High-elasticity antibacterial fiber material and preparation method thereof

By adopting a highly elastic antibacterial fiber material with a multi-layer structure and using a combination of aramid fiber, carbon fiber and guanidinium salt/polyurethane fiber, the problem of low elastic modulus of existing antibacterial fiber materials is solved, achieving high elasticity and excellent antibacterial effect. Fiber material, suitable for a variety of application scenarios.

CN118756403AActive Publication Date: 2024-10-11FOSHAN CITY JINXINGMA FURNITURE MFG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411086825.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-11
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The elastic modulus of existing antibacterial fiber materials is low and cannot meet high demand, such as bandages and sportswear. At the same time, the cost of adding metal ions is high and is detrimental to the mechanical properties of synthetic fibers.

Method used

It adopts a multi-layer structure of highly elastic antibacterial fiber material. The first layer is composed of aramid fiber and carbon fiber, and the second layer is guanidinium salt/polyurethane fiber. The binding force is enhanced through electrostatic interaction and intermolecular hydrogen bonding, and the guanidinium salt is combined with Antibacterial properties, improve the mechanical properties and antibacterial effect of the fiber.

Benefits of technology

It achieves the excellent elastic modulus and antibacterial effect of high elastic fiber materials, reduces costs, and at the same time enhances the fiber's hygroscopicity and breathability, making it suitable for a variety of application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756403A_ABST
    Figure CN118756403A_ABST
Patent Text Reader

Abstract

The invention provides a high-elasticity antibacterial fiber material and a preparation method thereof.The high-elasticity antibacterial fiber material comprises a first layer and a second layer, the first layer comprises aramid fibers and carbon fibers, the second layer comprises guanidine salt / polyurethane fibers, and the content ratio of the carbon fibers to the aramid fibers in the first layer is 1: 1-3. By combining the first layer and the second layer, the high-elasticity antibacterial fiber material not only has excellent elastic modulus, but also has an excellent antibacterial effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fiber material manufacturing, and in particular relates to a high-elasticity antibacterial fiber material and a preparation method thereof. Background Art

[0002] In order to meet the hygiene and health needs in various applications, including medical and health, personal care, home environment, public health, industrial agriculture and other fields, related technologies use metal ions added to fibers to make fibers with antibacterial effects. The metal ions can be silver ions, copper ions, etc.

[0003] Fiber materials with added antimicrobial agents can inhibit the growth of bacteria and other microorganisms, but there are disadvantages. On the one hand, the cost of adding metal ions is high. On the other hand, for synthetic fibers such as polyester and nylon, silver ions interact with polymer chain segments, changing the mechanical properties of the fibers, resulting in increased fiber brittleness and reduced elastic modulus of the woven fiber materials, which cannot meet the needs of elastic fabrics such as bandages and sportswear. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a high-elastic antibacterial fiber material and a preparation method thereof, aiming to solve the problem of low elastic modulus of the antibacterial fiber material in a low-cost manner.

[0005] To solve the above technical problems, the present invention is implemented as follows: a high-elastic antibacterial fiber material, the high-elastic antibacterial fiber material includes a first layer and a second layer, the first layer includes the aramid fiber and the carbon fiber, the second layer includes guanidine salt / polyurethane fiber, and the content ratio of the carbon fiber to the aramid fiber in the first layer is 1:1~3.

[0006] In some embodiments of the present invention, the guanidine salt / polyurethane fiber comprises a polyurethane dispersion and a guanidine salt, wherein the guanidine salt comprises at least one of polyhexamethyleneguanidine hydrochloride, polyhexamethyleneguanidine stearate, polyhexamethyleneguanidine propionate, and polyhexamethyleneguanidine phosphate.

[0007] In some embodiments of the present invention, the first layer includes a plurality of first longitudes and first latitudes, the second layer includes a plurality of second longitudes and second latitudes, and the first intersection points of the first latitudes and first latitudes are staggered with the second intersection points of the second longitudes and second latitudes.

[0008] In some embodiments of the present invention, at least a third intersection point of each of the second longitude lines with a first latitude line is exposed on the outer surface of the first layer.

[0009] In some embodiments of the present invention, the fineness of the carbon fiber and the polyester fiber are both 1-1.5D, and the fineness of the guanidine salt / polyurethane fiber is 0.5-1.5D.

[0010] The present invention provides a preparation method for preparing the high elastic antibacterial fiber material as described above, the preparation method comprising the following steps: S1. preparing a polyurethane dispersion; S2, adding the guanidine salt solution and the polyurethane dispersion dropwise and mixing them simultaneously, and spinning the mixed solution into the guanidine salt / polyurethane fiber; S3, first weaving the guanidine salt / polyurethane fiber into a second layer, and then mixing and weaving the carbon fiber and the aramid fiber with the second layer to form a first layer, so as to prepare the high-elastic antibacterial fiber material.

[0011] In some embodiments of the present invention, step S1 comprises: S1.1, mixing a vegetable oil-based polyol, a crosslinking agent, and a hydrophilic chain extender, and heating the mixture for the first time to obtain a polyurethane prepolymer; S1.2, sequentially adding a catalyst and an organic solvent to the polyurethane prepolymer, stirring and mixing, heating for a second time, and then adding an alkaline neutralizer and continuing stirring to obtain a polyurethane emulsion, wherein, calculated by mass ratio, the catalyst: the alkaline neutralizer: the hydrophilic chain extender: the cross-linking agent: the vegetable oil-based polyol = 0.02~0.01: 0.5~1: 1: 2~4: 5~8; S1.3, heating the polyurethane emulsion for a third time to prepare the polyurethane dispersion.

[0012] In some embodiments of the present invention, the plant oil-based polyol includes at least one of castor oil-based polyol, soybean oil-based polyol, and palm oil-based polyol; The cross-linking agent includes at least one of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, and isophorone diisocyanate; The hydrophilic chain extender includes at least one of 2,2-dihydroxymethylbutyric acid, N-methyldiethanolamine, and trimethylolpropane; The catalyst comprises at least one of stannous octoate, triethylenediamine, dibutyltin dilaurate, and zinc acetylmethylisobutylketone; The alkaline neutralizing agent includes at least one of trimethylamine, triethylamine, and triisopropylamine; The organic solvent includes at least one of ethyl acetate, butanone, toluene and methyl isobutyl ketone.

[0013] In some embodiments of the present invention, the heating temperature of the first heating is 70-80°C, the heating temperature of the second heating is 25-30°C, and the heating temperature of the third heating is 90-110°C.

[0014] Compared with the prior art, the high elastic antibacterial fiber material and the preparation method thereof in the present invention have the following beneficial effects: The combination of aramid fiber and carbon fiber in the first layer provides high elasticity of the fiber material. Aramid fiber, due to its excellent toughness and strength, enables the fiber material to quickly recover to its original shape when stretched or compressed; carbon fiber, due to its high modulus and low density, further enhances the elasticity and deformation resistance of the fiber material.

[0015] The polyurethane in the second layer is used as a matrix, and guanidine salt is introduced as an antibacterial agent and reinforcing agent. With the help of electrostatic interactions and intermolecular hydrogen bonds between the components, the binding force between the matrix and the reinforcing agent is enhanced, so that the mechanical properties of the guanidine salt / polyurethane fiber are improved. The introduction of guanidine salt destroys the original "water-in-oil" structure of polyurethane, increases the hydrophilic part inside the fiber, enhances the hygroscopicity and air permeability of the fiber material, and combines the antibacterial properties of guanidine salt to prevent the reproduction and growth of bacteria on the fiber surface. By combining the first layer and the second layer, the high-elasticity antibacterial fiber material not only has an excellent elastic modulus, but also has an excellent antibacterial effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is a schematic structural diagram of a high elastic antibacterial fiber material in one embodiment of the present invention; Figure 2 It is a schematic flow chart of a method for preparing a highly elastic antibacterial fiber material in one embodiment of the present invention.

[0017] In the accompanying drawings, each reference numeral represents: 100, high elastic antibacterial fiber material; 11, first layer; 111, first warp; 112, first weft; 113, first intersection; 12, second layer; 121, second warp; 122, second weft; 123, second intersection; 13, third intersection. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0019] Please refer to Figure 1The present invention proposes a high-elastic antibacterial fiber material 100, which includes a first layer 11 and a second layer 12. The first layer 11 includes aramid fiber and carbon fiber, and the second layer 12 includes guanidine / polyurethane fiber. The content ratio of the carbon fiber and the aramid fiber in the first layer 11 is 1:1~3.

[0020] The combination of aramid fiber and carbon fiber in the first layer 11 provides high elasticity of the fiber material. Aramid fiber, due to its excellent toughness and strength, enables the fiber material to quickly recover to its original shape when stretched or compressed; carbon fiber, due to its high modulus and low density, further enhances the elasticity and deformation resistance of the fiber material.

[0021] The polyurethane in the second layer 12 is used as a matrix, and guanidine salt is introduced as an antibacterial agent and reinforcing agent. By means of the electrostatic interaction between the components and the intermolecular hydrogen bonds, the binding force between the matrix and the reinforcing agent is enhanced, so that the mechanical properties of the guanidine salt / polyurethane fiber are improved. The introduction of guanidine salt destroys the original "water-in-oil" structure of polyurethane, increases the hydrophilic part inside the fiber, enhances the hygroscopicity and air permeability of the fiber material, and combines the antibacterial properties of guanidine salt to prevent the reproduction and growth of bacteria on the fiber surface. By combining the first layer 11 and the second layer 12, the high elastic antibacterial fiber material 100 not only has excellent mechanical properties, but also has excellent antibacterial effects.

[0022] The guanidine salt / polyurethane fiber includes a polyurethane dispersion and a guanidine salt, wherein the guanidine salt includes at least one of polyhexamethylene guanidine hydrochloride, polyhexamethylene guanidine stearate, polyhexamethylene guanidine propionate, and polyhexamethylene guanidine phosphate. The mechanism of action of the guanidine salt is to bind to the bacterial cell wall, destroy the cell membrane structure, and cause the cell contents to leak, thereby killing the bacteria. The use of different types of polyhexamethylene guanidine salts, such as hydrochloride, stearate, propionate, and phosphate, can provide more effective antibacterial effects against different microorganisms, and enhance the breadth and durability of the antibacterial effect.

[0023] Moreover, the thermal conductivity along the cross-sectional direction of the carbon fiber is extremely low, and the heat that contacts the first layer 11 is difficult to transmit. The first layer 11 woven with carbon fiber has a strong thermal insulation performance, and the high-elastic antibacterial fiber material 100 can extend the thermal insulation effect.

[0024] Specifically, the first layer 11 includes a plurality of first longitudes 111 and first latitudes 112, the second layer 12 includes a plurality of second longitudes 121 and second latitudes 122, and the first intersection 113 of the first latitudes 112 and the second intersection 123 of the second longitudes 121 and the second latitudes 122 are staggered.

[0025] The intersections of the longitude and latitude in the first layer 11 and the second layer 12 are staggered to help disperse stress and strain. In this way, when subjected to external force, each part of the material can bear the load evenly, reduce stress concentration at a single intersection, and improve overall strength and toughness. The staggered intersection design can form more tiny pores, which helps to enhance the air permeability and moisture absorption of the material, making it more suitable for application scenarios that require good air permeability and comfort, such as sportswear and medical textiles.

[0026] Furthermore, the third intersection 13 of each second warp 121 and at least one first weft 112 is exposed on the outer surface of the first layer 11. The double-layer connection structure forms a stronger connection point by exposing the intersection of the second warp 121 and the first weft 112 on the outer surface, thereby enhancing the bonding force between the two layers of fabric and improving the overall strength and durability of the fabric. At the same time, the interweaving density of the surface fibers is increased to form a more complex mesh structure, so that the two layers of fabric can jointly withstand external forces when stretched and torn, disperse stress, avoid stress concentration at a certain point, and significantly improve the tear and tensile resistance of the fabric.

[0027] Moreover, the exposed second warp 121 contains antibacterial components, which can directly exert antibacterial effects when exposed on the outer surface, effectively inhibit the reproduction of bacteria on the surface of the material, improve the hygienic properties of the material, and are suitable for medical and health-related applications.

[0028] Specifically, the fineness of carbon fiber and polyester fiber is 1~1.5D, and the fineness of guanidine salt / polyurethane fiber is 0.5~1.5D. The smaller the fineness, the finer the fiber, and the finer the fiber can provide a larger surface area, so that the antibacterial component of guanidine salt can more effectively contact and inhibit microorganisms, and at the same time can closely combine with the antibacterial layer to improve the performance of the overall fiber material.

[0029] In one embodiment, guanidine salt / polyurethane fibers, carbon fibers and polyester fibers can be spunbonded, meltblown, spunlaced or air-laid to form a web. The fibers can then be aggregated into a web and then made into a non-woven fiber material through mechanical, thermal or chemical bonding methods, which can also effectively maintain the antibacterial properties of the fiber material.

[0030] Embodiment 1: Please refer to Figure 2 Embodiment 1 of the present invention provides a preparation method for preparing a high elastic antibacterial fiber material 100. The preparation method comprises the following steps: S1. preparing a polyurethane dispersion.

[0031] The specific steps of S1 are as follows: S1.1, 10 g of castor oil-based polyol, 8 g of isophorone diisocyanate, and 2 g of 2,2-dimethylolbutyric acid were mixed and heated for the first time to obtain a polyurethane prepolymer. The first heating temperature was 80°C, the mixing stirring rate was 200 rpm, and the heating stirring time was 10 min.

[0032] Castor oil-based polyol provides hydroxyl groups for the synthesis of polyurethane, and isophorone diisocyanate provides isocyanate groups. The hydroxyl groups react with the isocyanate groups to generate urethane bonds in the polyurethane chain. 2,2-Dihydroxymethylbutyric acid is used as a hydrophilic chain extender to introduce hydrophilic groups, making the polyurethane water-soluble or dispersible, which is beneficial for mixing with guanidine salts in subsequent reactions.

[0033] As the basic chain segment, polyurethane prepolymer provides the basic mechanical properties and structural characteristics of polyurethane materials, such as high strength and elasticity. At the same time, the prepolymer has a certain hydrophilicity and can react with the alkaline neutralizer in the subsequent reaction to further improve the water solubility or dispersibility of polyurethane, making it suitable for the preparation of waterborne polyurethane dispersions.

[0034] S1.2, dibutyltin dilaurate and butanone were added to the polyurethane prepolymer in sequence, stirred and mixed, heated for the second time, and then 1g of triethylamine was added and stirred to obtain a polyurethane emulsion. The amount of dibutyltin dilaurate was 0.15g, the stirring time was 2h, the heating temperature of the second heating was 25°C, and the stirring rate was 500rpm.

[0035] Dibutyltin dilaurate is used as a reaction catalyst. By coordinating to the isocyanate group, it reduces the activation energy of the reaction, accelerates the reaction between isocyanate and polyol and chain extender, improves the reaction rate and efficiency, and promotes the formation of urethane bonds. Butanone dissolves the polyurethane prepolymer to reduce its viscosity, ensures that the mixture is uniform, and facilitates the subsequent stirring and emulsification process. Triethylamine is used as a neutralizer to neutralize the carboxyl group in the prepolymer to form a salt, improve the hydrophilicity and dispersibility of the polyurethane, and make it easier to disperse in water to form a stable emulsion.

[0036] The addition of dibutyltin dilaurate and butanone to the polyurethane prepolymer is carried out at the heating temperature of the first heating. Dibutyltin dilaurate is added first to be fully mixed in the prepolymer to ensure that it can efficiently catalyze the reaction between isocyanate and hydroxyl. If butanone is added first, the concentration of the catalyst may be reduced, affecting the catalytic efficiency.

[0037] The heating temperature of the second heating is lower than that of the first heating because triethylamine is easily volatilized at a higher temperature. By cooling, the volatilization loss of triethylamine can be reduced, ensuring that a sufficient amount of triethylamine participates in the neutralization reaction, thereby improving the reaction efficiency and the quality of the product. By cooling, the occurrence of these side reactions can also be reduced or avoided, ensuring that the main reaction proceeds smoothly.

[0038] After adding triethylamine, the stirring speed is accelerated. High-speed stirring can generate strong shear force, help form finer polyurethane particles, improve the emulsification effect, make the final polyurethane emulsion more stable, and the particle distribution is more uniform. In addition, high-speed stirring helps to maintain the uniformity of the system, prevent phase separation caused by density differences or uneven reactions, and ensure the consistency of the quality and performance of the final product.

[0039] S1.3, heating the polyurethane emulsion for the third time to prepare a polyurethane dispersion. The third heating temperature is 90°C.

[0040] At higher temperatures, the incompletely reacted isocyanate groups and hydroxyl groups can continue to react, ensuring that the polyurethane reacts completely and forms a more complete polymer network structure. During the heating process, the viscosity of the system decreases, which helps the polyurethane particles to disperse more evenly in the water to form a stable dispersion. In addition, heating helps to volatilize the solvent, reduce the residual solvent content in the system, and obtain a purer polyurethane dispersion.

[0041] S2, the guanidine salt solution and the polyurethane dispersion are simultaneously added dropwise and mixed, and the mixed solution is blended into guanidine salt / polyurethane fibers. The guanidine salt solution is a polyhexamethylene guanidine hydrochloride solution with a concentration of 1 wt%, and the mass ratio of the guanidine salt solution to the polyurethane dispersion is 1:1.

[0042] Adding guanidine salt solution and polyurethane dispersion simultaneously can ensure that the two are evenly dispersed during the mixing process, forming a uniform composite fiber structure and avoiding phase separation. Simultaneous addition can control the reaction rate, avoid rapid reaction or coagulation caused by excessive local concentration, and contribute to a stable fiber forming process. Synchronous addition can better adjust the composition ratio of the composite material, optimize the mechanical properties and functional characteristics of the fiber, and improve the antibacterial performance, flexibility and durability.

[0043] A lower concentration helps to form small and evenly distributed guanidine salt particles, ensuring a smooth surface and uniform internal structure of the fiber, thus improving the overall quality of the fiber. A low concentration of guanidine salt can also prevent the fiber from becoming too hardened or brittle, maintaining good flexibility and ductility.

[0044] Guanidine / polyurethane fibers were made by electrospinning as follows: Mix the guanidine salt solution and polyurethane dispersion evenly, filter and degas, and then load them into the syringe. The syringe is connected to a high-voltage power supply, and the syringe needle is used as a nozzle. Set the appropriate voltage and flow rate. Turn on the power supply, and the mixed solution is stretched into fine fibers through a high-voltage field. The fibers are continuously stretched and solidified in the electric field and finally collected on the receiving plate. The selection of specific spinning equipment and processes needs to be determined based on the material properties and the final application requirements.

[0045] S3, first weave the guanidine salt / polyurethane fiber into the second layer 12, and then mix and weave the carbon fiber and aramid fiber with the second layer 12 to form the first layer 11, so as to prepare the high elastic antibacterial fiber material 100.

[0046] The high elastic antibacterial fiber material 100 is knitted using a composite knitting machine, and the operation steps are as follows: (1) Using a loom, weave the guanidine salt / polyurethane fiber into a fiber material to form a second layer 12. Select an appropriate weaving method (such as plain weave, twill or satin weave) to achieve the desired fiber material properties and performance. In Example 1, the second layer 12 is woven into a plain weave. Plain weave fabrics are woven by alternating warp and weft threads to form a simple interlaced structure. Each warp thread passes through each weft thread up and down in turn. Due to the high frequency of each warp thread and weft thread interlacing, the structure of the plain weave fabric is very compact and has good stability and tear resistance.

[0047] (2) Prepare the carbon fiber and aramid fiber separately and ensure that they have a length and uniformity suitable for weaving. Use a composite weaving machine to mix and weave the carbon fiber, aramid fiber and the woven second layer 12 to form the first layer 11.

[0048] The weaving process needs to ensure that all types of fibers are evenly distributed, and the second intersection 123 of the second warp 121 and the second weft 122 of the second layer 12 is staggered with the first weft 112 and the first intersection 113 of the first weft 112 of the first layer 11. It is also necessary to ensure that the third intersection 13 of each second warp 121 and at least one first weft 112 is exposed on the outer surface of the first layer 11, so as to achieve the expected mechanical properties and functional characteristics.

[0049] Embodiment 2: Embodiment 2 of the present invention provides a preparation method for preparing a high-elastic antibacterial fiber material 100. The preparation method comprises the following steps: S1. preparing a polyurethane dispersion.

[0050] The specific steps of S1 are as follows: S1.1, 5g soybean oil-based polyol, 4g toluene diisocyanate, and 1.4g N-methyldiethanolamine were mixed and heated for the first time to obtain a polyurethane prepolymer. The first heating temperature was 70°C, the mixing stirring rate was 250rpm, and the heating stirring time was 10min.

[0051] S1.2, add stannous octoate and ethyl acetate to the polyurethane prepolymer in sequence, stir and mix, heat for the second time, add 0.7g trimethylamine and continue stirring to obtain a polyurethane emulsion. The amount of stannous octoate is 0.1g, the stirring time is 2h, the heating temperature of the second heating is 30°C, and the stirring rate is 500rpm.

[0052] S1.3, heating the polyurethane emulsion for the third time to prepare a polyurethane dispersion. The third heating temperature is 80°C.

[0053] S2, the guanidine salt solution and the polyurethane dispersion are simultaneously added dropwise and mixed, and the mixed solution is blended into guanidine salt / polyurethane fibers. The guanidine salt solution is a 0.5 wt% polyhexamethylene guanidine stearate solution, and the mass ratio of the guanidine salt solution to the polyurethane dispersion is 2:1.

[0054] S3, first weave the guanidine salt / polyurethane fiber into the second layer 12, and then mix the carbon fiber and aramid fiber with the second layer 12 to form the first layer 11 to make a highly elastic antibacterial fiber material 100. In Example 2, the second layer 12 is woven into a satin weave. Due to the smooth surface, water droplets roll off easily and are not easy to penetrate. Satin fabric has a certain natural waterproof effect, and the weaving structure of satin fabric allows the warp or weft to form continuous floating lines on the fabric surface, making the surface smoother and more skin-friendly.

[0055] Embodiment 3: Embodiment 3 of the present invention provides a preparation method for preparing a high-elastic antibacterial fiber material 100. The preparation method comprises the following steps: S1. preparing a polyurethane dispersion.

[0056] The specific steps of S1 are as follows: S1.1, 7.5 g palm oil-based polyol, 6 g diphenylmethane diisocyanate, and 1 g trimethylolpropane were mixed and heated for the first time to obtain a polyurethane prepolymer. The first heating temperature was 75° C., the mixing stirring rate was 250 rpm, and the heating stirring time was 10 min.

[0057] S1.2, triethylenediamine and toluene are added to the polyurethane prepolymer in sequence, stirred and mixed, and heated for the second time, and then 0.5 g of triisopropylamine is added and stirred continuously to obtain a polyurethane emulsion. The amount of triethylenediamine is 0.1 g, the stirring time is 2 h, the heating temperature of the second heating is 30°C, and the stirring rate is 500 rpm.

[0058] S1.3, heating the polyurethane emulsion for the third time to prepare a polyurethane dispersion. The third heating temperature is 110°C.

[0059] S2, the guanidine salt solution and the polyurethane dispersion are simultaneously added dropwise and mixed, and the mixed solution is blended into guanidine salt / polyurethane fibers. The guanidine salt solution is a polyhexamethylene guanidine propionate solution with a concentration of 1.5wt%, and the mass ratio of the guanidine salt solution to the polyurethane dispersion is 1:2.

[0060] S3, first weave the guanidine salt / polyurethane fiber into the second layer 12, then mix and weave the carbon fiber and aramid fiber with the second layer 12 to form the first layer 11, so as to make the high elastic antibacterial fiber material 100. In Example 3, the second layer 12 is woven into twill.

[0061] The twill weaving structure has good wrinkle resistance, and clothes and fabrics are not prone to permanent wrinkles during use. The surface of twill fabric has obvious diagonal texture, which is not only beautiful, but also has a certain three-dimensional sense visually, increasing the texture of the fabric.

[0062] Comparative Example 1: The difference from Example 1 is that the prepared high elastic antibacterial fiber material 100 is a single-layer structure.

[0063] Comparative Example 2 is different from Example 1 in that the ratio of carbon fiber to aramid fiber in the high elastic antibacterial fiber material 100 is 3:1.

[0064] Comparative Example 3: The difference from Example 1 is that the second layer 12 of the high elastic antibacterial fiber material 100 is polyurethane fiber.

[0065] Experiment 1: Tensile test.

[0066] Cut three rectangular specimens of different specifications from each high elastic antibacterial fiber material 100 of Examples 1-3 and Comparative Examples 1-3, and record the initial length and width of each specimen. Fix the specimen on the fixture of the tensile testing machine, and ensure that the specimen is perpendicular to the fixture and not loose. Set the parameters of the tensile testing machine, including the tensile speed and the termination condition, start the tensile testing machine, record the relationship curve between stress (tension) and strain (elongation), and calculate the slope of the stress-strain curve, i.e., the elastic modulus, within the elastic range. The experimental data are shown in Table 1.

[0067] Table 1: The elastic modulus of comparative example 1 is significantly lower than that of example 1, indicating that the single-layer structure affects the elastic modulus. The elastic modulus of comparative example 2 is lower than that of example 1, indicating that although increasing the carbon fiber ratio (3:1) increases the strength, the elastic modulus decreases.

[0068] Experiment 2: Antibacterial and anti-mite experiment.

[0069] Small pieces of uniform size (eg, circular pieces with a diameter of 1 cm) were cut from the high elastic antibacterial fiber material 100 of Example 1 and Comparative Example 3 for experiments.

[0070] (1) Antibacterial test: Escherichia coli and Staphylococcus aureus were inoculated on LB agar medium and cultured for 24 hours until colonies were formed. The fiber material sample was placed on the culture medium inoculated with bacteria to ensure that the fiber material sample was in full contact with the bacteria and cultured in a 37°C incubator for 24 hours. The culture dish was taken out, and the diameter of the inhibition zone (the area of ​​sterile growth) around each fiber material sample was observed and recorded. The bacterial growth on the surface of the fiber material was further observed under a microscope, and the bacterial density was recorded. The experimental data are shown in Table 2.

[0071] Table 2: Guanidine salt is a broad-spectrum antibacterial agent that can destroy the cell membranes of bacteria and fungi, thereby inhibiting or killing these microorganisms. Therefore, the diameter of the inhibition zone of Example 1 with the addition of guanidine salt is much larger than that of Comparative Example 3 without the addition of guanidine salt.

[0072] (2) Anti-mite experiment: Cultivate dust mites on the mite culture medium, ensure that the culture medium is suitable for the growth of mites (temperature 25°C, humidity 70%), and record the initial number and activity of mites. Place the fiber material sample together with the cultured mites in a culture dish, ensure that the fiber material sample is covered with mites, and culture for 7 days under constant temperature and humidity conditions. Take out the fiber material sample, observe the number and activity of mites on the surface of the fiber material under a microscope, and record the number and mortality of mites on each fiber material sample. The experimental data are shown in Table 3.

[0073] Table 3: The living environment of mites often breeds a large number of bacteria and fungi, and the antibacterial effect of guanidine salts can indirectly reduce the living environment of mites. Guanidine salts have the potential to indirectly reduce the living environment of mites through their broad-spectrum antibacterial effect, thereby playing an anti-mite effect. Therefore, the mite mortality rate of Example 1 containing guanidine salts is significantly higher than that of Comparative Example 3.

[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A highly elastic antibacterial fiber material, characterized in that: The high-elastic antibacterial fiber material includes a first layer and a second layer, the first layer includes the aramid fiber and the carbon fiber, the second layer includes guanidine salt / polyurethane fiber, and the content ratio of the carbon fiber to the aramid fiber in the first layer is 1:1-3.

2. The high elastic antibacterial fiber material according to claim 1, characterized in that: The guanidine salt / polyurethane fiber comprises a polyurethane dispersion and a guanidine salt, wherein the guanidine salt comprises at least one of polyhexamethyleneguanidine hydrochloride, polyhexamethyleneguanidine stearate, polyhexamethyleneguanidine propionate and polyhexamethyleneguanidine phosphate.

3. The high elastic antibacterial fiber material according to claim 1, characterized in that: The first layer includes a plurality of first warps and first wefts, the second layer includes a plurality of second warps and second wefts, and a first intersection point of the first wefts and first wefts is staggered with a second intersection point of the second warps and second wefts.

4. The high elastic antibacterial fiber material according to claim 3, characterized in that: The third intersection point of each of the second longitude lines with at least one of the first latitude lines is exposed on the outer surface of the first layer.

5. The high elastic antibacterial fiber material according to claim 1, characterized in that: The fineness of the carbon fiber and the polyester fiber are both 1-1.5D, and the fineness of the guanidine salt / polyurethane fiber is 0.5-1.5D.

6. A preparation method, characterized in that: For preparing the high elastic antibacterial fiber material according to any one of claims 1 to 5, the preparation method comprises the following steps: S1. preparing a polyurethane dispersion; S2, adding the guanidine salt solution and the polyurethane dispersion dropwise and mixing them simultaneously, and spinning the mixed solution into the guanidine salt / polyurethane fiber; S3, first weaving the guanidine salt / polyurethane fiber into a second layer, and then mixing and weaving the carbon fiber and the aramid fiber with the second layer to form a first layer, so as to prepare the high-elastic antibacterial fiber material.

7. The preparation method according to claim 6, characterized in that: The step S1 comprises: S1.1, mixing a vegetable oil-based polyol, a crosslinking agent, and a hydrophilic chain extender, and heating the mixture for the first time to obtain a polyurethane prepolymer; S1.2, sequentially adding a catalyst and an organic solvent to the polyurethane prepolymer, stirring and mixing, heating for a second time, and then adding an alkaline neutralizer and continuing stirring to obtain a polyurethane emulsion, wherein, calculated by mass ratio, the catalyst: the alkaline neutralizer: the hydrophilic chain extender: the cross-linking agent: the vegetable oil-based polyol = 0.02~0.01: 0.5~1: 1: 2~4: 5~8; S1.3, heating the polyurethane emulsion for a third time to prepare the polyurethane dispersion.

8. The preparation method according to claim 7, characterized in that: The vegetable oil-based polyol includes at least one of castor oil-based polyol, soybean oil-based polyol, and palm oil-based polyol; The cross-linking agent includes at least one of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, and isophorone diisocyanate; The hydrophilic chain extender includes at least one of 2,2-dihydroxymethylbutyric acid, N-methyldiethanolamine, and trimethylolpropane; The catalyst comprises at least one of stannous octoate, triethylenediamine, dibutyltin dilaurate, and zinc acetylmethylisobutylketone; The alkaline neutralizing agent includes at least one of trimethylamine, triethylamine, and triisopropylamine; The organic solvent includes at least one of ethyl acetate, butanone, toluene and methyl isobutyl ketone.

9. The preparation method according to claim 7, characterized in that: The heating temperature of the first heating is 70-80°C, the heating temperature of the second heating is 25-30°C, and the heating temperature of the third heating is 90-110°C.

Citation Information

Patent Citations

  • Dual-layer fabric

    CN102330243A

  • Double-woven fabric with antibacterial property

    CN104018266A

  • Carbon dioxide-based polyurethane antibacterial fiber and preparation method thereof

    CN111394826A

  • Moisture-conducting quick-drying breathable fabric based on vortex spinning covering yarns

    CN111791562A

  • Single-sided wear-resistant striped fabric

    CN209568192U