Solid gum containing ferrous sulfate and preparation method thereof

By using solid glue with inorganic substances such as ferrous sulfate and specific auxiliary preparations, the problem of health effects caused by the volatilization of organic matter in existing solid glues has been solved, and an environmentally friendly and high-performance solid glue product has been achieved, with low cost, high transparency and strong strength. Adhesion.

CN118725822APending Publication Date: 2024-10-01GUIZHOU ZHICHENG NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410931240.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing solid glue has a high organic content when it volatilizes, which affects human health and fails to achieve environmental protection effects.

Method used

Using inorganic substances such as ferrous sulfate, wax powder, pentonite, manganese sulfate and sodium sulfate as raw materials, combined with specific auxiliary preparations and process steps, a solid glue containing ferrous sulfate is prepared, which reduces the organic content and improves the product's resistance. Thermal high temperature resistance.

Benefits of technology

This solid glue not only maintains the excellent performance of the original solid glue, reduces the volatilization of organic matter, improves the safety and environmental performance of the product, but also has low production cost, high transparency and strong adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725822A_ABST
    Figure CN118725822A_ABST
Patent Text Reader

Abstract

The invention discloses solid gum containing ferrous sulfate, and relates to the technical field of solid gum. The environment-friendly rust remover is prepared from the following raw materials in parts by weight: 25 parts of ferrous sulfate, 13 parts of wax powder, 13 parts of bentonite, 15 parts of manganese sulfate, 15 parts of sodium sulfate, 13 parts of 2, 4, 6-trichlorobenzene, 15 parts of stearic acid, 23 parts of an auxiliary preparation and the balance of deionized water. The preparation method of the solid gum comprises the following steps: sequentially adding the deionized water, the ferrous sulfate, the wax powder, the bentonite, the manganese sulfate and the sodium sulfate into a reaction kettle, uniformly stirring and mixing, adding the 2, 4, 6-trichlorobenzene and the transparent agent, uniformly stirring, adding the stearic acid and the pH regulator, uniformly stirring, adding the gelling agent, the excipient and the preservative, injecting into a mold, and cooling to obtain the product. According to the solid gum containing ferrous sulfate, inorganic matters such as ferrous sulfate, wax powder, bentonite, manganese sulfate and sodium sulfate are adopted as raw materials, so that the content of organic matters is reduced, and the solid gum is harmless to a human body and also has all excellent properties of the solid gum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid glue, in particular to a solid glue containing ferrous sulfate and a preparation method thereof. Background Art

[0002] Solid glue is also called solid glue stick, solid paste, lipstick paste, etc. It is made of glue, essence and water as raw materials and is reasonably prepared. Solid glue is a new product in adhesives. Its main features are: easy to obtain raw materials, simple to make, long shelf life, easy to carry, easy to use, strong bonding, and suitable for paper bonding.

[0003] The invention with the publication number of CN 104277731 B discloses a high temperature resistant solid glue and a preparation method thereof, wherein the high temperature resistant solid glue comprises the following raw materials in parts by weight: 10 to 30 parts of 2-(diethylamino)ethyl diphenylacetate sodium hydrochloride, 20 to 30 parts of 2,4,6-trichlorobenzoic acid, 10 to 40 parts of dimethylaminoethyl p-chlorophenoxyacetate, 10 to 50 parts of N,N-di(2-chloroethyl)methylamine, 20 to 40 parts of sorbitan sesquioleate, 2 to 7 parts of propylene glycol fatty acid ester, 20 to 30 parts of polyglycerol-2-dipolyhydroxystearate, 10 to 40 parts of gelling agent, 20 to 40 parts of excipient, and 15 to 35 parts of moisturizer. The preparation method is: mix the raw materials evenly, stir for 1 to 2 hours, heat to 78-80°C, add gelling agent, excipient, moisturizer, keep warm for 1 to 2 hours, continue to mix evenly, inject into mold, and cool.

[0004] As shown in the above invention, the existing solid glue has a certain high temperature resistance effect, but the solid glue has a high organic content, which will affect human health when volatilizing and cannot achieve the effect of environmental protection. Summary of the invention

[0005] In view of the deficiencies of the prior art, the present invention provides a solid glue containing ferrous sulfate and a preparation method thereof, which solves the existing problems.

[0006] To achieve the above object, the present invention is implemented by the following technical scheme: the solid glue containing ferrous sulfate, the raw materials of which include in parts ratio:

[0007] 20-25 parts of ferrous sulfate, 12-13 parts of wax powder, 12-13 parts of pyrotein, 13-15 parts of manganese sulfate, 13-15 parts of sodium sulfate, 11-13 parts of 2,4,6-trichlorobenzoic acid, 13-15 parts of stearic acid, 18-23 parts of auxiliary agents, and the balance is deionized water.

[0008] Preferably, the auxiliary preparation comprises 0.5-1 parts of excipient, 15-17 parts of transparent agent, 1-2 parts of pH adjuster, 0.5-1 parts of preservative and 1-2 parts of gelling agent.

[0009] Preferably, the excipient is a mixture of one or more of polyvinyl alcohol, polyvinyl formal, polyvinyl pyrrolidone, carboxymethyl cellulose and sodium polyacrylate.

[0010] Preferably, the clarifier is a mixture of one or more of sorbitol and sucrose.

[0011] Preferably, the pH regulator is sodium hydroxide, potassium hydroxide or a mixture of the two.

[0012] Preferably, the gelling agent is one or more of fatty acid salts, betaine or 1,3-glucan, and the fatty acid salt is sodium stearate or sodium palmitate.

[0013] Preferably, the preservative is a mixture of BIT and PHMB, the weight percentage of BIT to the raw material is 0.1-1.0%, and the weight percentage of PHMB to the raw material is 0.1-1.0%.

[0014] The present invention also discloses a method for preparing a solid glue containing ferrous sulfate, comprising the following steps:

[0015] Step 1: Add deionized water, ferrous sulfate, wax powder, pyrolusite, manganese sulfate and sodium sulfate into the reaction kettle in sequence, and stir to mix evenly;

[0016] Step 2: Add 2,4,6-trichlorobenzene and a transparent agent while stirring, raise the temperature, and stir and mix at a constant temperature until the solution becomes transparent;

[0017] Step 3: Add stearic acid while stirring, and add pH adjuster after stirring and mixing evenly, adjust the pH value of the system to 10 to 12, and stir to dissolve completely;

[0018] Step 4: Add the gelling agent and excipients, add the preservatives while stirring, stir evenly again and let stand at a constant temperature for 160 to 180 minutes;

[0019] Step 5: Inject the glue liquid into the mold, stir until the bubbles are completely eliminated, then slowly cool down to room temperature. After the glue liquid is completely solidified, a highly transparent solid glue stick product is obtained.

[0020] Preferably, the stirring time in steps 1 to 3 is 8-10 min, the rotation speed is 300-500 r / min, and the constant temperature stirring is carried out at 90-100°C.

[0021] Preferably, in step 2, the temperature is raised to 85-90°C and kept constant for 10-20 minutes, and in step 4, the stirring speed is 400-500r / min, and the stirring is carried out at a constant temperature of 90-100°C.

[0022] Beneficial Effects

[0023] The present invention provides a solid glue containing ferrous sulfate and a preparation method thereof. Compared with the prior art, the solid glue has the following beneficial effects:

[0024] 1. The solid glue containing ferrous sulfate adopts inorganic substances such as ferrous sulfate, wax powder, bromine clay, manganese sulfate and sodium sulfate as raw materials, which reduces the content of organic matter and is harmless to the human body. It also has all the excellent properties of solid collagen, improves the competitiveness of the product, and assumes the social responsibility of environmental protection.

[0025] 2. The solid glue containing ferrous sulfate uses fatty acid salt as an excipient, the raw materials are easy to obtain, the production cost is low, it has high transparency, strong adhesion, smooth coating, long shelf life, safe raw materials, non-toxic and harmless, and also has very good heat and high temperature resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the method flow of the present invention. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The present invention provides multiple technical solutions:

[0029] The first implementation method:

[0030] A solid glue containing ferrous sulfate, the raw materials of which include, by parts ratio:

[0031] 20 parts of ferrous sulfate, 12 parts of wax powder, 12 parts of bromopentane, 13 parts of manganese sulfate, 13 parts of sodium sulfate, 11 parts of 2,4,6-trichlorobenzoic acid, 13 parts of stearic acid, 18 parts of auxiliary preparations, and the balance is deionized water.

[0032] The auxiliary preparation comprises 0.5 parts of excipient, 15 parts of clarifier, 1 part of pH regulator, 0.5 parts of preservative and 1 part of gelling agent. The excipient is a mixture of one or more of polyvinyl alcohol, polyvinyl formal, polyvinyl pyrrolidone, carboxymethyl cellulose and sodium polyacrylate. The clarifier is a mixture of one or more of sorbitol and sucrose. The clarifier is a mixture of one or more of sorbitol and sucrose. The pH regulator is one or a mixture of two of sodium hydroxide and potassium hydroxide. The gelling agent is one or more of fatty acid salts, betaine or 1,3-glucan. The fatty acid salt is sodium stearate or sodium palmitate. The preservative is a mixture of BIT and PHMB. The weight percentage of BIT in the raw material is 0.1%, and the weight percentage of PHMB in the raw material is 0.1%.

[0033] A method for preparing a solid glue containing ferrous sulfate comprises the following steps:

[0034] Step 1: Add deionized water, ferrous sulfate, wax powder, pyrolusite, manganese sulfate and sodium sulfate into the reaction kettle in sequence, stir and mix evenly, the stirring time is 8 minutes, and the speed is 300r / min;

[0035] Step 2: Add 2,4,6-trichlorobenzene and a transparent agent while stirring, raise the temperature to 85°C, and stir and mix at this temperature for 10 minutes until the solution becomes transparent;

[0036] Step 3: Add stearic acid while stirring, and add pH adjuster after stirring and mixing evenly, adjust the pH value of the system to 10, and stir to dissolve completely. The stirring time is 8 minutes and the speed is 300r / min;

[0037] Step 4: Add the gelling agent and excipients, add the preservatives while stirring, stir evenly again, and let stand at a constant temperature for 160 minutes at a stirring speed of 400 r / min. The stirring is carried out at a constant temperature of 90° C.

[0038] Step 5: Inject the glue liquid into the mold, stir until the bubbles are completely eliminated, then slowly cool down to room temperature. After the glue liquid is completely solidified, a highly transparent solid glue stick product is obtained.

[0039] The second implementation method:

[0040] A solid glue containing ferrous sulfate, the raw materials of which include, by parts ratio:

[0041] 23 parts of ferrous sulfate, 12 parts of wax powder, 13 parts of bromopentane, 14 parts of manganese sulfate, 14 parts of sodium sulfate, 12 parts of 2,4,6-trichlorobenzoic acid, 14 parts of stearic acid, 20 parts of auxiliary preparations, and the balance is deionized water.

[0042] The auxiliary preparation comprises 0.5 parts of excipient, 16 parts of transparent agent, 2 parts of pH adjusting agent, 0.5 parts of preservative and 1 part of gelling agent. The excipient is a mixture of one or more of polyvinyl alcohol, polyvinyl formal, polyvinyl pyrrolidone, carboxymethyl cellulose and sodium polyacrylate. The transparent agent is a mixture of one or more of sorbitol and sucrose. The transparent agent is a mixture of one or more of sorbitol and sucrose. The pH adjusting agent is one or a mixture of two of sodium hydroxide and potassium hydroxide. The gelling agent is one or more of fatty acid salts, betaine or 1,3-glucan. The fatty acid salt is sodium stearate or sodium palmitate. The preservative is a mixture of BIT and PHMB. The weight percentage of BIT in the raw material is 0.5%, and the weight percentage of PHMB in the raw material is 0.5%.

[0043] A method for preparing a solid glue containing ferrous sulfate comprises the following steps:

[0044] Step 1: Add deionized water, ferrous sulfate, wax powder, pyrolusite, manganese sulfate and sodium sulfate into the reaction kettle in sequence, stir and mix evenly, the stirring time is 9 minutes, and the speed is 400r / min;

[0045] Step 2: Add 2,4,6-trichlorobenzene and a transparent agent while stirring, raise the temperature to 88°C, and stir and mix at this temperature for 15 minutes until the solution becomes transparent;

[0046] Step 3: Add stearic acid while stirring, and add pH adjuster after stirring and mixing evenly, adjust the pH value of the system to 11, and stir to dissolve completely. The stirring time is 9 minutes and the speed is 400r / min;

[0047] Step 4: Add the gelling agent and excipients, add the preservatives while stirring, stir evenly again, and let stand at a constant temperature for 170 minutes at a stirring speed of 450 r / min. The stirring is carried out at a constant temperature of 95° C.

[0048] Step 5: Inject the glue liquid into the mold, stir until the bubbles are completely eliminated, then slowly cool down to room temperature. After the glue liquid is completely solidified, a highly transparent solid glue stick product is obtained.

[0049] The third implementation method:

[0050] A solid glue containing ferrous sulfate, the raw materials of which include, by parts ratio:

[0051] 25 parts of ferrous sulfate, 13 parts of wax powder, 13 parts of roentgenite, 15 parts of manganese sulfate, 15 parts of sodium sulfate, 13 parts of 2,4,6-trichlorobenzoate, 15 parts of stearic acid, 23 parts of auxiliary agents, and the balance is deionized water.

[0052] The auxiliary preparation comprises 1 part of excipient, 17 parts of transparent agent, 2 parts of pH adjusting agent, 1 part of preservative and 2 parts of gelling agent. The excipient is a mixture of one or more of polyvinyl alcohol, polyvinyl formal, polyvinyl pyrrolidone, carboxymethyl cellulose and sodium polyacrylate. The transparent agent is a mixture of one or more of sorbitol and sucrose. The transparent agent is a mixture of one or more of sorbitol and sucrose. The pH adjusting agent is one or a mixture of two of sodium hydroxide and potassium hydroxide. The gelling agent is one or more of fatty acid salts, betaine or 1,3-glucan. The fatty acid salt is sodium stearate or sodium palmitate. The preservative is a mixture of BIT and PHMB. The weight percentage of BIT in the raw material is 1.0%, and the weight percentage of PHMB in the raw material is 1.0%.

[0053] A method for preparing a solid glue containing ferrous sulfate comprises the following steps:

[0054] Step 1: Add deionized water, ferrous sulfate, wax powder, pyrolusite, manganese sulfate and sodium sulfate into the reaction kettle in sequence, stir and mix evenly, the stirring time is 10 minutes, and the speed is 500r / min;

[0055] Step 2: Add 2,4,6-trichlorobenzene and a transparent agent while stirring, raise the temperature to 90°C, and stir and mix at this temperature for 20 minutes until the solution becomes transparent;

[0056] Step 3: Add stearic acid while stirring, and add pH adjuster after stirring and mixing evenly, adjust the pH value of the system to 12, and stir to dissolve completely. The stirring time is 10 minutes and the speed is 500r / min;

[0057] Step 4: Add the gelling agent and excipients, add the preservative while stirring, stir evenly again, and let stand at a constant temperature for 180 minutes at a stirring speed of 500 r / min. The stirring is carried out at a constant temperature of 100° C.

[0058] Step 5: Inject the glue liquid into the mold, stir until the bubbles are completely eliminated, then slowly cool down to room temperature. After the glue liquid is completely solidified, a highly transparent solid glue stick product is obtained.

[0059] Product performance comparison summary table

[0060]

[0061]

[0062] In summary, the above three embodiments can all produce solid glue with better effects, select non-organic solvents, and use specific additives and new substances to improve and reduce the volatility of organic volatiles remaining in the raw materials of the product, lock the relevant organic matter, and make it non-volatile, which greatly reduces the volatilization of organic volatiles into the environment, protects the environment, and has the characteristics of crystal clearness, beautiful appearance, and reduced organic volatiles.

[0063] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art, and the model parameters of each electrical appliance are not specifically limited, and conventional equipment can be used.

[0064] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0065] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A solid glue containing ferrous sulfate, characterized in that: The raw materials include: 20-25 parts of ferrous sulfate, 12-13 parts of wax powder, 12-13 parts of pyrotein, 13-15 parts of manganese sulfate, 13-15 parts of sodium sulfate, 11-13 parts of 2,4,6-trichlorobenzoic acid, 13-15 parts of stearic acid, 18-23 parts of auxiliary agents, and the balance is deionized water.

2. The solid glue containing ferrous sulfate according to claim 1, characterized in that: The auxiliary preparation comprises, by proportion: 0.5-1 parts of excipients, 15-17 parts of transparent agents, 1-2 parts of pH adjusters, 0.5-1 parts of preservatives, and 1-2 parts of gelling agents.

3. The solid glue containing ferrous sulfate according to claim 2, characterized in that: The excipient is a mixture of one or more of polyvinyl alcohol, polyvinyl formal, polyvinyl pyrrolidone, carboxymethyl cellulose and sodium polyacrylate.

4. The solid glue containing ferrous sulfate according to claim 2, characterized in that: The clarifier is a mixture of one or more of sorbitol and sucrose.

5. The solid glue containing ferrous sulfate according to claim 2, characterized in that: The pH regulator is sodium hydroxide, potassium hydroxide or a mixture of the two.

6. The solid glue containing ferrous sulfate according to claim 2, characterized in that: The gelling agent is one or more of fatty acid salts, betaine or 1,3-glucan.

7. The solid glue containing ferrous sulfate according to claim 2, characterized in that: The preservative is a mixture of BIT and PHMB.

8. A method for preparing a solid glue containing ferrous sulfate, characterized in that: The following steps are involved: Step 1: Add deionized water, ferrous sulfate, wax powder, pyrolusite, manganese sulfate and sodium sulfate into the reaction kettle in sequence, and stir to mix evenly; Step 2: Add 2,4,6-trichlorobenzene and a transparent agent while stirring, raise the temperature, and stir and mix at a constant temperature until the solution becomes transparent; Step 3: Add stearic acid while stirring, and add pH adjuster after stirring and mixing evenly, adjust the pH value of the system to 10 to 12, and stir to dissolve completely; Step 4: Add the gelling agent and excipients, add the preservatives while stirring, stir evenly again and let stand at a constant temperature for 160 to 180 minutes; Step 5: Inject the glue liquid into the mold, stir until the bubbles are completely eliminated, then slowly cool down to room temperature. After the glue liquid is completely solidified, a highly transparent solid glue stick product is obtained.

9. The method for preparing a solid glue containing ferrous sulfate according to claim 8, characterized in that: The stirring time in step 1 to step 3 is 8-10 min, the rotation speed is 300-500 r / min, and the constant temperature stirring is carried out at 90-100° C.

10. The method for preparing a solid glue containing ferrous sulfate according to claim 8, characterized in that: In step 2, the temperature is raised to 85-90°C and kept constant for 10-20 minutes. In step 4, the stirring speed is 400-500r / min, and the stirring is carried out at a constant temperature of 90-100°C.