wt% of the mass of the waterborne epoxy resin;
[0057] S5: The stainless steel strip raw material is sequentially rolled, bright solution annealed, secondary rolled, degreased, coated, tension leveled, and sheared to obtain a high-strength, corrosion-resistant, precision stainless steel strip.
[0058] Experiment: Corrosion resistance test: Electrochemical impedance spectroscopy was measured using a CS310 electrochemical workstation. The electrochemical impedance spectroscopy test was conducted at open circuit potential (OCP), where the electrolyte was a neutral 3.5wt.% NaCl solution and a 3.5wt.% NaCl solution with a pH of 4.0. The test frequency range was 10 5 Hz~10 -2 Hz, and the applied voltage amplitude was 20 mV. The EIS data were analyzed by ZSimpWin3.60 software.
[0059] In the above experiments, the coating thickness was 80 μm. The coating was cured at room temperature for 5 days after coating, and the high temperature curing condition was 100°C for 6 hours.
[0060] Table 1 Corrosion resistance test data
[0061]
[0062] Conclusion: The stainless steel strip prepared by the present invention has excellent mechanical strength and corrosion resistance. Comparative Example 1 does not use dopamine to modify molybdenum disulfide in-situ growth composite nanocontainer, resulting in reduced corrosion resistance. Comparative Example 2 lacks a layered double hydroxide structure, resulting in reduced corrosion resistance.
[0063] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. The processing technology of high-strength corrosion-resistant precision stainless steel strip is characterized by: The following steps are involved: S1: Add 2-methylimidazole to deionized water, add encapsulated corrosion inhibitor mesoporous silica and dopamine-modified molybdenum disulfide, ultrasonically disperse, heat to 35-37°C, ultrasonically disperse zinc phytate in deionized water and add it thereto, keep warm for reaction, centrifuge, wash, and vacuum dry to obtain an intermediate; add the intermediate to an aqueous solution composed of cobalt nitrate hexahydrate and 2-methylimidazole, stir for reaction, centrifuge, wash, and vacuum dry to obtain a nanocomposite material; ultrasonically disperse the nanocomposite material in an ethanol solution of nickel nitrate hexahydrate, stir evenly, add sodium phytate solution, adjust the pH to 10-10.5, heat for reaction under a nitrogen atmosphere, centrifuge, and vacuum dry to obtain a multi-layer structure nanocomposite material; ultrasonically disperse the multi-layer structure nanocomposite material in deionized water, add the dispersion to a water-based epoxy resin, ultrasonically disperse, add a curing agent, stir evenly, and obtain a corrosion-resistant coating; S2: The stainless steel strip raw material is sequentially rolled, bright solution annealed, secondary rolled, degreased, coated, tension leveled, and sheared to obtain a high-strength, corrosion-resistant, precision stainless steel strip; In the corrosion-resistant coating, the amount of the multi-layer structure nanocomposite material added is 0.6-1.5wt% of the mass of the waterborne epoxy resin; The preparation process of the mesoporous silica encapsulating the corrosion inhibitor comprises the following steps: Step (1): adding hexadecyltrimethylammonium bromide to deionized water, adjusting the pH to 12-12.5, heating to 80-85° C., adding ethyl silicate, keeping the temperature for 2-3 hours, centrifuging, washing, purifying, and vacuum drying to obtain mesoporous silica; Step (2): activating the mesoporous silica, placing the activated mesoporous silica in a corrosion inhibitor solution, evacuating the solution, stirring for 6-8 hours, centrifuging, and vacuum drying at 60° C. for 12 hours to obtain the corrosion inhibitor encapsulated mesoporous silica; The preparation process of dopamine-modified molybdenum disulfide comprises the following steps: Add molybdenum disulfide to an ethanol solution, perform ultrasonic peeling, centrifuge, collect the upper suspension, rotary evaporate at 40°C, and freeze-dry to obtain a few-layer molybdenum disulfide; ultrasonically disperse the few-layer molybdenum disulfide in anhydrous ethanol, add Tris buffer solution, perform ultrasonic dispersion, add dopamine hydrochloride, stir at room temperature for 24 hours, centrifuge, wash, and vacuum dry at 50°C for 6 hours to obtain polydopamine-modified molybdenum disulfide.
2. The processing technology of high-strength, corrosion-resistant, precision stainless steel strip according to claim 1 is characterized in that: In the intermediate, Zn in phytate 2+ The molar ratio of molybdenum disulfide in 2-methylimidazole: dopamine modified molybdenum disulfide is (45-60): 1: (1.5-2); the mass ratio of zinc phytate: encapsulated corrosion inhibitor mesoporous silica is 1:
1.
3. The processing technology of high-strength, corrosion-resistant, precision stainless steel strip according to claim 1 is characterized in that: In the nanocomposite material, the mass ratio of the intermediate: cobalt nitrate hexahydrate: 2-methylimidazole is (0.1-0.2):0.1:
1.
4. The processing technology of high-strength, corrosion-resistant, precision stainless steel strip according to claim 1 is characterized in that: In the multi-layer structure nanocomposite material, the mass ratio of the nanocomposite material: nickel nitrate hexahydrate: sodium phytate is 100:80:(230.9-277.1).
5. The processing technology of high-strength, corrosion-resistant, precision stainless steel strip according to claim 1 is characterized in that: In the mesoporous silica, the mass ratio of hexadecyltrimethylammonium bromide:ethyl silicate is (1-2):(5-10); in the encapsulated corrosion inhibitor mesoporous silica, the sustained-release agent solvent includes any one of a phytic acid-hydroxylamine sulfate solution and a phytic acid-ammonium molybdate solution; in the phytic acid-hydroxylamine sulfate solution, the molar ratio of phytic acid:hydroxylamine sulfate is (2-3):(1-1.5); in the phytic acid-ammonium molybdate solution, the molar ratio of phytic acid:ammonium molybdate is (1.6-2):(1-1.4); the mass ratio of corrosion inhibitor in the mesoporous silica:corrosion inhibitor solution is 1:
10.
6. The processing technology of high-strength, corrosion-resistant, precision stainless steel strip according to claim 1 is characterized in that: In the few-layer molybdenum disulfide, the ultrasonic stripping time is 5.5-6.5h; in the polydopamine-modified molybdenum disulfide, the mass ratio of the few-layer molybdenum disulfide to dopamine hydrochloride is 1:(0.5-0.7).
7. A high-strength, corrosion-resistant, precision stainless steel strip prepared according to the processing technology of the high-strength, corrosion-resistant, precision stainless steel strip according to any one of claims 1 to 6.
Citation Information
Cited By
Automatic cleaning equipment for high-temperature-resistant and corrosion-resistant stainless steel band
CN223185219U