Epoxy resin composition for RTM, cured resin, fiber-reinforced composite material, and method for producing same
By using components such as tetrafunctional glycidylamine type epoxy resin, alkylphenylenediamine and methylenedianiline in the epoxy resin composition for RTM, combined with core-shell rubber particles, the problem of moisture and heat in fiber-reinforced composite materials can be solved Performance and viscosity and volatility issues in injection molding methods, enabling efficient fiber-reinforced composite manufacturing.
Patent Information
- Application Number
- CN202380022413.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-07-25
- Filing Date
- 2023-03-16
- Publication Date
- 2024-10-01
AI Technical Summary
When using existing epoxy resin compositions to manufacture fiber-reinforced composite materials, it is difficult to balance the elastic modulus, heat resistance and fracture toughness under humid heat, and the problems of resin viscosity and volatility in the injection molding method have not been effectively solved.
An epoxy resin composition for RTM using a tetrafunctional glycidylamine type epoxy resin, an aromatic amine curing agent containing alkylphenylenediamine and methylenedianiline, an aniline type epoxy resin, and core-shell rubber particles. , through specific ingredient ratios and process conditions, to ensure the excellent performance of the resin cured product in hot and humid environments.
It achieves a balance of elastic modulus, heat resistance and fracture toughness in hot and humid environments, reduces the viscosity and volatility of the resin, and is suitable for manufacturing large-scale fiber-reinforced composite materials with high fiber content through injection molding.
Smart Images

Figure CN118742585A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an epoxy resin composition for RTM preferably used in aviation / aerospace parts and general industrial applications, a cured resin, and a fiber-reinforced composite material using the cured resin, and a method for producing the same. Background Art
[0002] Epoxy resin compositions have the characteristics of high heat resistance, adhesion, and excellent mechanical strength, and are generally used as matrix resins of fiber-reinforced composite materials. Fiber-reinforced composite materials are manufactured by integrating reinforcing fibers with matrix resins. As their manufacturing methods, there are methods of laminating prepregs pre-impregnated with reinforcing fibers and matrix resins, and methods of curing by injecting low-viscosity matrix resins into shaped reinforcing fiber substrates. In general, the method of using prepregs is widely used in the fields of industry and aircraft because of their high mechanical properties, but has the disadvantage that the manufacturing processes such as the preparation and shaping of prepregs take time.
[0003] In recent years, the demand for high productivity in the use of structural materials in aircraft, automobiles, etc. has also increased, requiring the high-speed production of large composite components, and the technology to obtain fiber-reinforced composite materials with high mechanical properties and heat resistance. Therefore, the demand for fiber-reinforced composite materials that can be applied to injection molding methods such as resin transfer molding (RTM) and show excellent properties has increased.
[0004] In the injection molding method, two-component epoxy resin compositions are often used from the viewpoint of molding processability. The so-called two-component epoxy resin composition is an epoxy resin composition obtained by mixing the epoxy main agent liquid containing epoxy resin as a main component and the curing agent liquid containing curing agent as a main component immediately before use. In contrast, an epoxy resin composition in which all components including the main agent and the curing agent are mixed into one is called a one-component epoxy resin composition.
[0005] In the injection molding method, in order to obtain a large fiber reinforced composite material, the matrix resin needs to be low viscosity in the injection process. In addition, in order to use the fiber reinforced composite material for primary structural materials such as aircraft applications, it is expected to have a good balance of elastic modulus and heat resistance and fracture toughness when wet and hot. In order to have both elastic modulus and heat resistance when wet and hot, and to make the matrix resin low viscosity at the same time, there is a method of mixing a large amount of multifunctional and low molecular weight epoxy resins, but because the cross-linking density of the resin cured product is excessively improved, there is a problem that the fracture toughness is reduced and the impact resistance of the fiber reinforced composite material is reduced. In addition, by volatilizing the low molecular weight resin component in the molding process, the fiber volume content (Vf) of the molded product is reduced and the mechanical properties are not easy to show. Therefore, it is expected to construct a resin design technology that does not damage the elastic modulus, heat resistance, and fracture toughness when wet and hot, and is used to obtain a large and high Vf fiber reinforced composite material using injection molding.
[0006] Patent Document 1 describes a technique for obtaining an epoxy resin cured product having high fracture toughness by using a thermoplastic resin and core-shell rubber particles in combination at a specific ratio.
[0007] Patent Document 2 discloses a technique for achieving both a high fracture toughness of a cured resin and good impregnation of a reinforcing fiber base material with the epoxy resin composition in the resin injection step by containing a low-viscosity epoxy resin and core-shell rubber particles.
[0008] Patent Document 3 discloses a technique that uses 4,4-methylenebis(isopropyl-6-methylaniline) and core-shell rubber particles together as a curing agent for epoxy resin to increase the fracture toughness of the cured resin compared to the case where no 4,4-methylenebis(isopropyl-6-methylaniline) is used together.
[0009] Patent Document 4 discloses an epoxy resin composition blended with low-volatile N,N-diglycidyl-4-phenoxyaniline, which can provide a prepreg capable of obtaining a molded product with few voids, and also generally describes that the composition can be used in a resin transfer molding method.
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent No. 5808057
[0013] Patent Document 2: International Publication No. 2021 / 241734
[0014] Patent Document 3: Japanese Patent Application Publication No. 2010-150310
[0015] Patent Document 4: International Publication No. 2010 / 109929 Summary of the invention
[0016] Problems to be solved by the invention
[0017] The epoxy resin composition described in Patent Document 1 has excellent fracture toughness of a cured resin obtained by curing the epoxy resin composition, but has problems such as slow curing reaction and long production cycle of fiber-reinforced composite materials due to the use of M-CDEA as a curing agent. In addition, the elastic modulus under wet heat is insufficient.
[0018] The epoxy resin composition described in Patent Document 2 has a low viscosity in the resin injection step and can provide a cured resin having high heat resistance, but its elastic modulus under wet heat is significantly insufficient.
[0019] The epoxy resin composition described in Patent Document 3 has a low viscosity in the resin injection step and is excellent in impregnation into a reinforcing fiber substrate. However, the elastic modulus of the cured resin obtained by curing the epoxy resin composition is significantly low, and although the fracture toughness is also improved, it does not reach the required level.
[0020] Regarding the epoxy resin composition described in Patent Document 4, the water absorption of the cured resin obtained by curing the epoxy resin composition is high, the elastic modulus and glass transition temperature under wet heat are significantly reduced, and in addition, the viscosity is high in the resin injection step and the impregnation property into the reinforcing fiber base material is poor, making it difficult to apply to the RTM method.
[0021] An object of the present invention is to provide an epoxy resin composition for RTM, a cured resin product, and a fiber-reinforced composite material using the cured resin product, which improve the disadvantages of the prior art.
[0022] Means for solving problems
[0023] The present inventors have conducted intensive studies to solve the above-mentioned problems, and as a result, have found an epoxy resin composition for RTM having the following constitution, thereby completing the present invention. That is, the epoxy resin composition for RTM of the present invention has the following constitution.
[0024] [1] An epoxy resin composition for RTM, comprising the following components [A], [B], and [C], and satisfying all of the following conditions 1 to 4.
[0025] [A] 4-functional glycidylamine type epoxy resin
[0026] [B] At least one aromatic amine curing agent selected from alkylphenylenediamine and methylenedianiline
[0027] [C] Aniline type epoxy resin represented by formula (I)
[0028]
[0029] (In formula (I), R 1 and R 2 Each represents at least one selected from aliphatic hydrocarbon groups having 1 to 4 carbon atoms. 1 and R 2 In the case of a plurality of each, each may be the same or different. n is an integer of 0 to 4, and m is an integer of 0 to 5. X represents -O- or -S-. )
[0030] Condition 1: Viscosity at 110°C is 1 mPa·s or more and 200 mPa·s or less
[0031] Condition 2: Mass reduction after heating at 110°C for 30 minutes is 0.3 mass % or less
[0032] Condition 3: The rubber elastic modulus of the cured resin obtained by curing at 180°C for 2 hours is 2 MPa or more and 8 MPa or less
[0033] Condition 4: The water absorption of the cured resin obtained by curing at 180°C for 2 hours is 1% or more and 3% or less
[0034] [2] The epoxy resin composition for RTM according to [1], comprising 10 parts by mass or more and 50 parts by mass or less of the component [C] based on 100 parts by mass of the total epoxy resin.
[0035] [3] The epoxy resin composition for RTM according to [1] or [2], comprising, as component [D], 1 part by mass or more and 10 parts by mass or less of core-shell type rubber particles based on 100 parts by mass of the total epoxy resin.
[0036] [4] The epoxy resin composition for RTM according to any one of [1] to [3], comprising, as component [E], 10 parts by mass or more and 50 parts by mass or less of at least one solid epoxy resin selected from the group consisting of dicyclopentadiene epoxy resin, biphenyl epoxy resin, phenol aralkyl epoxy resin, and naphthalene epoxy resin, based on 100 parts by mass of all epoxy resins.
[0037] [5] The epoxy resin composition for RTM according to any one of [1] to [4], comprising both alkylphenylenediamine and methylenedianiline as component [B].
[0038] [6] The epoxy resin composition for RTM according to any one of [1] to [4], wherein the component [B] is an alkylphenylenediamine.
[0039] [7] The epoxy resin composition for RTM according to any one of [1] to [6], comprising dimethylthiotoluenediamine as the alkylphenylenediamine.
[0040] [8] The epoxy resin composition for RTM according to any one of [1] to [5] and [7], comprising 4,4-methylenebis(isopropyl-6-methylaniline) as the methylenebisaniline.
[0041] [9] The epoxy resin composition for RTM according to any one of [1] to [8], wherein the value (Mh / Me) obtained by dividing the total number of moles of active hydrogen contained in component [B] (Mh) by the total number of moles of active groups contained in all epoxy resins (Me) is 0.8 or more and 1.1 or less.
[0042]
[10] A cured resin obtained by thermally curing the epoxy resin composition for RTM according to any one of [1] to [9].
[0043]
[11] A fiber-reinforced composite material comprising the cured resin material described in
[10] and a reinforcing fiber substrate.
[0044]
[12] The fiber-reinforced composite material according to
[11] , wherein the reinforcing fiber substrate is a carbon fiber substrate.
[0045]
[13] A method for producing a fiber-reinforced composite material, comprising injecting the epoxy resin composition for RTM described in any one of [1] to [9] into a reinforcing fiber substrate arranged in a molding die heated to 70°C to 190°C to impregnate the substrate, and curing the epoxy resin composition in the molding die.
[0046]
[14] The method for producing a fiber-reinforced composite material according to
[13] , wherein the reinforcing fiber substrate is a carbon fiber substrate.
[0047] Effects of the Invention
[0048] According to the present invention, an epoxy resin composition for RTM can be provided that can obtain a resin cured product having an excellent balance of elastic modulus, heat resistance, and fracture toughness in a hot and humid environment. In addition, the epoxy resin composition for RTM of the present invention can be used as an epoxy resin composition for RTM suitable for manufacturing a large and high Vf fiber-reinforced composite material by injection molding because it maintains the above-mentioned properties in the resin cured product and has low viscosity and low volatility in the resin injection process. DETAILED DESCRIPTION
[0049] The epoxy resin composition for RTM of the present invention comprises [A] a tetrafunctional glycidylamine type epoxy resin, [B] at least one aromatic amine curing agent selected from alkylphenylenediamine and methylenedianiline, and [C] an aniline type epoxy resin represented by formula (I) as essential components. In addition, it is preferred to comprise core-shell rubber particles as component [D], and at least one solid epoxy resin selected from dicyclopentadiene type epoxy resin, biphenyl type epoxy resin, phenol aralkyl type epoxy resin, and naphthalene type epoxy resin as component [E]. First, these components are described.
[0050] (ingredient [A])
[0051] The epoxy resin composition for RTM of the present invention needs to include a 4-functional glycidylamine type epoxy resin as component [A]. By including component [A], the cured resin obtained by curing the epoxy resin composition for RTM of the present invention exhibits high heat resistance, and has excellent wet heat elastic modulus. In the absence of component [A], the heat resistance of the cured resin obtained by curing the epoxy resin composition is insufficient. In addition, component [A] preferably includes 20 parts by mass or more and 80 parts by mass or less among 100 parts by mass of all epoxy resins, more preferably includes 40 parts by mass or more and 60 parts by mass or less, and further preferably includes 40 parts by mass or more and 50 parts by mass or less. Here, the so-called 20 parts by mass or more and 80 parts by mass or less among 100 parts by mass of all epoxy resins means that when all epoxy resins contained in the epoxy resin composition for RTM of the present invention are set to 100 parts by mass, it means that 20 parts by mass or more and 80 parts by mass or less (the same expression below is also the same). The so-called all epoxy resins here refer to all epoxy resin components contained in the epoxy resin composition for RTM of the present invention. By satisfying the above range, when the epoxy resin composition for RTM of the present invention is cured, an epoxy resin cured product having high heat resistance and high elastic modulus under wet heat can be obtained. Therefore, by using the epoxy resin composition as a matrix resin, a fiber-reinforced composite material having excellent compressive strength under wet heat can be obtained.
[0052] Examples of such a component [A] include tetraglycidyldiaminodiphenylmethane and tetraglycidyldiaminodiphenylsulfone.
[0053] Among the above-mentioned commercial products of tetraglycidyldiaminodiphenylmethane, there are "スミエポキシ (registered trademark)" ELM-434, "スミエポキシ (registered trademark)" "Micro (Registered Trademark)" ELM-434VL (above, manufactured by Sumitomo Chemical Co., Ltd.), YH434L (Japanese Iron & Steel Co., Ltd. Made by Mitsubishi Aircraft Co., Ltd.), "jER (registered trademark)" 604 (manufactured by Mitsubishi Aircraft Co., Ltd.), "JER (registered trademark) (Trademark)" MY720, "Alaron (Registered Trademark)" MY721 (above, manufactured by Hinoman Co., Ltd.), etc.
[0054] Commercially available products of the tetraglycidyldiaminodiphenylsulfone include TG3DAS (manufactured by Konishi Chemical Industries, Ltd.) and the like.
[0055] (ingredient [C])
[0056] The epoxy resin composition for RTM of the present invention needs to contain the aniline epoxy resin shown in formula (I) as component [C]. By containing component [C], the elastic modulus of the cured resin obtained by curing the epoxy resin composition for RTM of the present invention can be maintained, while the elastic modulus of the rubber state is low. In the case where component [C] is not included, the elastic modulus of the cured resin obtained by curing the epoxy resin composition is low. In addition, component [C] preferably contains 10 parts by mass or more and 50 parts by mass or less among 100 parts by mass of all epoxy resins, and more preferably contains 20 parts by mass or more and 40 parts by mass or less. By satisfying the above range, if the epoxy resin composition for RTM of the present invention is cured, an epoxy resin cured product with high heat resistance and high elastic modulus during wet heat can be obtained.
[0057] Examples of such component [C] include diglycidyl-p-phenoxyaniline, diglycidyl-4-(4-methylphenoxy)aniline, diglycidyl-4-(4-tert-butylphenoxy)aniline, and diglycidyl-4-(4-phenoxyphenoxy)aniline. Among them, diglycidyl-p-phenoxyaniline (n=0, m=0, X=-O- in formula (I)) having a small molecular weight exhibits a low viscosity and is suitable for use in the resin injection process.
[0058] Examples of commercially available products of such diglycidyl-p-phenoxyaniline include "TOREP (registered trademark)" A-204E (diglycidyl-p-phenoxyaniline) (manufactured by Toray Film Chemical Co., Ltd.).
[0059] (ingredient [D])
[0060] The epoxy resin composition for RTM of the present invention preferably contains 1 part by mass or more and 10 parts by mass or less of core-shell rubber particles as component [D] relative to 100 parts by mass of the total epoxy resin, and more preferably contains 3 parts by mass or more and 6 parts by mass or less. By containing the component [D] in the above range, when the epoxy resin composition for RTM of the present invention is cured, the elastic modulus of the obtained resin cured product can be not damaged and the fracture toughness can be made higher. Therefore, by using the epoxy resin composition for RTM of the present invention as a matrix resin, a fiber-reinforced composite material with better compression characteristics and impact resistance can be obtained. When the compounding amount of component [D] is less than 1 part by mass, sometimes the effect of sufficient toughness improvement cannot be obtained in the obtained resin cured product. When the compounding amount of component [D] exceeds 10 parts by mass, sometimes the viscosity of the epoxy resin composition for RTM is high in the resin injection process, and sometimes the elastic modulus is low in the obtained resin cured product.
[0061] As commercially available products of such component [D], “Kaneace (registered trademark)” MX-125, “Kaneace (registered trademark)” MX-150, “Kaneace (registered trademark)” MX-154, “Kaneace (registered trademark)” MX-257, “Kaneace (registered trademark)” MX-267, “Kaneace (registered trademark)” MX-416, “Kaneace (registered trademark)” MX-451 (all manufactured by Kaneka Co., Ltd.), “PARALOID (registered trademark)” EXL-2655, “PARALOID (registered trademark)” EXL-2668 (all manufactured by Dow Chemical Co., Ltd.) and the like can be used.
[0062] The resin toughness value of the epoxy resin cured product in the present invention can be evaluated, for example, by the K1c value obtained from the SENB test described in ASTM D5045-99.
[0063] (ingredient [B])
[0064] The component [B] in the present invention is at least one aromatic amine curing agent selected from the group consisting of alkylphenylenediamine and methylenedianiline.
[0065] Such alkylphenylenediamine is an aromatic amine compound having one or more alkyl groups and two amino groups on a benzene ring, and diethyltoluenediamine, dimethylthiotoluenediamine and other toluenediamines are preferably used. By using alkylphenylenediamine as a curing agent for epoxy resin, the viscosity of the epoxy resin composition for RTM can be suppressed in the resin injection process, and a resin cured product with excellent elastic modulus can be obtained. Among them, dimethylthiotoluenediamine is particularly preferred in that a resin cured product with excellent balance between elastic modulus and toughness can be obtained.
[0066] Commercially available products of such alkylphenylenediamines include "jER Cure (registered trademark)" WA (manufactured by Mitsubishi Chemika, Ltd.), "Ethacure (registered trademark)" 100 (manufactured by Albemarle), "Huto Cure (registered trademark)" 10 (manufactured by Kumiai Chemical Industries, Ltd.), "Lonzacure (registered trademark)" DETDA80 (manufactured by Lonza), "Ethacure (registered trademark)" 300 (manufactured by Albemarle), and "Huto Cure (registered trademark)" 30 (manufactured by Kumiai Chemical Industries, Ltd.).
[0067] Such methylenedianiline is an aromatic amine compound obtained by cross-linking two aniline compounds through a methylene group, and various substituents may exist on each benzene ring. By using methylenedianiline as a curing agent for epoxy resin, a resin cured product with low water absorption and excellent toughness can be obtained.
[0068] Examples of such methylenedianiline include 4,4-methylenebis(isopropyl-6-methylaniline) (M-MIPA), methylenebis(diethylaniline) (M-DEA), methylenebis(chlorodiethylaniline) (M-CDEA), and methylene(methylethylaniline)-(chlorodiethylaniline) (M-MEACDEA). Among them, 4,4-methylenebis(isopropyl-6-methylaniline) is particularly preferred because a cured resin having an excellent balance between elastic modulus and toughness can be obtained.
[0069] Commercially available products of such methylenedianiline include MDA-220 (manufactured by Mitsui Chemicals, Inc.), "Lonzacure (registered trademark)" M-MIPA, "Lonzacure (registered trademark)" M-DEA, "Lonzacure (registered trademark)" M-CDEA, "Lonzacure (registered trademark)" M-DIPA (all manufactured by Lonza Corporation), and "Kayama (registered trademark)" AA (PT) (manufactured by Nippon Kayaku Co., Ltd.).
[0070] In the present invention, component [B] is preferably an alkylphenylenediamine, and more preferably contains both an alkylphenylenediamine and methylenedianiline as component [B].
[0071] When the component [B] in the present invention is an alkylphenylenediamine, it is preferred in that the viscosity of the epoxy resin composition for RTM can be sufficiently suppressed in the resin injection step and a cured resin having an excellent elastic modulus can be obtained.
[0072] On the other hand, when alkylphenylenediamine and methylenedianiline are contained as component [B] in the present invention, it is preferable in that the viscosity of the epoxy resin composition for RTM can be suppressed in the resin injection step, and a resin cured product having an excellent balance among elastic modulus, low water absorption and toughness can be obtained.
[0073] In the present invention, component [B] is preferably liquid at 23° C. When component [B] is liquid, the viscosity of the epoxy resin composition for RTM of the present invention can be reduced, and the composition can be suitably used for injection molding of fiber-reinforced composite materials.
[0074] (ingredient [E])
[0075] In the present invention, it is preferred that at least one solid epoxy resin selected from the group consisting of dicyclopentadiene epoxy resin, biphenyl epoxy resin, phenol aralkyl epoxy resin, and naphthalene epoxy resin is contained as component [E] in an amount of 10 parts by mass or more and 50 parts by mass or less, and more preferably 20 parts by mass or more and 40 parts by mass or less. By containing component [E] in the above range, the water absorption of the epoxy resin cured product can be reduced, and thus the wet heat elastic modulus can be increased.
[0076] In addition, for epoxy resins that can be used as component [E] and have a skeleton that can be classified as a dicyclopentadiene-type epoxy resin, a biphenyl-type epoxy resin, a phenol aralkyl-type epoxy resin, or a naphthalene-type epoxy resin, and that can correspond to component [A] or component [C] at the same time, they are treated as component [A] or component [C], respectively.
[0077] As component [E], dicyclopentadiene epoxy resin and naphthalene epoxy resin are preferably used in terms of excellent balance between elastic modulus and toughness. Dicyclopentadiene epoxy resin is particularly preferably used. In addition to the effect of reducing the water absorption of epoxy resin cured product, the fracture toughness of the resin cured product can also be improved.
[0078] Commercially available products of dicyclopentadiene-type epoxy resins that can be used as component [E] include "EPICLON (registered trademark)" HP-7200L, "EPICLON (registered trademark)" HP-7200, "EPICLON (registered trademark)" HP-7200H, and "EPICLON (registered trademark)" HP-7200HH (all manufactured by DIC Corporation).
[0079] Examples of commercially available biphenyl epoxy resins that can be used as the component [E] include "jER (registered trademark)" YX-4000 (manufactured by Mitsubishi Chemical Co., Ltd.).
[0080] Examples of commercially available phenol aralkyl epoxy resins that can be used as the component [E] include NC-3000H, NC-3000, NC-3000L, NC-7000, NC-7300, NC-2000, and NC-2000L (all manufactured by Nippon Kayaku Co., Ltd.).
[0081] Examples of commercially available naphthalene-type epoxy resins that can be used as the component [E] include "EPICLON (registered trademark)" HP-4770 and "EPICLON (registered trademark)" HP-4700 (each manufactured by DIC Corporation).
[0082] The epoxy resin composition for RTM of the present invention needs to satisfy all of the following conditions 1 to 4.
[0083] Condition 1: Viscosity at 110°C is 1 mPa·s or more and 200 mPa·s or less
[0084] Condition 2: Mass reduction after heating at 110°C for 30 minutes is 0.3 mass % or less
[0085] Condition 3: The rubber elastic modulus of the cured resin obtained by curing at 180°C for 2 hours is 2 MPa or more and 8 MPa or less
[0086] Condition 4: The water absorption of the cured resin obtained by curing at 180° C. for 2 hours is 1% or more and 3% or less.
[0087] Regarding the above condition 1, the epoxy resin composition for RTM of the present invention needs to have a viscosity at 110°C of 1 mPa·s or more and 200 mPa·s or less, preferably 2 mPa·s or more and 100 mPa·s or less, more preferably 5 mPa·s or more and 45 mPa·s or less, and further preferably 5 mPa·s or more and 40 mPa·s or less. By being in such a range, the epoxy resin composition for RTM has excellent impregnation into the reinforcing fiber substrate in the resin injection step, so the epoxy resin composition for RTM of the present invention can be used suitably for large structural materials.
[0088] The viscosity of the epoxy resin composition for RTM was measured using a dynamic viscoelasticity device in the measurement mode: parallel plates (25 mm φ, 1.0 mm interval), shear rate: 100 s. -1 The measurement was performed under the condition of setting the temperature to 110°C. At this time, the epoxy resin composition was placed on parallel plates heated to 110°C within 5 minutes after preparation with a gap of 1.0 mm, and the measurement was started. The complex viscosity at the time when the sample temperature rose to 110°C was defined as η0.
[0089] Regarding the above condition 2, the epoxy resin composition for RTM of the present invention needs to have a mass reduction rate of 0.3% by mass or less, preferably 0.2% by mass or less, and more preferably 0.15% by mass or less after heating at 110° C. for 30 minutes. By being within such a range, the volatilization of the resin component in the molding process can be suppressed, thereby obtaining a fiber-reinforced composite material with a high Vf and exhibiting excellent mechanical properties.
[0090] The mass reduction rate of the epoxy resin composition for RTM is obtained by placing about 2 g of the epoxy resin composition into an aluminum cup with an inner diameter of 50 mm, weighing it with an electronic balance, heating it in a forced air oven set at 110° C., taking it out after 30 minutes and cooling it to room temperature, and then weighing it again to calculate the mass reduction rate of the resin.
[0091] Regarding the above condition 3, the epoxy resin composition for RTM of the present invention needs to make the epoxy resin composition cured at 180°C for 2 hours to obtain a cured resin with a rubber state elastic modulus of 2MPa to 8MPa, preferably 2MPa to 6MPa, and more preferably 2MPa to 5MPa. By being in such a range, the cured resin obtained by curing the epoxy resin composition for RTM of the present invention maintains elastic modulus and heat resistance, while showing excellent fracture toughness, so the fiber-reinforced composite material obtained by using the epoxy resin composition as a matrix resin has excellent impact resistance. In the case where the rubber state elastic modulus is greater than 8MPa, the above effect cannot be obtained. In the case where the rubber state elastic modulus is less than 2MPa, although the fracture toughness is improved, the elastic modulus and heat resistance of the epoxy resin cured material are reduced, so the wet heat compression strength of the fiber-reinforced composite material is reduced.
[0092] The rubber state elastic modulus of such a cured resin is obtained by placing a test piece of thickness 2.0 mm, width 12.7 mm, and length 45 mm on a solid torsion fixture using a dynamic viscoelasticity measuring device, and measuring at a temperature range of 40°C to 260°C at a heating rate of 5°C / min, a frequency of 1 Hz, and a strain of 0.08%. Such a rubber state elastic modulus is the storage modulus at a temperature exceeding the glass transition temperature by 50°C in the obtained storage modulus and temperature graph. Such a glass transition temperature is the temperature at the intersection of the tangent drawn in the glass state and the tangent drawn in the glass transition temperature region in the obtained storage modulus and temperature graph.
[0093] Regarding the above condition 4, the epoxy resin composition for RTM of the present invention needs to make the epoxy resin composition cured at 180°C for 2 hours to obtain a resin cured product with a water absorption of 1% to 3%, preferably 1% to 2.5%, more preferably 1.5% to 2.2%, and further preferably 1.5% to 1.9%. By being in such a range, the elastic modulus of the cured resin obtained by curing the epoxy resin composition for RTM of the present invention is high, so the fiber-reinforced composite material obtained by using the epoxy resin composition as a matrix resin has excellent compression strength during wet heat. When the water absorption is greater than 3%, the above effect cannot be obtained. When the water absorption is less than 1%, the adhesion between the epoxy resin cured product and the reinforcing fiber in the fiber-reinforced composite material is reduced, so the impact resistance of the fiber-reinforced composite material is reduced.
[0094] The water absorption rate of such a cured resin is calculated from the difference in mass before and after immersing a test piece having a thickness of 2.0 mm, a width of 10 mm, and a length of 60 mm in boiling water for 48 hours.
[0095] The value (Mh / Me) obtained by dividing the sum of the number of active hydrogen moles (Mh) of the component [B] included in the epoxy resin composition for RTM of the present invention by the sum of the number of active epoxy moles (Me) included in all epoxy resins is preferably in the range of 0.8 or more and 1.1 or less, and more preferably in the range of 0.9 or more and 1.0 or less. Here, all epoxy resins refer to all epoxy resin components included in the epoxy resin composition for RTM of the present invention. By being such a range, when the epoxy resin composition for RTM of the present invention is cured, the reaction of the epoxy resin and the curing agent occurs efficiently, so that the water absorption of the resin cured product decreases, and therefore the wet heat elastic modulus of the resin cured product is high, and a fiber-reinforced composite material showing higher compression characteristics during wet heat is obtained when the resin cured product is used as a matrix resin. In addition, since the heat resistance after wetting is also excellent, it is suitable for use as a fiber-reinforced composite material for structural materials.
[0096] The total number of moles of active epoxy groups contained in all epoxy resins (Me) is the sum of the number of moles of active groups of each epoxy resin contained in the epoxy resin composition for RTM, and is represented by the following formula.
[0097] Me=(mass of epoxy resin A / epoxy equivalent of epoxy resin A)+(mass of epoxy resin B / epoxy equivalent of epoxy resin B)+····+(mass of epoxy resin W / epoxy equivalent of epoxy resin W).
[0098] The total number of active hydrogen moles (Mh) of the component [B] is obtained by dividing the mass of the component [B] contained in the epoxy resin composition for RTM by the active hydrogen equivalent thereof.
[0099] Mh = (mass of component [B]1 / active hydrogen equivalent of component [B]1) + (mass of component [B]2 / active hydrogen equivalent of component [B]2) + ... + (mass of component [B]1 / active hydrogen equivalent of component [B]1) n Quality / composition [B] n active hydrogen equivalent).
[0100] Here, the epoxy resin composition for RTM of the present invention has the characteristic that the heat resistance (wet Tg) of the resin cured product formed by curing the epoxy resin composition at 180°C for 120 minutes when wet is less than the heat resistance (dry Tg) when dry. In the case of applying fiber-reinforced composite materials as structural materials represented by aircraft, the smaller the reduction of wet Tg, the more preferred. As an index thereof, the reduction rate can be represented by the ratio of wet Tg to dry Tg (wet Tg / dry Tg), but wet Tg / dry Tg is preferably in the range of more than 0.9 and less than 1.0, more preferably more than 0.93 and less than 1.0. Wet Tg, for example, can be evaluated by the following DMA determination using a test piece in which the resin cured product is immersed in boiling water for 48 hours.
[0101] The glass transition temperature (Tg) of the cured resin of the present invention can be calculated from a scatter diagram of storage modulus and temperature obtained by performing a temperature increase measurement of a DMA measurement (dynamic viscoelasticity measurement). The glass transition temperature is the temperature at the intersection of a tangent drawn in the glass region and a tangent drawn in the glass transition region in the scatter diagram. In addition, the storage modulus in the rubber state (rubber state elastic modulus) is the storage modulus at a temperature exceeding the glass transition temperature by 50°C.
[0102] The epoxy resin composition for RTM of the present invention also has a wet heat flexural modulus of 82° C. (E 82 ) and the flexural modulus of elasticity (E 23 ) is smaller than that of the previous one. As an indicator, E 82 With E 23 The ratio (E 82 / E 23 ) indicates the reduction rate, but E 82 / E 23 It is preferably 0.75 or more, more preferably 0.80 or more, and even more preferably 0.85 or more.
[0103] The epoxy resin composition for RTM used in the present invention may contain an epoxy resin different from the components [A], [C], and [E] as the component [F] within a range that does not impair the effects of the present invention.
[0104] Examples of such epoxy resins include bisphenol A epoxy resins, bisphenol F epoxy resins, phenol novolac epoxy resins, triglycidylaminophenol epoxy resins, etc. These may be used alone or in combination of two or more.
[0105] Examples of commercially available products of the bisphenol A type epoxy resin include "jER (registered trademark)" 828 and "jER (registered trademark)" 825 (each manufactured by Mitsubishi Chemical Co., Ltd.).
[0106] Examples of commercially available products of the bisphenol F-type epoxy resin include "EPICLON (registered trademark)" 830, "EPICLON (registered trademark)" 807 (each manufactured by DIC Corporation), and "jER (registered trademark)" 806 (manufactured by Mitsubishi Chemical Corporation).
[0107] Examples of commercially available products of the phenol novolac epoxy resin include "jER (registered trademark)" 152, "jER (registered trademark)" 154, and "jER (registered trademark)" 180S (all manufactured by Mitsubishi Chemical Co., Ltd.).
[0108] Examples of commercially available products of the triglycidylaminophenol-type epoxy resins include “Sumipochi (registered trademark)” ELM100 and ELM120 (manufactured by Sumitomo Chemical Industries, Ltd.), “Aldite (registered trademark)” MY0500, “Aldite (registered trademark)” MY0510, and “Aldite (registered trademark)” MY0600 (all manufactured by Handman Advanced Materials Co., Ltd.), and “jER (registered trademark)” 630 (manufactured by Mitsubishi Chemical Corporation).
[0109] In the preparation of the epoxy resin composition for RTM of the present invention, kneading can be performed using machines such as a kneader, planetary mixer, three-roll and twin-screw extruder. Alternatively, mixing can be performed manually using a beaker or a spatula as long as uniform kneading can be performed.
[0110] The epoxy resin composition for RTM of the present invention is particularly suitable for the RTM method because it shows long-term viscosity stability at a relatively high temperature and has excellent impregnation characteristics for the reinforcing fiber substrate. The so-called RTM method is a method in which a reinforcing fiber substrate or a preform is placed in a molding die, a liquid matrix resin is injected into the molding die to impregnate the reinforcing fiber, and then the epoxy resin composition is cured by heating to obtain a fiber-reinforced composite material as a molded product. The temperature of the matrix resin during injection in the method for manufacturing a fiber-reinforced composite material using the epoxy resin composition for RTM of the present invention is not particularly limited, but it is preferred to place a reinforcing fiber substrate in a molding die preheated to 70°C to 190°C and inject the epoxy resin composition for RTM of the present invention. By preheating the molding die, the viscosity of the epoxy resin composition is reduced, the injection time is shortened, and therefore mass production is excellent. In addition, the thermal curing temperature does not need to be the same as the temperature at the time of injection, and the time required for thermal curing can be shortened by appropriately increasing the temperature.
[0111] In the present invention, the mold used in the RTM method can use a closed mold formed of a rigid material, and can also use an open mold of a rigid material and a flexible film (bag). In the latter case, the reinforcing fiber substrate can be arranged between the open mold of the rigid material and the flexible film. As the rigid material, various existing materials such as metals such as steel and aluminum, fiber reinforced plastics (FRP), wood, gypsum, etc. are used. Among the materials of the flexible film, polyamide, polyimide, polyester, fluororesin, silicone resin, etc. are used.
[0112] The reinforcing fiber used in the reinforcing fiber substrate used in the fiber-reinforced composite material of the present invention is not particularly limited, and the reinforcing fiber used in the present invention is not particularly limited, and glass fiber, carbon fiber, aramid fiber, boron fiber, alumina fiber, silicon carbide fiber, etc. can be used. These fibers can also be mixed with two or more and used. From the viewpoint of obtaining a lightweight and highly rigid fiber-reinforced composite material, it is preferred to use carbon fiber.
[0113] The fiber-reinforced composite material of the present invention has excellent mechanical properties, compression strength when wet and hot, and impact resistance, and can therefore be preferably used for a large number of structural materials such as aircraft components such as fuselages, main wings, tail wings, control surfaces, fairings, cowls, doors, seats, and interior materials, spacecraft components such as motor housings and main wings, artificial satellite components such as structures and antennas, automobile components such as outer panels, chassis, aerodynamic components, and seats, railway vehicle components such as structures and seats, and ship components such as hulls and seats.
[0114] Example
[0115] The present invention will be described in more detail below with reference to Examples, but the present invention is not limited to the description of these Examples.
[0116] The materials, sample preparation methods, and evaluation methods used in the present examples are as follows.
[0117] <Materials used>
[0118] (1) Component [A]: tetrafunctional glycidylamine type epoxy resin
[0119] [A]-1 "Sumipokishi (registered trademark)" ELM434VL (manufactured by Sumitomo Chemical Co., Ltd., epoxy equivalent: 115 g / eq),
[0120] [A]-2 "Araldo (Registered Trademark)" MY721 (manufactured by Hakuman Co., Ltd., epoxy equivalent: 115g / eq),
[0121] [A]-3 "Sumipokishi (registered trademark)" ELM434 (manufactured by Sumitomo Chemical Co., Ltd., epoxy equivalent: 120 g / eq).
[0122] (2) Component [B]: at least one aromatic amine curing agent selected from alkylphenylenediamine and methylenedianiline
[0123] (2-1) Alkylphenylenediamine
[0124] [B]-1: "jER CURA (registered trademark)" WA (manufactured by Mitsubishi Chemical Co., Ltd., active hydrogen equivalent: 45 g / eq),
[0125] [B]-2: "Ethacure (registered trademark)" 300 (manufactured by Albemarle Corporation, active hydrogen equivalent: 54 g / eq),
[0126] (2-2) Methylenedianiline
[0127] [B]-3: "Lonzacure (registered trademark)" M-MIPA (manufactured by Lonza, active hydrogen equivalent: 78 g / eq),
[0128] [B]-4: “Lonzacure (registered trademark)” M-CDEA (manufactured by Lonza, active hydrogen equivalent: 95 g / eq).
[0129] (3) Component [D]: a mixture of core-shell rubber particles and component [A] or component [F]
[0130] [D]-1 "Kaneace (registered trademark)" MX-416 (75% by mass of glycidylamine epoxy resin (corresponding to component [A]), and 25% by mass of butadiene core-shell rubber particles, epoxy equivalent: 148 g / eq),
[0131] [D]-2 "Kaneice (registered trademark)" MX-267 (63% by mass of bisphenol F epoxy resin (equivalent to component [F]), and 37% by mass of butadiene core-shell rubber particles, epoxy equivalent: 270 g / eq) (all manufactured by Kaneka Co., Ltd.).
[0132] (4) Component [C]: glycidylaniline epoxy resin represented by formula (I)
[0133] "TOREP (registered trademark)" A-204E (manufactured by Higashikata Chemical Co., Ltd., epoxy equivalent: 162 g / eq).
[0134] (5) Component [E]: at least one solid epoxy resin selected from the group consisting of dicyclopentadiene epoxy resin, biphenyl epoxy resin, phenol aralkyl epoxy resin, and naphthalene epoxy resin
[0135] (5-1) Dicyclopentadiene type epoxy resin
[0136] [E]-1 "EPICLON (registered trademark)" HP-7200L (manufactured by DIC Corporation, epoxy equivalent: 246 g / eq),
[0137] [E]-2 "EPICLON (registered trademark)" HP-7200H (manufactured by DIC Corporation, epoxy equivalent: 278 g / eq),
[0138] (5-2) Biphenyl type epoxy resin
[0139] [E]-3 "jER (registered trademark)" YX-4000 (manufactured by Mitsubishi Chemical Co., Ltd., epoxy equivalent: 186 g / eq),
[0140] (5-3) Phenol aralkyl type epoxy resin
[0141] [E]-4NC-3000L (manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent: 272 g / eq).
[0142] (6) Component [F]: other epoxy resin
[0143] [F]-1GAN (manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent: 125 g / eq),
[0144] [F]-2 "jER (registered trademark)" 828 (manufactured by Mitsubishi Chemical Co., Ltd., epoxy equivalent: 189 g / eq),
[0145] [F]-3 "EPICLON (registered trademark)" 830 (manufactured by DIC Corporation, epoxy equivalent: 171 g / eq),
[0146] [F]-4 "jER (registered trademark)" 630 (manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: 98 g / eq).
[0147] (7) Other curing agent components
[0148] [G]-1: "Seika Kyua (registered trademark)" S (manufactured by Wakayama Seika Co., Ltd., active hydrogen equivalent: 62 g / eq).
[0149] <Method for preparing epoxy resin composition for RTM>
[0150] Predetermined amounts of components other than component [B] and other curing agent components were placed in a stainless steel beaker, the temperature was raised to 60 to 150° C., and kneaded appropriately until the components were compatible to obtain an epoxy main agent liquid.
[0151] Component [B] and other curing agent components are added to another container, and heated as necessary to compatibilize them to obtain a curing agent liquid.
[0152] Predetermined amounts of epoxy main agent liquid and curing agent liquid were mixed at about 60° C. and kneaded for 3 minutes using a planetary mixer to obtain an epoxy resin composition for RTM. The compositions are shown in Tables 1 to 4.
[0153] <Method for producing fiber-reinforced composite materials>
[0154] (1) Preparation of reinforcing fiber substrate with non-woven fabric
[0155] A nonwoven fabric made of polyamide 12 (fiber weight per unit area: 6 g / m 2 ) is attached to a plain woven fabric made of carbon fiber "トレカ (registered trademark)" T700G-12K-31E as a reinforcing fiber (fiber unit area weight: 285g / m 2 Then, the nonwoven fabric was fused using a far-infrared heater, thereby obtaining a reinforcing fiber substrate with a nonwoven fabric applied to one surface.
[0156] (2) Fabrication of fiber-reinforced composite materials
[0157] The reinforcing fiber substrate with nonwoven fabric obtained by the preparation of the reinforcing fiber substrate with nonwoven fabric described above (1) was cut into 400 mm × 400 mm in such a way that the fiber directions became 0° / 90° and 45° / -45°. The cut reinforcing fiber substrate with nonwoven fabric was stacked in a mold in a configuration of [(45° / -45°) / (0° / 90°)]4s. Next, the mold was heated to 110°C, and the epoxy resin composition obtained according to the above <Preparation method of epoxy resin composition> which was pre-heated to 110°C was injected into the mold. Then, the temperature was raised to 180°C at a rate of 1.5°C / min, and it was cured at 180°C for 2 hours to obtain a fiber-reinforced composite material.
[0158] <Evaluation Method>
[0159] The evaluation methods in Examples are described below. In the evaluation methods, for evaluations where the number of measurements n is 1, the description of the number of measurements n is omitted.
[0160] (1) Method for evaluating viscosity (η0) of epoxy resin composition for RTM at 110°C
[0161] The epoxy resin composition for RTM obtained according to the above-mentioned <Preparation method of epoxy resin composition for RTM> is mixed and set on a parallel plate set at 110°C in the following apparatus within 5 minutes so as to be 1.0 mm. The measurement is started under the following conditions, and the complex viscosity of the epoxy resin composition for RTM when it reaches 110°C is defined as η0.
[0162] Measuring device: Dynamic viscoelasticity measuring device (Discovery HR-2, manufactured by TA Instruments Co., Ltd.)
[0163] Measurement mode: Parallel plate (25mmφ, interval 1.0mm)
[0164] Shear speed: 100s -1
[0165] Set temperature: 110℃.
[0166] (2) Method for evaluating mass reduction rate of epoxy resin composition for RTM at 110°C
[0167] About 2 g of the epoxy resin composition for RTM obtained according to the above <Preparation method of epoxy resin composition for RTM> was put into an aluminum cup with an inner diameter of 50 mm, weighed with an electronic balance, and heated in a forced air oven (DKM400, manufactured by Yamato Scientific Co., Ltd.) set at 110°C. After 30 minutes, it was taken out and cooled to room temperature, and then weighed again to calculate the mass reduction rate of the resin. The number of samples n = 5, and the average value was adopted as the value of the mass reduction rate.
[0168] (3) Flexural modulus of cured resin (23°C, 50% RH): E 23 Evaluation method
[0169] The epoxy resin composition for RTM obtained according to the above <Preparation method of epoxy resin composition for RTM> was degassed in vacuum, and then cured at 180°C for 2 hours in a mold set to have a thickness of 2mm through a 2mm thick "Teflon (registered trademark)" spacer, to obtain a plate-shaped resin cured product with a thickness of 2mm. A test piece with a width of 10mm and a length of 60mm was cut out from the resin cured product, and a span of 32mm and a crosshead speed of 10mm / min were used using an Instron universal testing machine (manufactured by Instron Co., Ltd.), and three-point bending was performed at room temperature (23°C, 50%RH) in accordance with JIS K7171 (1994), and the bending modulus (23°C, 50%RH) was measured. At this time, the number of samples n=6, and the average value thereof was adopted as the value of the bending modulus.
[0170] (4) Flexural modulus of cured resin (wet heat 82°C): E 82 Evaluation method of water absorption
[0171] By comparing with the above (3) Flexural modulus of the cured resin (23°C, 50% RH): E 23 The resin cured product was obtained by the same method as the evaluation method of the test piece, and a test piece with a width of 10 mm and a length of 60 mm was cut out and immersed in boiling water for 48 hours. The taken-out test piece was used with an Instron universal testing machine (manufactured by Instron Co., Ltd.), with a span of 32 mm and a crosshead speed of 10 mm / min. According to JIS K7171 (1994), three-point bending was performed under a high temperature environment (82°C) to measure the bending modulus (wet heat 82°C). In addition, the mass of the above-mentioned test piece before and after immersion in boiling water for 48 hours was measured, and the water absorption was calculated from the difference in mass. At this time, the number of samples n=6, and the average value was used as the value of the bending modulus.
[0172] (5) Evaluation method of glass transition temperature (drying Tg) of cured resin
[0173] The epoxy resin composition for RTM obtained according to the above <Preparation method of epoxy resin composition for RTM> was degassed in a vacuum in an uncured state, and then cured at a temperature of 180°C for 2 hours in a mold set to a thickness of 2mm by a 2mm thick "Teflon (registered trademark)" spacer, to obtain a plate-shaped resin cured product with a thickness of 2mm. A test piece with a width of 12.7mm and a length of 45mm was cut out from the cured resin, and the test piece was set in a solid torsion fixture with a distance of 30mm between the fixtures using a dynamic viscoelasticity measuring device (ARES-G2, manufactured by TA Instruments Co., Ltd.), and the test piece was set in the solid torsion fixture, and the temperature range of 40 to 260°C was measured at a heating rate of 5°C / min, a frequency of 1Hz, and a strain of 0.08%. At this time, the glass transition temperature (drying Tg) is set to the temperature at the intersection of the tangent line drawn in the glass state and the tangent line drawn in the glass transition temperature region in the obtained storage modulus and temperature graph. The rubber state elastic modulus is set to the storage modulus at a temperature exceeding the glass transition temperature by 50°C in the obtained storage modulus and temperature graph.
[0174] (6) Evaluation method of glass transition temperature (wet Tg) of cured resin
[0175] The resin cured product was obtained by the same method as the evaluation method of the glass transition temperature (dry Tg) of the resin cured product (5) above, and a test piece with a width of 12.7 mm and a length of 45 mm was cut out and immersed in boiling water for 48 hours. The viscoelasticity was measured by the same method as the evaluation method of the glass transition temperature (dry Tg) of the resin cured product above, and the glass transition temperature (wet Tg) was obtained.
[0176] (7) Evaluation method of fracture toughness value of cured resin
[0177] The epoxy resin composition for RTM obtained according to the above <Preparation method of epoxy resin composition for RTM> was degassed in vacuum, and then cured at 180°C for 2 hours in a mold set to a thickness of 6 mm by a 6 mm thick "Teflon (registered trademark)" spacer, to obtain a 6 mm thick plate-shaped resin cured product. The obtained resin cured product was processed into a test piece shape described in ASTM D5045-99, and a SENB test was performed according to ASTM D5045-99. At this time, the number of samples n = 16, and the average value was used as the fracture toughness value K1c value.
[0178] (8) Open hole compressive strength of fiber reinforced composite materials (23°C, 50% RH): OHC 23 Evaluation method
[0179] From the fiber reinforced composite material obtained according to the above <Preparation of fiber reinforced composite material>, a rectangle with a length of 304.8 mm in the 0° direction and 38.1 mm in the 90° direction was cut to obtain a test piece with a circular hole with a diameter of 6.35 mm in the center. For this test piece, the open hole compression strength (23°C, 50% RH) was measured at room temperature (23°C, 50% RH) using an Instron universal testing machine (manufactured by Instron Co., Ltd.) in accordance with ASTM-D6484. At this time, the number of samples n = 5, and the average value is used as the OHC 23 value.
[0180] (9) Open hole compressive strength of fiber reinforced composite materials (wet heat 82°C): OHC 82 Evaluation method
[0181] The test piece was obtained by the same method as the evaluation method of the open hole compressive strength (23°C, 50% RH) of the fiber reinforced composite material (8). The test piece was immersed in 72°C warm water for 14 days, and then the open hole compressive strength (wet heat 82°C) was measured in a high temperature environment (82°C) using an Instron universal testing machine (manufactured by Instron Co., Ltd.) in accordance with ASTM-D6484. At this time, the number of samples n = 5, and the average value was used as the OHC 82 value.
[0182] (10) Evaluation method of compressive impact strength (CAI) of fiber-reinforced composite materials
[0183] A rectangular test piece having a length of 150 mm in the 0° direction and 100 mm in the 90° direction was cut out from the fiber-reinforced composite material obtained according to the above <Production of fiber-reinforced composite material>. The test piece was subjected to a 6.7 J / mm water drop impact at the center of the test piece according to JIS K7089 (1996), and the post-impact compressive strength was measured using an Instron universal testing machine (manufactured by Instron Co., Ltd.) according to JIS K7089 (1996). At this time, the number of samples n = 5, and the average value thereof was adopted as the CAI value.
[0184] The following describes the method for preparing the samples in each example, the properties of the cured resin, and the measurement results of the properties of the uncured resin.
[0185] (Example 1)
[0186] As epoxy resins, 25 parts by mass of "Sumi Epoxi (registered trademark)" ELM-434VL (component [A]), 30 parts by mass of "TOREP (registered trademark)" A-204E (component [C]), 30 parts by mass of "EPICLON (registered trademark)" HP-7200H (component [E]), 20 parts by mass of "Kaneace (registered trademark)" MX-416 (5 parts by mass of component [D] and 15 parts by mass of component [A]), 9.5 parts by mass of "jER Kyura (registered trademark)" WA (component [B]), and 28.4 parts by mass of "Lonzacure (registered trademark)" M-MIPA (component [B]) were used to prepare an epoxy resin composition for RTM according to the above-mentioned <Method for preparing epoxy resin composition for RTM>.
[0187] Regarding the epoxy resin composition for RTM, the bending elastic modulus (23° C., 50% RH) of the cured resin in the above (3) is: 23 Evaluation method and (4) Flexural modulus of cured resin (wet heat 82°C): E 82 The flexural properties were obtained by evaluating the water absorption rate. 23 3.75GPa, E 82 3.20GPa, E 82 / E 23 It is 0.85, showing excellent wet heat elastic modulus. In addition, the heat resistance was evaluated according to the above-mentioned (5) evaluation method of the glass transition temperature (dry Tg) of the resin cured product and (6) the evaluation method of the glass transition temperature (wet Tg) of the resin cured product. The result was that the dry Tg was 178°C, the wet Tg was 170°C, and the wet Tg / dry Tg was 0.96, showing excellent heat resistance. In addition, the water absorption rate was 1.7%, which is extremely good, and the rubber state elastic modulus was 4.2 MPa. In addition, according to the above-mentioned (7) evaluation method of the fracture toughness value of the resin cured product, the fracture toughness value was evaluated, and the result was 1.2 MPa·m 0.5 , is good.
[0188] In addition, regarding the viscosity, η0 was evaluated according to the evaluation method of the viscosity (η0) of the epoxy resin composition for RTM at 110°C described above (1), and the result was 40 mPa·s. In addition, the mass reduction rate was evaluated according to the evaluation method of the mass reduction rate of the epoxy resin composition for RTM at 110°C described above (2), and the result was 0.12 mass %.
[0189] (Examples 2 to 21)
[0190] Epoxy resin compositions for RTM and cured resins were prepared by the same method as in Example 1 except that the resin compositions were changed as shown in Tables 1 to 3, respectively.
[0191] The wet heat and room temperature elastic modulus, wet and dry Tg, water absorption, and fracture toughness of the epoxy resin composition for RTM of each example were evaluated, and good physical properties were obtained at all levels. In addition, η0 of each example was 18 mPa·s or more and 50 mPa·s or less, the mass reduction rate was 0.07 mass% or more and 0.20 mass% or less, and the rubber state elastic modulus was within the range of 3.5 MPa or more and 8.0 MPa or less.
[0192] (Comparative Example 1)
[0193] An epoxy resin composition for RTM was prepared by the method described in Example 2 of Patent Document 1 (Japanese Patent No. 5808057) with the resin composition shown in Table 4. The curing agent (M-CDEA) of the epoxy resin composition was solid.
[0194] Regarding the epoxy resin composition for RTM, the bending elastic modulus (23° C., 50% RH) of the cured resin in the above (3) is: 23 Evaluation method and (4) Flexural modulus of cured resin (wet heat 82°C): E 82 and water absorption evaluation method, the bending properties were obtained, and the results showed that although E 23 Up to 3.80GPa, but E 82 2.60GPa, significantly lower than E 82 / E 23 It became 0.68. In addition, the heat resistance was evaluated according to the evaluation method of the glass transition temperature (dry Tg) of the resin cured product (5) and the evaluation method of the glass transition temperature (wet Tg) of the resin cured product (6). The result was that the dry Tg was 175°C, the wet Tg was 155°C, and the wet Tg / dry Tg was 0.89. The heat resistance decreased significantly after wetting, and the water absorption rate was as high as 3.0%. In addition, according to the evaluation method of the fracture toughness value of the resin cured product (7), the fracture toughness value was evaluated, and the result was 0.9 MPa·m 0.5 , which is insufficient. The elastic modulus in the rubber state is 10.0 MPa, which is out of the range. η0 is 50 mPa·s, and the mass reduction rate is 0.22 mass %.
[0195] (Comparative Example 2)
[0196] An epoxy resin composition for RTM was prepared with the resin composition shown in Table 4 by the method described in Example 26 of Patent Document 2 (International Publication No. 2021 / 241734).
[0197] The epoxy resin composition was evaluated by the same method as in Example 1. 82 and E23 , wet and dry Tg, water absorption, fracture toughness value, rubber state elastic modulus, η0, and mass reduction rate.
[0198] This epoxy resin composition contains component [A] and component [B], but does not contain component [C], and instead contains bisphenol F-type epoxy resin and TGpAP as other epoxy resins. 82 As low as 2.40GPa, E 82 / E 23 The elastic modulus after wetting is 0.71, and the elastic modulus after wetting is greatly reduced. In addition, the dry Tg is 184°C, the wet Tg is 160°C, the wet Tg / dry Tg is 0.87, and the heat resistance after wetting is greatly reduced. The water absorption rate is also as high as 2.8%. In addition, the fracture toughness value is 0.8MPa·m 0.5 The elastic modulus in the rubber state is 12.0 MPa, which is out of the range.
[0199] (Comparative Example 3)
[0200] An epoxy resin composition for RTM was prepared with the resin composition shown in Table 4 by the method described in Example 24 of Patent Document 2 (Japanese Patent Application Laid-Open No. 2010-150310).
[0201] The epoxy resin composition was evaluated by the same method as in Example 1. 82 and E 23 , wet and dry Tg, water absorption, fracture toughness value, rubber state elastic modulus, η0, and mass reduction rate.
[0202] The epoxy resin composition contains component [A] and component [B], but does not contain component [C]. 82 As low as 2.40GPa, E 82 / E 23 The elastic modulus after wetting is 0.73, and the elastic modulus after wetting is greatly reduced. In addition, the dry Tg is 182°C, the wet Tg is 158°C, the wet Tg / dry Tg is 0.87, and the heat resistance after wetting is greatly reduced. The water absorption rate is also as high as 2.7%. In addition, the fracture toughness value is 0.9MPa·m 0.5 The elastic modulus in the rubber state is 10.1 MPa, which is out of the range.
[0203] (Comparative Example 4)
[0204] The epoxy resin composition for RTM was prepared by the same method as in Example 1 with the resin composition shown in Table 4, and the E 82 and E 23 , wet and dry Tg, water absorption, fracture toughness value, rubber state elastic modulus, η0, and mass reduction rate.
[0205] Since the epoxy resin composition did not contain the component [C] but contained low-molecular-weight glycidyl aniline instead, the mass reduction rate was 0.41 mass %, which was out of the range.
[0206] (Comparative Example 5)
[0207] An epoxy resin composition for RTM was prepared with the resin composition shown in Table 4 by the method described in Example 3 of Patent Document 4 (International Publication No. 2010 / 109929).
[0208] The epoxy resin composition was evaluated by the same method as in Example 1. 82 and E 23 , wet and dry Tg, water absorption, fracture toughness value, rubber state elastic modulus, η0, and mass reduction rate.
[0209] The epoxy resin composition did not contain the component [B] but contained 4,4′-diaminodiphenyl sulfone having high polarity instead. Therefore, η0 was 230 mPa·s, which was outside the range, and the water absorption of the cured resin was also 3.5%, which was outside the range.
[0210] (Comparative Example 6)
[0211] The epoxy resin composition for RTM was prepared by the same method as in Example 1 using the resin composition shown in Table 4, and the E 82 and E 23 , wet and dry Tg, water absorption, fracture toughness value, rubber state elastic modulus, η0, and mass reduction rate.
[0212] The epoxy resin composition does not contain component [A], but contains "jER (registered trademark)" 630 instead, so the elastic modulus in the rubber state is 10.0 MPa, which is out of range. The elastic modulus in wet heat and the heat resistance in wet state of the epoxy resin composition are low, and the water absorption rate is also as high as 2.7%. In addition, the fracture toughness value is 0.8 MPa·m 0.5 , is not sufficient.
[0213] (Comparative Example 7)
[0214] The epoxy resin composition for RTM was prepared by the same method as in Example 1 using the resin composition shown in Table 4, and the E 82 and E 23 , wet and dry Tg, water absorption, fracture toughness value, rubber state elastic modulus, η0, and mass reduction rate.
[0215] The epoxy resin composition does not contain component [C] but contains "EPICLON (registered trademark)" 830 instead, so the rubber state elastic modulus is 9.8 MPa, which is outside the range. The fracture toughness value is 0.8 MPa·m 0.5 In addition, the elastic modulus under wet heat was 2.40 GPa, which was insufficient.
[0216] [Table 1]
[0217]
[0218] [Table 2]
[0219]
[0220] [Table 3]
[0221]
[0222] [Table 4]
[0223]
[0224] In addition, the unit of each component in the table is part by mass.
[0225] The properties of the fiber-reinforced composite material of each example are as follows.
[0226] (Example 1')
[0227] Using the resin compositions shown in Table 5, fiber-reinforced composite materials were prepared according to the above-mentioned <Preparation of fiber-reinforced composite materials>.
[0228] Regarding the fiber-reinforced composite material, according to the above (8) Open hole compressive strength (23°C, 50%RH) of the fiber-reinforced composite material: OHC 23 Evaluation method and (9) Open hole compressive strength of fiber reinforced composite materials (wet heat 82°C): OHC 82 The open hole compressive strength was obtained by the evaluation method, and the results were OHC 23 316MPa,OHC 82 250MPa,OHC 82 / OHC 23 The post-impact compressive strength was 307 MPa, indicating excellent impact resistance.
[0229] (Examples 6', 12', 16', 18')
[0230] Except that the resin compositions were changed as shown in Table 5, fiber-reinforced composite materials were prepared and evaluated in the same manner as in Example 1.
[0231] The OHC of the fiber-reinforced composite material of each example was evaluated. 23 、OHC 82 , CAI, and the results showed excellent compression characteristics under wet heat and compression strength after impact at all levels.
[0232] (Comparative Example 1')
[0233] Except that the resin compositions were changed as shown in Table 5, fiber-reinforced composite materials were prepared and evaluated in the same manner as in Example 1.
[0234] Regarding this fiber-reinforced composite material, OHC 23 311MPa,OHC 82 200MPa,OHC 82 / OHC 23 It is as low as 0.64. In addition, the CAI is 269 MPa, and the impact resistance is also insufficient.
[0235] (Comparative Example 7')
[0236] Except that the resin compositions were changed as shown in Table 5, fiber-reinforced composite materials were prepared and evaluated in the same manner as in Example 1.
[0237] Regarding this fiber-reinforced composite material, OHC 23 The compressive strength at room temperature is low, and OHC 82 The CAI was 255 MPa, and the impact resistance was also insufficient.
[0238] [Table 5]
[0239]
[0240] Industrial Availability
[0241] The epoxy resin composition for RTM of the present invention can provide an epoxy resin cured product having low viscosity and low volatility and high elastic modulus and fracture toughness when wet and hot. The fiber-reinforced composite material formed from the epoxy resin composition is also excellent in compression characteristics and impact resistance when wet and hot, and is therefore suitable for use in aerospace components and general industrial structural components.
Claims
1. An epoxy resin composition for RTM, comprising the following components [A], [B], and [C], and satisfying all of the following conditions 1 to 4, [A] 4-functional glycidylamine type epoxy resin [B] At least one aromatic amine curing agent selected from alkylphenylenediamine and methylenedianiline [C] Aniline type epoxy resin represented by formula (I) In formula (I), R 1 and R 2 Each represents at least one selected from aliphatic hydrocarbon groups having 1 to 4 carbon atoms; R 1 and R 2 When there are plural of each, each may be the same or different; n is an integer of 0 to 4, m is an integer of 0 to 5; X represents -O- or -S-; Condition 1: Viscosity at 110°C is 1 mPa·s or more and 200 mPa·s or less Condition 2: Mass reduction after heating at 110°C for 30 minutes is 0.3 mass % or less Condition 3: The rubber elastic modulus of the cured resin obtained by curing at 180°C for 2 hours is 2 MPa or more and 8 MPa or less Condition 4: The water absorption of the cured resin obtained by curing at 180° C. for 2 hours is 1% or more and 3% or less. 2 . The epoxy resin composition for RTM according to claim 1 , comprising 10 parts by mass or more and 50 parts by mass or less of the component [C] based on 100 parts by mass of the total epoxy resin.
3. The epoxy resin composition for RTM according to claim 1 or 2, wherein The core-shell type rubber particles are contained as a component [D] in an amount of 1 part by mass or more and 10 parts by mass or less based on 100 parts by mass of the total epoxy resin.
4. The epoxy resin composition for RTM according to claim 1, comprising, as component [E], 10 parts by mass or more and 50 parts by mass or less of at least one solid epoxy resin selected from the group consisting of dicyclopentadiene epoxy resin, biphenyl epoxy resin, phenol aralkyl epoxy resin, and naphthalene epoxy resin, based on 100 parts by mass of the total epoxy resin. 5 . The epoxy resin composition for RTM according to claim 1 , comprising both alkylphenylenediamine and methylenedianiline as component [B]. 6 . The epoxy resin composition for RTM according to claim 1 , wherein component [B] is an alkylphenylenediamine. 7 . The epoxy resin composition for RTM according to claim 1 , comprising dimethylthiotoluenediamine as the alkylphenylenediamine. 8 . The epoxy resin composition for RTM according to claim 1 , comprising 4,4-methylenebis(isopropyl-6-methylaniline) as the methylenebisaniline.
9. The epoxy resin composition for RTM according to claim 1 or 4, wherein Mh / Me, a value obtained by dividing the total number of moles of active hydrogen contained in component [B] by the total number of moles of active groups contained in all epoxy resins, is 0.8 or more and 1.1 or less. 10 . A cured resin product obtained by thermally curing the epoxy resin composition for RTM according to claim 1 or 4 .
11. A fiber-reinforced composite material, comprising the cured resin according to claim 10 and a reinforcing fiber substrate. 12 . The fiber-reinforced composite material according to claim 11 , wherein the reinforcing fiber substrate is a carbon fiber substrate.
13. A method for producing a fiber-reinforced composite material, wherein: The epoxy resin composition for RTM according to claim 1 or 4 is injected into a reinforcing fiber base material placed in a molding die heated to 70° C. to 190° C. to impregnate the base material, and then cured in the molding die. 14 . The method for producing a fiber-reinforced composite material according to claim 13 , wherein the reinforcing fiber substrate is a carbon fiber substrate.