Medical polyimide catheter as well as preparation method and application thereof
By introducing a high-adhesion thermoplastic polyimide transition layer into medical polyimide catheters, the problem of poor adhesion between the thermosetting base material layer and the reinforcement layer is solved, and the catheter's high strength, distortion resistance and safety are achieved. , suitable for minimally invasive surgeries in high-end medical fields.
Patent Information
- Application Number
- CN202410888965.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-29
AI Technical Summary
Existing medical polyimide catheters are difficult to meet the requirements for high strength, distortion resistance and reliability in the high-end medical field. In particular, the poor adhesion between the thermosetting base material layer and the reinforcement layer causes inter-layer separation problems, which affects its use in the field. Safety and reliability in minimally invasive surgery.
It adopts a multi-layer structure design, introduces high-adhesion thermoplastic polyimide as the transition layer, combines the thermosetting polyimide base material layer, reinforcement layer and lubricating layer, and controls the thickness and interface strength of each layer through solution coating to form One-piece construction to improve adhesion and stress transition capabilities.
It achieves high strength, anti-torsion, smoothness and pushability of the catheter, improves surgical results, enhances patient safety, and provides higher flexibility, safety and reliability in minimally invasive surgeries.
Smart Images

Figure CN118846246A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of medical devices, and in particular to a medical polyimide catheter and a preparation method and application thereof. Background Art
[0002] Medical catheters are made of polymer materials that meet medical standards and are used as medical device catheters for insertion into the human body or outside the body during disease diagnosis or treatment. They can effectively reduce patients' traumatic bleeding, surgical pain, and quick recovery in minimally invasive surgical procedures such as cardiovascular interventional therapy, gastrointestinal interventional therapy, and endoscopy. As a result, they have been widely used, further prompting an increase in the demand for fine and precise medical catheters, especially in high-end fields such as high-performance medical polyimide catheters, which are already in short supply. However, the quality of medical catheters in the existing technology cannot meet the needs of medical technology development.
[0003] Polyimide materials are the preferred materials for ultra-fine and high-precision medical catheters, mainly because they have good biocompatibility and can pass ISO10993-5, 10 standard testing, as well as excellent chemical resistance, radiation resistance, excellent stress strength, torque transmission, bending toughness, etc., which can better meet the requirements of long-distance medical operations in the body. In the existing technology, there are two main routes for the preparation of polyimide tubes. The most widely used technology generally adopts the melt extrusion method, such as Figure 1 As shown, the polyimide resin is usually directly extruded into shape by a screw extruder in a molten state. The equipment and process of this route are relatively mature, with advantages such as high production efficiency, relatively easy control of the inner and outer diameter tolerances of the catheter, and the apparent quality. However, in order to ensure that the polyimide resin can melt at high temperature, there are a large number of flexible units in the structure, resulting in low strength and anti-kink performance. In addition, because it is a pure resin body molding, the extruded tube wall cannot be ultra-thin. It is currently mainly used in insulating sleeves and optical fiber protective layers, and cannot meet the requirements of high-precision minimally invasive treatment. Another technical route is the solution coating molding method. Its biggest advantage is the diversified structural selection, such as non-melting and insoluble structures. High-strength anti-twisting catheters can be prepared. With the help of solvent evaporation and film thinning, ultra-thin catheters with a wall less than 6um can be prepared. However, it involves the dual processes of stable drying and high-temperature curing of the catheter film. The comprehensive performance, tube diameter, wall thickness, especially the outer diameter of the catheter and the apparent quality of the outer surface are difficult to control.
[0004] Based on the above problems, polyimide catheters can also use more complex solution coating molding technology routes, and multiple functional layers are added to the substrate of the single-layer polyimide catheter to prepare functional composite catheters with higher performance and wider applications. For example, adding a layer of polytetrafluoroethylene on the outer surface of the catheter can reduce the friction coefficient of the catheter surface from 0.50 of polyimide to 0.20-0.30 of polytetrafluoroethylene, which can greatly improve the lubricity of the catheter in the body and reduce friction pain during minimally invasive surgery. Typical multi-layer composite catheter products in the prior art, such as Reinforced PolyimideTubing,Nordson Braid-Reinforced Tubing usually adopts a three-layer structure design. Figure 2 As shown, from the inside to the outside, it includes a base layer 1, a reinforcement layer 2 and a lubricating layer 5, wherein the inner base layer is a high-strength and high-model polyimide material, which serves as the "backbone" and pinhole-free substrate of the catheter structure, and can withstand air pressure or fluid pressure; the middle reinforcement layer 2 can be customized according to specific needs, and stainless steel or nickel-titanium alloy can be used to increase pushability, and high braiding density can enhance flexibility and anti-kink ability; the lubricating layer 5 of the surface polytetrafluoroethylene can improve the smoothness of the catheter surface, while pressing the braided layer and being used to "carry" the metal wire braided layer, so that it can stretch or shrink as the tube bends. However, in order to ensure its high strength, high modulus and anti-twisting properties, the inner base material layer adopts a thermosetting, infusible and insoluble rigid molecular structure. The polymer condensed state is densely stacked and has a smooth surface, which results in poor adhesion to the braided reinforcement layer. Especially under bending and torsional stress, interlayer separation and other phenomena are prone to occur. The gaps in the braided fabric of the braided reinforcement layer also need to be filled with polyimide resin, and there are a large number of interfaces between the two materials, which will greatly reduce the reliability and safety of the catheter and even cause surgical accidents.
[0005] In the prior art, fillers or polymers are blended and modified for polyimide single-layer catheters. For example, patents CN114452446A and CN114075385A improve the strength and anti-kink performance of the catheter by adding inorganic compounds (such as silica) or polymers for physical mixing. However, the problem of interface adhesion cannot be solved.
[0006] Based on the problems existing in the prior art, a reinforced medical polyimide catheter and its preparation method and application are developed. By introducing a layer of high-adhesion thermoplastic polyimide into the catheter structure, which serves as the adhesion and stress transition layer between the thermosetting polyimide substrate layer and the reinforced braided layer, the delamination problem of the multi-layer interface can be effectively solved, and the reliability and safety of the multi-layer polyimide medical catheter can be improved. Summary of the invention
[0007] In view of the technical problems existing in the prior art, the present invention discloses a polyimide compound, a medical polyimide catheter, and a preparation method and application thereof. The provided medical polyimide catheter has excellent comprehensive properties such as ultra-thinness, high strength, anti-twisting, solvent resistance, wear resistance, and water resistance, and meets the requirements of the prior art for high-end medical polyimide catheters.
[0008] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a medical polyimide catheter, which is a multi-layer structure, and is composed of a first substrate layer, a reinforcement layer, an adhesion layer, a second substrate layer and a lubricating layer from the inside to the outside; the adhesion layer fuses the first substrate layer, the reinforcement layer, the second substrate layer and the lubricating layer to form an integrated structure.
[0009] Preferably, the first substrate layer and the second substrate layer are both thermosetting polyimide compounds;
[0010] Preferably, the adhesive layer is a thermoplastic polyimide compound;
[0011] Preferably, the reinforcement layer is made of stainless steel, nickel-titanium alloy, Liquid crystal polymer fibers, One or more synthetic fibers;
[0012] Preferably, the lubricating layer is tetrafluoroethylene (PTFE), fluorinated ethylene propylene copolymer (FEP), soluble polytetrafluoroethylene (PFA), polyvinylidene fluoride (PVDF), polyphenylene sulfone Nylon 11 Nylon 12 Polyurethane Polyetheramide One or more combinations of .
[0013] Preferably, the material of the reinforcement layer is a braided tube made of linear material.
[0014] Preferably, the braided tube comprises a braided mesh or a coil wire; the braided mesh has a cross-in-inch (PIC) of 10 to 200;
[0015] Preferably, the number of windings per inch (WPI) of the coil wire is 20-180.
[0016] Preferably, the linear material is a flat or round linear material.
[0017] More preferably, the cross-sectional thickness*width dimension of the flat linear material is 0.006mm*0.032mm-0.05mm*0.25mm, and the cross-sectional diameter of the circular linear material is 0.012mm-0.1mm.
[0018] Preferably, the thermosetting polyimide compound is prepared by a first dianhydride monomer compound and a first diamine monomer compound through a condensation reaction, wherein the dianhydride monomer compound is selected from phthalic anhydride, pyrazine tetracarboxylic anhydride, cyclobutane dianhydride, 1,4,5,8-naphthalene tetracarboxylic anhydride, 4,4′-biphenyl dianhydride, 2,3,6,7-anthracene tetracarboxylic anhydride, dibenzodioxane hexacyclic dianhydride, 4,4′-terphenyl dianhydride, 3,4,9,10-pyrene tetracarboxylic anhydride, tetraphenyl diether dianhydride, 9,9-bis[4-(3,4-dicarboxylic acid phenoxy)phenyl]fluorene dianhydride The diamine monomer compound is selected from one or more combinations of p-phenylenediamine, 2,6-diaminopyridine, 1,4-benzidine, 4,4′-diamino-2,2′-dimethylbiphenyl, 2-amino-5(4-aminophenyl)-pyrimidine, 2,5-di(4-aminophenyl)pyridine, 4,4′-diaminodiphenylmethane, 4,4′-diaminodiphenyl ether, 5-amino-2-(3′-aminophenyl)benzimidazole, 3,3′-dihydroxybiphenyl diamine, and 4,4′-diamino-tetramethyl-p-terphenyl.
[0019] Preferably, the thermoplastic polyimide compound is prepared by a second dianhydride compound and a second diamine compound through a condensation reaction, wherein the second dianhydride compound is selected from 4,4′-diphenyl ether dianhydride, 4,4′-dibenzophenone tetracarboxylic dianhydride, di-trimellitate anhydride hydroquinone ester, 4,4′-(3,4-dicarboxyphenoxy)benzophenone dianhydride, 4,4′-diphenyl sulfide dianhydride, 4,4′-diphenyl sulfone dianhydride, 4,4′-diphenyl ether dianhydride and 4,4′-bisphenol A diether dianhydride The second diamine monomer is one or more of 4,4'-diaminodiphenyl ether, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,2'-bis[4-(4-aminophenoxy)phenyl]propane, 3,4'-diaminodiphenyl ether, 2,7-bis(4-aminophenoxy)naphthalene, 4,4'-bis(3-aminophenoxy)biphenyl and 4,4'-bis(3-aminophenoxy)benzophenone.
[0020] Preferably, the inner diameter of the polyimide catheter is 10-1000 μm.
[0021] Preferably, the lubricating layer has a thickness of 0.5 to 20 μm.
[0022] As another object, the present invention also provides a method for preparing the above-mentioned polyimide catheter, using polyimide materials as the first substrate layer and the second substrate layer with a supporting function, and the bonding layer with an adhesion function, a braid or a coil as a reinforcing layer, and a fluoroplastic or polyetheramide thermoplastic material as a lubricating layer, and controlling the thickness and interface strength of each layer layer by layer through solution coating, thereby preparing the polyimide catheter.
[0023] Preferably, the preparation method comprises adopting a multi-stage dip-forming process to sequentially form a substrate layer-reinforcement layer-adhesion layer-lubricating layer on the surface of the tube core; specifically comprising the following steps:
[0024] S1. Preparation of the first substrate layer; first, a thermosetting polyamic acid precursor solution is dip-coated on the surface of the tube core, and a uniform film is formed on the surface of the tube core after a first pre-drying and qualitative analysis, which is the substrate layer;
[0025] S2. Preparation of a reinforcing layer and an adhesive layer; nesting the braided tube on the surface of the substrate layer to form a reinforcing layer; immersing the tube core attached with the reinforcing layer in a thermoplastic polyamic acid precursor solution, filling the thermoplastic polyamic acid precursor solution into the gap of the braided tube, and performing a second pre-drying qualitatively to form an adhesive layer on the surface of the reinforcing layer;
[0026] S3. Preparation of a second substrate layer; immersing the die having the adhesive layer attached thereto in the thermosetting polyamic acid precursor solution, performing a high temperature curing treatment, and completely drying the second substrate layer and the adhesive layer;
[0027] S4. Preparation of polyimide catheter; finally, the tube core after drying is placed in the lubricant solution, a lubricating layer is coated on the surface of the adhesion layer, and after a third pre-drying and qualitative determination, high-temperature drying is performed again, and the lubricant softens to form a dense and smooth surface structure, thus obtaining the polyimide catheter.
[0028] Preferably, the solvent used in the preparation of the thermosetting polyamic acid precursor solution and the thermoplastic polyamic acid precursor solution is a polar aprotic solvent; preferably, the solvent includes formamide, acetamide, sulfoxide, pyrrolidone; phenolic solvent, tetrahydrofuran (THF), dioxane, dichloromethane, chloroform, hexamethylphosphorus triamide, γ-butyrolactone, cyclopentanone, one or more combinations thereof; the solid content of the thermosetting polyamic acid precursor solution and the thermoplastic polyamic acid precursor solution is 6-50wt%, preferably 8-40wt%, more preferably 10-30wt%; the viscosity is 1-100000cP, preferably 10-10000cP, more preferably 1000-8000cP;
[0029] Preferably, the tube core is sequentially transferred to the thermosetting polyamic acid precursor solution and the thermoplastic polyamic acid precursor solution, and the transfer speed is 0.1 to 50 m / min, preferably 0.5 to 30 m / min;
[0030] Preferably, the thickness of the first substrate layer and the second substrate layer is 0.5 to 10 μm, preferably 1 to 7 μm, and more preferably 2 to 4 μm;
[0031] Preferably, the temperature of the first pre-drying and the second pre-drying is 80-200°C, preferably 100-180°C, more preferably 120-160°C.
[0032] Preferably, the high temperature curing treatment includes drying and imidizing the first substrate layer, the second substrate layer and the adhesive layer using a multi-stage high temperature heating process;
[0033] Preferably, the process conditions of the high temperature curing treatment include first heating up in stages and then annealing;
[0034] Preferably, the range of the staged heating is 200-700°C, and the heat treatment time of each stage is 1-100 min; the temperature range of the annealing is 150-500°C, and the annealing time is 1-100 min;
[0035] Preferably, the staged heating includes heat treatment at 300°C, 360°C, 420°C and 480°C for 3 min respectively; the annealing includes annealing at 400°C, 300°C and 200°C for 3 min respectively;
[0036] Preferably, the high temperature treatment temperature ranges from 200 to 700° C., more preferably from 250 to 600° C., and the treatment time is preferably from 1 to 100 min, more preferably from 2 to 40 min.
[0037] The reinforced medical polyimide catheter provided by the present invention can effectively solve the problem of interlayer separation of multi-layer functional catheters, making them more flexible and safer and more reliable in minimally invasive surgery. Based on the above technical solution, the role and process conditions of each layer structure are analyzed as follows;
[0038] (1) For polyimide substrates, this layer needs to meet the requirements of high strength, high modulus, anti-distortion, wear resistance, gas or liquid penetration resistance, and air pressure or hydraulic expansion resistance; in addition, it needs to be adjustable in thickness, especially ultra-thin tube walls. In order to meet the above requirements, rigid dianhydride and diamine monomers are selected from the molecular structure design, such as pyromellitic anhydride (PMDA), 4,4'-biphenyltetracarboxylic anhydride (4,4'-BPDA), p-phenylenediamine (PDA), etc., so that even ultra-thin catheters have extremely high specific strength and anti-distortion properties. At the same time, the advantages of a small amount of multiple solution coating process and the thinning of the film by the volatilization of the glue liquid are used to prepare a catheter with controllable wall thickness and adjustable thickness.
[0039] (2) For the reinforcement layer, the layer needs to meet the requirements of high column stiffness, anti-circumferential compression, anti-kink, etc., and can be customized according to special functional requirements. The metal used in the present invention or the weavable organic fiber is selected as the reinforcement material, especially the fiber material suitable for weaving low density. The shape is selected as a woven mesh or a coil wire. At the same time, the woven mesh selects a full-load or half-load weaving pattern and adjusts the performance by selecting the number of crosses per inch (PIC). For example, a higher PIC can improve flexibility, while a lower PIC can increase longitudinal stiffness. The coil is selected to be wound clockwise or counterclockwise and the rigidity-flexibility ratio is adjusted by the number of windings per inch (WPI).
[0040] (3) For the top lubricating layer, the layer needs to meet the requirements of low friction coefficient, good biological compatibility, resistance to chemical solvents, low hardness, good hot melt and adhesion, etc. The present invention uses a fusible thermoplastic polymer as the lubricating layer material, such as polytetrafluoroethylene (PTFE), fluorinated ethylene propylene copolymer (FEP), nylon, polyether amide Polyurethane, etc., is formed by coating with a solution or emulsion, then dried to remove the solvent, and finally heat-baked near the melting point to form a dense and smooth surface.
[0041] (4) In order to solve the problem of low adhesion and easy delamination between the polyimide substrate layer and the metal reinforcement layer, the present invention introduces a high-adhesion thermoplastic polyimide as a bonding transition layer and a stress buffer layer between the two. The high-adhesion thermoplastic polyimide is immersed in the woven structure of the reinforcement layer, which has good compatibility with the substrate layer (thermosetting polyimide), thereby solving the interface problem between the layers. Furthermore, the present application adopts a solution coating method to control the thickness of the solution, and utilizes the advantages of fast solution infiltration and good diffusion to make the substrate layer and the reinforcement layer have a strong interface bonding force, thereby solving the interface delamination problem in the prior art.
[0042] In the present invention, the forming core wire used for the polyimide substrate layer is made of a material that can withstand high temperature treatment, such as metal stainless steel wire, silver wire, copper wire, silver-plated copper wire, or non-metal glass rod, quartz rod, etc., and in order to smoothly separate the tube core from the catheter, the core wire is pre-coated with fluorine material or other lubricants. According to the inner diameter requirement of the catheter, the diameter of the tube core is 10-20000um.
[0043] In the present invention, the method for synthesizing the polyimide resin of the substrate layer and the adhesive layer will fully consider the effects of reaction concentration, addition order, reaction temperature and time, stirring method and rate, mass transfer and heat transfer process in the kettle, viscosity control method, etc. on resin polymerization, use mass spectrometry and liquid chromatography to detect the molecular weight and distribution of the resin, and systematically establish the relationship between the influence of different reaction scales on the molecular weight size and distribution and comprehensive performance, and optimize the most suitable process conditions to achieve uniform and stable resin performance and batches.
[0044] In the present invention, the external factors of the polymerization reaction of the polyimide resin are strictly controlled, the reaction device is installed in a class 1,000 constant temperature and humidity clean room, the reactor adopts a jacket heat transfer method, and a high-power integrated cooling and heating machine is used for rapid and accurate temperature control, the reaction solvent is transported by a precise metering pump that is water-proof and oxygen-proof, and the resin after the reaction is precisely filtered by a filter element with a pore size of 1-2um to reduce the impact of the external environment.
[0045] In the present invention, the polyimide substrate layer is prepared by a solution coating molding method, the tube core is passed through a polyimide glue tank, a scraping die and a pre-drying tunnel, and the thickness of the substrate layer is controlled by adjusting the viscosity and solid content of the polyimide resin, the running speed of the tube core and the size of the die diameter.
[0046] In the present invention, the drying and curing of the polyimide solution after coating adopts a multi-stage programmed temperature-controlled heat treatment method. If the solvent evaporates too slowly, the molecular chain will be severely broken during the heating process, resulting in low elongation and poor flexibility. If it evaporates too quickly, the plasticizing effect of the residual solvent will be lacking, resulting in a decrease in the mobility of the molecular chain, insufficient imidization, and easy generation of membrane surface bubbles. By optimizing the heat treatment process, excellent catheter substrate layer performance and surface quality can be achieved.
[0047] In the present invention, the preparation of the high adhesion transition layer, the schematic diagram of the catheter is as follows Figure 3 As shown, first, the polyimide substrate layer containing the tube core is immersed in a thermoplastic polyimide solution and then dried to form a surface adhesive layer, and the thickness of the adhesive layer is regulated by the viscosity, solid content and number of dipping times of the adhesive solution; then the reinforcement is nested on the polyimide substrate layer with the tube core, and then they pass through the thermoplastic polyimide solution glue tank and pre-drying channel together for multiple times until the reinforcement is completely buried in the adhesive thermoplastic polyimide resin, and then the tube core passes through the thermosetting polyimide resin solution glue tank and pre-drying channel, and finally it is subjected to multi-gradient high-temperature imidization to form a dense tube wall, wherein the thermoplastic transition layer between the thermosetting polyimide substrate layer and the reinforcement can play a role of high adhesion and buffering stress to prevent delamination.
[0048] In the present invention, the high temperature cured polyimide conduit is passed through polytetrafluoroethylene (PTFE) or polyetheramide The dilute solution is then dried in a hot drying tunnel, and the target thickness is achieved by adjusting the solid content, viscosity and number of coatings of the solution. Finally, the surface lubricating layer is heated to near the melting point for heat treatment to make it dense and smooth.
[0049] In the present invention, the prepared polyimide catheter is first cut into specific lengths according to market user requirements, and then the catheter and the tube core are separated to finally obtain a multi-layer functional composite catheter.
[0050] The technical effects of the technical solution of the present invention are as follows:
[0051] 1. By adopting the technical solution of the present invention, the present invention adopts a catheter with a multi-layer structure design, functionally combines a polyimide substrate layer, a reinforcement layer and a lubricating layer, and introduces a high-adhesion polyimide as a transition layer to effectively solve the problem of interlayer separation, so that it has excellent flexibility, kink resistance, smoothness and pushability, as well as high burst pressure, circumferential strength and column strength, thereby improving surgical results in minimally invasive surgery and enhancing patient safety.
[0052] 2. The technical solution of the present invention is adopted, and a method of dipping the tube core in a polyamic acid precursor solution is adopted. By controlling the solid content and viscosity of the polyamic acid precursor solution, the diameter of the rubber notch die, and the number of dipping times, controllable forming of a catheter wall thickness of 4-100 μm is achieved. Compared with the extrusion-molded catheter in the prior art, the thinnest wall thickness can only reach 30 μm, and the catheter wall of the present invention can reach a thinnest 10 μm.
[0053] 3. In view of the problem that during the conversion of the polyamic acid precursor into a polyimide catheter, the molecular chain degrades when heated in the medium and high temperature range, resulting in the brittleness of the short tube, the present invention adopts process steps such as dipping in glue solution, die shaping, pre-baking, soaking in imidization agent, and high-temperature baking in the imidization process of polyamic acid. Among them, soaking in imidization agent will greatly improve the toughness of the polyimide catheter, and increase the surface density to make it have excellent water resistance, which is beneficial to reduce the penetration of blood into the catheter in the cardiovascular system.
[0054] 4. The present invention adopts a combination of block-type molecular segments to achieve high strength, high modulus, anti-twisting and wear resistance of its polyimide catheter, and adopts polyamic acid precursor solution to first form and then solidify to achieve adjustable tube wall thickness, and utilizes the catalytic effect of chemical reagents to ensure its high toughness and density, so as to achieve wide application in high-end medical devices, especially in cardiovascular interventional treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 It is a schematic diagram of the device structure of the medical catheter extrusion process in the prior art.
[0056] Figure 2 It is a schematic diagram of the multi-layer structure of a medical catheter product in the prior art.
[0057] Figure 3 Schematic diagram of the multilayer structure of the polyimide catheter prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0058] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.
[0059] The disclosures of all patent and non-patent literature cited herein are incorporated herein by reference in their entirety.
[0060] As used in the invention, the terms "comprises," "includes," "contains," "covers," "has," "with," or any other variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, article, or apparatus that includes a list of elements need not be limited to only those elements, but may include other elements that are not explicitly listed or that are inherent to the process, method, article, or apparatus. In addition, unless expressly indicated to the contrary, "or" refers to an inclusive "or" rather than an exclusive "or." For example, conditions A or B satisfy any of the following: A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), and both A and B are true (or exist). The phrase "one or more" is intended to cover non-exclusive inclusions. For example, one or more of A, B, and C, means any of the following: A alone, B alone, C alone, a combination of A and B, a combination of B and C, a combination of A and C, or a combination of A, B, and C.
[0061] In addition, "a", "an", "first", etc. are used to describe elements and components described herein. This is done only for convenience and to provide a general sense of the scope of the invention. This description should be understood to include one or at least one, one or at least one, and the singular also includes the plural unless it is obvious that it is meant otherwise.
[0062] Hereinafter, preferred embodiments of the present invention will be described in detail, but the present invention is not limited thereto.
[0063] The present invention provides a design and manufacture of a multifunctional medical polyimide catheter with a multilayer structure, wherein the polyimide material is divided into a substrate layer for supporting function and a bonding layer for adhesion function, a braid or a coil is used as a reinforcing layer, and a thermoplastic material such as fluoroplastic or polyetheramide is used as a lubricating layer. The thickness of each layer and the interface strength are controlled by solution coating, thereby preparing a high-performance precision medical catheter.
[0064] The substrate layer of the polyimide catheter in the present invention adopts a thermosetting polyimide structure, which is prepared by the polycondensation reaction of dianhydride and diamine, wherein the dianhydride monomer mainly includes one or more combinations of phthalic anhydride, pyrazine tetracarboxylic anhydride, cyclobutane dianhydride, 1,4,5,8-naphthalene tetracarboxylic anhydride, 4,4'-biphenyl dianhydride, 2,3,6,7-anthracene tetracarboxylic anhydride, dibenzodioxane hexacyclic dianhydride, 4,4'-terphenyl dianhydride, 3,4,9,10-pyrene tetracarboxylic anhydride, tetraphenyl diether dianhydride, 9,9-bis[4-(3,4-dicarboxylic acid phenoxy)phenyl]fluorene dianhydride, etc., and the dianhydride molecular structure formula is as follows:
[0065]
[0066] In addition, the diamine monomer of the polyimide in the substrate layer mainly includes one or more combinations of p-phenylenediamine, 2,6-diaminopyridine, 1,4-benzidine, 4,4'-diamino-2,2'-dimethylbiphenyl, 2-amino-5 (4-aminophenyl)-pyrimidine, 2,5-di (4-aminophenyl) pyridine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 5-amino-2- (3'-aminophenyl) benzimidazole, 3,3'-dihydroxybiphenyl diamine, 4,4'-diamino-tetramethyl-p-terphenyl, etc., and the diamine molecular formula is as follows:
[0067]
[0068] The adhesive layer of the polyimide catheter in the present invention adopts a thermoplastic polyimide structure, which is also prepared by the polycondensation reaction of dianhydride and diamine, wherein the dianhydride monomer mainly includes one or more combinations of 4,4′-diphenyl ether dianhydride, 4,4′-dibenzophenone tetracarboxylic dianhydride, di-trimellitic anhydride hydroquinone ester, 4,4′-(3,4-dicarboxyphenoxy) benzophenone dianhydride, 4,4′-diphenyl sulfide dianhydride, 4,4′-diphenyl sulfone dianhydride, 4,4′-diphenyl ether dianhydride and 4,4′-bisphenol A diether dianhydride, and the dianhydride molecular formula is as follows:
[0069]
[0070] In addition, the diamine monomer of the thermoplastic polyimide in the adhesive layer mainly includes one or a combination of 4,4′-diaminodiphenyl ether, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,2′-bis[4-(4-aminophenoxy)phenyl]propane, 3,4′-diaminodiphenyl ether, 2,7-bis(4-aminophenoxy)naphthalene, 4,4′-bis(3-aminophenoxy)biphenyl and 4,4′-bis(3-aminophenoxy)benzophenone, and the like, and its structural formula is as follows:
[0071]
[0072] The solvent used to prepare the polyamic acid precursor in the present invention is mainly a polar aprotic solvent, including formamide solvents such as N,N-dimethylformamide or N,N-diethylformamide; acetamide solvents such as N,N-dimethylacetamide or N,N-diethylacetamide; sulfoxide solvents such as dimethyl sulfoxide or diethyl sulfoxide; pyrrolidone solvents such as N-methyl-2-pyrrolidone and N-ethyl-2-pyrrolidone; phenol solvents such as o-cresol, m-cresol, p-cresol; and organic solvents such as tetrahydrofuran (THF), dioxane, dichloromethane, chloroform, hexamethylphosphorotriamide, γ-butyrolactone, cyclopentanone, etc.; the above reagents can be used alone or in combination of two or more as needed.
[0073] The solid content of the polyamic acid solution of the substrate layer and the adhesive layer prepared by the present invention is preferably 6-50wt%, more preferably 8-40wt%, and further preferably 10-30wt%; if the solid content is lower than 6wt%, the polyimide component of the catheter dip coating is small and the single glue application amount is low; if the solid content is higher than 50wt%, the resin will be too viscous or the molecular weight is too small, and it cannot be coated or formed or the performance is brittle.
[0074] The viscosity of the polyamic acid precursor solution prepared by the present invention is preferably 1-100000 cP, more preferably 10-10000 cP, and further preferably 1000-8000 cP. When the viscosity is less than 1 cP, the solution is too thin to adhere to the surface of the tube core. When the viscosity is higher than 10000 cP, the solution is too thick, the leveling property of the glue is low, and the catheter membrane surface is not smooth.
[0075] To improve the leveling, color, adhesion, etc. of the polyamic acid precursor solution prepared by the present invention, leveling agents, pigments, dyes, surfactants, plasticizers, fillers, sensitizers, etc. may be added to the solution, and the added amount is preferably 0.001 to 5 wt%, more preferably 0.01 to 3 wt%.
[0076] In the present invention, the polyimide substrate layer is prepared by a dip coating process, and the tube core is passed through a glue tank of a thermosetting polyimide precursor, and the conveying speed is preferably 0.1 to 50 m / min, more preferably 0.5 to 30 m / min, and further preferably 1 to 10 m / min. At the same time, a die is used to scrape off excess glue, and the thickness of a single molding dry film is preferably 0.5-10 um, more preferably 1-7 um, and further preferably 2-4 um; in addition, the tube core dipped in glue is pre-baked in time, and the temperature of the drying channel is preferably 80-200°C, more preferably 100-180°C, and further preferably 120 to 160°C.
[0077] In the present invention, the reinforcement is made of stainless steel, nickel-titanium alloy, Liquid crystal polymer fibers, Synthetic fibers, etc., preferably corrosion-resistant 304V stainless steel or nickel-titanium alloy in terms of specific strength and specific stiffness; the linear shape of the reinforcement body is flat or round, the thickness * width of the flat section is preferably 0.006mm*0.032mm~0.05mm*0.25mm, more preferably 0.012mm*0.064mm~0.025mm*0.12mm, and the diameter of the circular section is preferably 0.012mm~0.1mm, more preferably 0.024mm~0.072mm; in addition, the PIC of the braided type is preferably 10~200, more preferably 30~150, and the WPI of the coil is preferably 20~180, more preferably 50~150.
[0078] In the present invention, the pre-baked thermosetting and thermoplastic polyimide films are dried and imidized by a multi-stage high-temperature heating process, first heating and then annealing. The high-temperature treatment temperature range is preferably 200-700°C, more preferably 250-600°C, and the treatment time is preferably 1-100min, more preferably 2-40min.
[0079] In the present invention, a layer of thermoplastic lubricating layer material is coated on the surface of the polyimide after high temperature imidization, preferably tetrafluoroethylene (PTFE), fluorinated ethylene propylene copolymer (FEP), soluble polytetrafluoroethylene (PFA), polyvinylidene fluoride (PVDF), polyphenylene sulfone Nylon 11 Nylon 12 Polyurethane Polyetheramide Further pre-selection of tetrafluoroethylene (PTFE) and polyetheramide The thickness of the lubricating layer is preferably 0.5-20 um, more preferably 1-10 um, and even more preferably 2-8 um. In addition, the catheter is subjected to high temperature heat treatment near the melting point of the thermoplastic coating lubricating layer to make its surface dense and smooth, thereby achieving a good lubricating effect.
[0080] In the present invention, the finally processed multi-layer polyimide catheter is tested for thickness tolerance, color uniformity, surface defects, etc., and the catheter that initially meets the requirements is cut according to the product length specification, and then the tube core and the catheter are separated, and finally the key performance indicators of the catheter are tested and analyzed.
[0081] The technical solution of the present invention is further described below by means of specific examples, but the present invention is not limited to these examples.
[0082] First, in the following examples and comparative examples, the following methods were used to evaluate the key properties of the multilayer polyimide catheter.
[0083] (1) Evaluation of catheter cross-section performance
[0084] The multi-layer polyimide catheter sample to be tested was cut into several small sections and placed in a mold. Then the prepared resin and curing agent (2:1) were evenly mixed and slowly poured into the mold to immerse the catheter. Then it was placed in a vacuum oven for heating and curing. After it was completely hardened, it was taken out of the mold, and then finely polished, rough polished and fine polished. Finally, it was cleaned and dried to obtain a transparent sample with a cross section perpendicular to the lens. In addition, the catheter was bent 20 times, and then the bent part was cut and sampled using the same method. The cross-section of the multi-layer catheter was observed and analyzed using a Thermo scientific thermal field emission scanning electron microscope (SEM).
[0085] (2) Catheter pushing force evaluation
[0086] According to ISO 25539-1:2017 standard, a medical catheter pushability tester is used to perform a push test on the catheter sample at a specific path and distance, and its maximum push force value is recorded.
[0087] (3) Catheter torque control response time and torque evaluation
[0088] According to the GB / T16823.3-2010 test standard, a torsion tester is used to test and evaluate the torsion response time and torque of the catheter sample. The flexibility of the catheter is mainly evaluated by the torsion response data. By rotating the proximal end of the catheter, the force of the proximal rotation is transmitted along the catheter to the distal end, so that the distal end rotates 360 degrees. The less time it takes, the more flexible the catheter controllability is. In addition, the force required for the proximal and distal ends of the test catheter to rotate 720 degrees twice is the torque of the catheter. Push force, torsion response and torque are the three key evaluation indicators of the catheter.
[0089] 4) Evaluation of catheter surface sliding performance
[0090] According to the YY / T1536-2017 test standard, the catheter guidewire friction performance tester is used to test the sliding friction of the catheter. The sample catheter clip is installed and the spacing between the two sliding clamps is adjusted, and then the clip is tightened to maintain a good fit; one end of the test catheter is passed through the two catheter clips from bottom to top; the rest of the catheter is inserted into a barrel filled with water, and the positions of the two sliding clamps in the slide are adjusted so that the catheter is located in the center; the test speed, friction times and other parameters of the test are set; the catheter is passed through the silicone sheet for a sufficient distance, and the force relative to displacement curve is recorded, and the guide line on the curve is taken. Tube Tube The average force value of the wetted section of the body.
[0091] Example 1
[0092] This embodiment provides a medical polyimide catheter with a multi-layer structure. Figure 3The polyimide catheter is a multi-layer structure, which is composed of a first substrate layer 1, a reinforcement layer 2, an adhesion layer 3, a second substrate layer 4 and a lubricating layer 5 from the inside to the outside; the adhesion layer is fused with the reinforcement layer, and the adhesion layer and the substrate layer have similar polyimide materials and have good compatibility, so that the entire multi-layer structure forms an integrated structure.
[0093] The specific preparation steps include:
[0094] 1) Preparation of thermosetting polyimide precursor for substrate layer: In a class 1000 clean room at a constant temperature of 23°C and a constant humidity of 50RH%, N,N-dimethylacetamide (DMAc, 15.08kg), 4,4′-diaminodiphenyl ether (4,4′-ODA, 3.5mol, 0.7008kg) and p-phenylenediamine monomer (PDA, 3.5mol, 0.3785kg) were added to a 20L reactor with mechanical stirring and nitrogen protection at room temperature. After stirring for 30min until completely dissolved, 4,4′-biphenyl dicarboxylic anhydride (4,4 ′-BPDA, 3.5 mol, 1.030 kg), stirred for reaction for 2 hours, and then slowly added with isoprene tetracarboxylic anhydride (PMDA, 3.5 mol, 0.763 kg) in multiple batches. When the viscosity reached 2000 cP, the addition was stopped. The mixture was fully stirred for 4 hours to obtain a polyamic acid resin solution with a solid content concentration of 16 wt%. The residual bubbles in the solution were removed by vacuum defoaming (<1 Pa) and allowed to stand for 24 hours. The impurities were removed by filtering the solution through a 2 um filter element. Finally, a polyimide precursor solution for substrate coating was prepared.
[0095] 2) Preparation of the catheter substrate layer: A 0.50 mm silver-plated copper wire was selected as the tube core, which was first coated with a 0.05 mm PTFE lubricating layer, and then the tube core was passed through the glue tank of the thermosetting polyimide precursor at a transmission speed of 2 m / min. At the same time, a die was used to scrape off excess glue, and then the tube core was baked in a pre-oven at 130°C and 150°C for 3 min to dry the solvent for pre-forming. The final dry film thickness of a single gluing was about 0.003 mm. The dipping and pre-baking cycles were repeated 10 times, and finally the substrate layer thickness was about 0.030 mm.
[0096] 3) Preparation of thermoplastic polyimide precursor for adhesion layer: In a class 1000 clean room at a constant temperature of 23°C and a constant humidity of 50 RH%, N,N-dimethylacetamide (DMAc, 14.14 kg), 1,3-bis(4-aminophenoxy)benzene (1,3,4-APB, 2.0 mol, 0.5847 kg) and 4,2′-bis[4-(4-aminophenoxy)phenyl]propane (BAPP, 3.0 mol, 0.8204 kg) were added to a 20 L reactor with mechanical stirring and nitrogen protection at room temperature. ), stirred for 30 minutes until completely dissolved, and then 4,4′-dibenzophenone tetraacid dianhydride (4,4′-BTDA, 4.0 mol, 1.289 kg) was slowly added in batches. When the viscosity reached 2000 cP, the addition was stopped. The mixture was fully stirred for 4 hours to obtain a polyamic acid resin solution with a solid content concentration of 16 wt%. The residual bubbles in the solution were removed by vacuum defoaming (<1 Pa) and allowed to stand for 24 hours. The solution was then passed through a 2 um filter element to remove impurities, and finally a polyimide precursor solution for an adhesion layer was prepared.
[0097] 4) Preparation of catheter reinforcement layer and adhesive layer: 304V stainless steel flat wire braided tube is selected as the reinforcement layer, wherein the flat cross-section thickness*width size of the braided tube is 0.02mm*0.08mm, and the number of crosses per inch (PIC) is 100. First, the pre-baked polyimide substrate layer containing the tube core is passed through the glue tank and pre-baking channel of the thermoplastic polyimide precursor at a speed of 2m / min to prepare a layer of thermoplastic adhesive layer of about 3um; then the reinforced braided tube is nested on the polyimide substrate layer containing the tube core, and then passed through the thermoplastic polyimide solution glue tank and pre-baking channel at a speed of 1m / min, and the thermoplastic polyimide resin is filled into the gap of the braided mesh until the reinforcement is completely buried in the adhesive thermoplastic polyimide resin, and then the tube core is passed through the thermosetting polyimide resin solution glue tank and pre-baking channel as a whole, and then a thermosetting polyimide glue layer of about 3um is coated on the outer surface. Finally, the pre-baked thermosetting and thermoplastic polyimide films were subjected to high-temperature heat treatment, first heat treated at 300°C, 360°C, 420°C and 480°C for 3 minutes each, and then annealed at 400°C, 300°C and 200°C for 3 minutes each, to completely dry and imidize them.
[0098] 5) Preparation of catheter lubrication layer: Using water-soluble polytetrafluoroethylene (PTFE) with a concentration of 10wt% as the raw material for the lubrication layer, the tube core containing the polyimide layer and the reinforcement layer is passed through the PTFE aqueous solution glue tank at a speed of 1m / min, and then passed through a 120°C pre-drying tunnel for drying. The PTFE is coated with a thickness of about 1um per time, and the cycle is repeated 4 times to prepare a 4um lubrication layer. The catheter is then heated to 320°C to soften the PTFE to form a dense and smooth surface structure, thereby achieving a good lubrication effect.
[0099] 6) The tube core was cut into 0.8 m / segments according to the product length specification, and the tube core was separated from the polyimide catheter using a tube core extraction device. The prepared catheter had an inner diameter of 0.50 mm and a wall thickness of about 0.060 mm. Finally, the performance of the catheter was evaluated. The test results are shown in Table 1.
[0100] Example 2
[0101] The only difference between this embodiment and embodiment 1 is that the thermoplastic polyimide formula of the adhesion layer is replaced with a new thermoplastic structure: 4,4′-bis(3-aminophenoxy)benzophenone (BABP, 4.0 mol, 1.586 kg), 4,4′-diphenyl ether dianhydride (4,4′-ODPA, 3.0 mol, 0.9307 kg) and 4,4′-diphenyl sulfone dianhydride (4,4′-DSDA, 1.0 mol, 0.3583 kg), and the other catheter structures and manufacturing processes are the same as those in embodiment 1.
[0102] Example 3
[0103] The difference between this embodiment and embodiment 1 is that the 304V stainless steel braided tube of the reinforcement layer is replaced by a 304V stainless steel coil wire, the number of windings per inch (WPI) is 100, and the other catheter structures and manufacturing processes are the same as those in embodiment 1.
[0104] Example 4
[0105] The difference between this embodiment and embodiment 1 is that the polytetrafluoroethylene (PTFE) of the lubricating layer on the outermost surface is made of polyether amide. Instead, the other catheter structures and manufacturing processes are the same as those in Example 1.
[0106] Comparative Example 1
[0107] The only difference between this comparative example and Example 1 is that the thermoplastic polyimide adhesion layer is not included, and the other catheter structures and manufacturing processes are the same as those of Example 1.
[0108] Comparative Example 2
[0109] The difference between this comparative example and Example 1 is that the thermoplastic polyimide of the adhesive layer is completely replaced by the thermosetting polyimide of the substrate layer. The other catheter structures and manufacturing processes are the same as those of Example 1.
[0110] Comparative Example 3
[0111] The difference between this comparative example and Example 1 is that the number of crosses per inch (PIC) of the reinforcement layer braided tube is 150, and the other catheter structures and manufacturing processes are the same as those of Example 1.
[0112] Comparative Example 4
[0113] The difference between this comparative example and Example 1 is that the number of crosses per inch (PIC) of the reinforcement layer braided tube is 50, and the other catheter structures and manufacturing processes are the same as those of Example 1.
[0114] Comparative Example 5
[0115] The difference between this comparative example and Example 1 is that the reinforcement layer is not included, and the other catheter structures and manufacturing processes are the same as those of Example 1.
[0116] Comparative Example 6
[0117] The difference between this comparative example and Example 1 is that the thermosetting polyimide of the substrate layer is completely replaced by the thermoplastic polyimide of the adhesive layer. The other catheter structures and manufacturing processes are the same as those of Example 1.
[0118] Comparative Example 7
[0119] The only difference between this comparative example and Example 1 is that the lubricating layer on the outermost surface is not included, and the other catheter structures and manufacturing processes are the same as those in Example 1.
[0120] The performance evaluation results of the multilayer polyimide catheters prepared in the embodiments and comparative examples are shown in Table 1. Table 1 Performance comparison of multilayer polyimide catheters prepared in Examples and Comparative Examples
[0121]
[0122] In Table 1, √ represents no stratification; × represents stratification; -- represents stratification cannot be characterized.
[0123] As shown in the performance in the table, Example 1 and Comparative Example 1 and Comparative Example 2 analyze that thermosetting polyimide has good strength, modulus and hardness, but the structure is rigid, the surface is smooth, the interface adhesion with the reinforcement layer is low, and it is easy to delaminate under bending or torsion. Thermoplastic polyimide as an adhesion layer and a buffer layer can greatly improve the interface performance. Example 1, Example 3, Comparative Example 3, Comparative Example 4 and Comparative Example 5 analyze that the reinforcement layer can greatly reduce the pushing force and improve the pushing ability, as well as shorten the torsion control response time and reduce the torque, and improve the flexibility of catheter control. Example 1, Example 4 and Comparative Example 7 analyze that the catheter surface is coated with a lubricating layer such as PTFE and polyetheramide, which can greatly reduce the surface friction coefficient of the catheter and improve the smoothness of the catheter in minimally invasive surgery.
[0124] It should be noted in particular that the present invention is not limited to the various structures described above, and various changes can be made within the scope indicated by the claims. The embodiments and examples obtained by appropriately combining the technical equipment disclosed in different embodiments and examples are also included in the technical scope of the present invention.
[0125] Unless otherwise defined, the meaning of all technical and scientific terms used herein is the same as that generally understood by those of ordinary skill in the art to which the present disclosure belongs. Although methods and materials similar or equivalent to those described herein can be used in the practice or testing of the disclosed composition embodiments, suitable methods and materials are described below. Unless citing a specific paragraph, all publications, patent applications, patents and other references mentioned herein are incorporated herein by reference in their entirety. If a conflict occurs, this specification and the definitions included therein shall prevail. In addition, materials, methods and examples are illustrative only, and not restrictive.
[0126] The technical scheme of the present invention, its implementation process and principle, etc. will be further explained through specific embodiments as follows. It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. The described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. Unless otherwise specified, the reagents and raw materials used in the following examples are commercially available, and the test methods for which specific conditions are not specified are usually carried out under conventional conditions or according to the conditions recommended by the manufacturers. In addition, unless otherwise specified, the experimental methods, detection methods, and preparation methods disclosed in the present invention all adopt conventional techniques in the art. These technologies have been fully described in the existing literature.
[0127] The above are only preferred embodiments of the present invention, which do not limit the protection scope of the present invention. For those skilled in the art, the present invention may have various modifications and changes. Within the spirit and principle of the present invention, changes, modifications, replacements, integrations and parameter changes to these embodiments by conventional substitutions or by being able to achieve the same functions without departing from the principles and spirit of the present invention all fall within the protection scope of the present invention.
Claims
1. A medical polyimide catheter, It is characterized in that The polyimide catheter is a multi-layer structure, which consists of a first substrate layer, a reinforcement layer, an adhesion layer, a second substrate layer and a lubricating layer from the inside to the outside; the adhesion layer fuses the first substrate layer, the reinforcement layer, the second substrate layer and the lubricating layer to form an integrated structure.
2. The polyimide catheter according to claim 1, It is characterized in that The first substrate layer and the second substrate layer are both thermosetting polyimide compounds; The adhesive layer is a thermoplastic polyimide compound; The reinforcement layer is made of stainless steel, nickel-titanium alloy, Liquid crystal polymer fibers, One or a combination of synthetic fibers; The lubricating layer is tetrafluoroethylene (PTFE), fluorinated ethylene propylene copolymer (FEP), soluble polytetrafluoroethylene (PFA), polyvinylidene fluoride (PVDF), polyphenylene sulfone Nylon 11 Nylon 12 Polyurethane Polyetheramide One or a combination of the following.
3. The polyimide catheter according to claim 2, It is characterized in that The material of the reinforcement layer is a braided tube made of linear material; The braided tube comprises a braided mesh or a coil wire; the braided mesh has a cross-in-inch (PIC) number of 10 to 200; The number of windings per inch (WPI) of the coil wire is 20 to 180; The linear material is a flat or round linear material; preferably, the cross-sectional thickness*width of the flat linear material is 0.006mm*0.032mm~0.05mm*0.25mm, and the cross-sectional diameter of the round linear material is 0.012mm~0.1mm.
4. The polyimide catheter according to claim 2, It is characterized in that The thermosetting polyimide compound is prepared by a first dianhydride monomer compound and a first diamine monomer compound through a polycondensation reaction, wherein the dianhydride monomer compound is selected from phthalic anhydride, pyrazine tetracarboxylic anhydride, cyclobutane dianhydride, 1,4,5,8-naphthalene tetracarboxylic anhydride, 4,4'-biphenyl dianhydride, 2,3,6,7-anthracene tetracarboxylic anhydride, dibenzodioxane hexacyclic dianhydride, 4,4'-terphenyl dianhydride, 3,4,9,10-pyrene tetracarboxylic anhydride, tetraphenyl diether dianhydride, 9,9-bis[4-(3,4-dicarboxylic acid phenoxy)phenyl]fluorene dianhydride. One or a combination of several; the diamine monomer compound is selected from one or a combination of p-phenylenediamine, 2,6-diaminopyridine, 1,4-benzidine, 4,4′-diamino-2,2′-dimethylbiphenyl, 2-amino-5(4-aminophenyl)-pyrimidine, 2,5-di(4-aminophenyl)pyridine, 4,4′-diaminodiphenylmethane, 4,4′-diaminodiphenyl ether, 5-amino-2-(3′-aminophenyl)benzimidazole, 3,3′-dihydroxybiphenyl diamine, 4,4′-diamino-tetramethyl-p-terphenyl; And / or, the thermoplastic polyimide compound is prepared by a second dianhydride compound and a second diamine compound through a condensation reaction, wherein the second dianhydride compound is selected from 4,4′-diphenyl ether dianhydride, 4,4′-dibenzophenone tetracarboxylic dianhydride, trimellitic anhydride hydroquinone ester, 4,4′-(3,4-dicarboxyphenoxy)benzophenone dianhydride, 4,4′-diphenyl sulfide dianhydride, 4,4′-diphenyl sulfone dianhydride, 4,4′-diphenyl ether dianhydride and 4,4′-bisphenol A diether dianhydride The second diamine monomer is one or more of 4,4'-diaminodiphenyl ether, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,2'-bis[4-(4-aminophenoxy)phenyl]propane, 3,4'-diaminodiphenyl ether, 2,7-bis(4-aminophenoxy)naphthalene, 4,4'-bis(3-aminophenoxy)biphenyl and 4,4'-bis(3-aminophenoxy)benzophenone.
5. The polyimide catheter according to any one of claims 1 to 4, It is characterized in that The inner diameter of the polyimide catheter is 10 to 1000 μm; The thickness of the lubricating layer is 0.5-20 μm.
6. A method for preparing a polyimide catheter according to any one of claims 1 to 5, It is characterized in that Polyimide materials are used as the first substrate layer and the second substrate layer with a supporting function, and the bonding layer with an adhesion function, a braid or a coil is used as a reinforcing layer, and a fluoroplastic or polyetheramide thermoplastic material is used as a lubricating layer. The thickness and interface strength of each layer are controlled layer by layer through solution coating, thereby preparing the polyimide catheter.
7. The method for preparing a polyimide catheter according to claim 6, It is characterized in that The method comprises adopting a multi-stage dipping-forming process to sequentially form a substrate layer, a reinforcing layer, an adhesion layer, and a lubricating layer on the surface of the tube core; specifically comprising the following steps: S1. Preparation of the first substrate layer; first, a thermosetting polyamic acid precursor solution is dip-coated on the surface of the tube core, and a uniform film is formed on the surface of the tube core after a first pre-drying and qualitative analysis, which is the substrate layer; S2. Preparation of a reinforcing layer and an adhesive layer; nesting the braided tube on the surface of the substrate layer to form a reinforcing layer; immersing the tube core attached with the reinforcing layer in a thermoplastic polyamic acid precursor solution, filling the thermoplastic polyamic acid precursor solution into the gap of the braided tube, and performing a second pre-drying qualitatively to form an adhesive layer on the surface of the reinforcing layer; S3. Preparation of a second substrate layer; immersing the die having the adhesive layer attached thereto in the thermosetting polyamic acid precursor solution, performing a high temperature curing treatment, and completely drying the second substrate layer and the adhesive layer; S4. Preparation of polyimide catheter; finally, the tube core after drying is placed in the lubricant solution, a lubricating layer is coated on the surface of the adhesion layer, and after a third pre-drying and qualitative determination, high-temperature drying is performed again, and the lubricant softens to form a dense and smooth surface structure, thus obtaining the polyimide catheter.
8. The method for preparing a polyimide catheter according to claim 7, It is characterized in that The solvent used in the preparation of the thermosetting polyamic acid precursor solution and the thermoplastic polyamic acid precursor solution is a polar aprotic solvent; preferably, the solvent includes formamide, acetamide, sulfoxide, pyrrolidone; phenolic solvent, tetrahydrofuran (THF), dioxane, dichloromethane, chloroform, hexamethylphosphorus triamide, γ-butyrolactone, cyclopentanone, one or more combinations thereof; the solid content of the thermosetting polyamic acid precursor solution and the thermoplastic polyamic acid precursor solution is 6-50wt%, preferably 8-40wt%, more preferably 10-30wt%; the viscosity is 1-100000cP, preferably 10-10000cP, more preferably 1000-8000cP; The tube core is sequentially transferred to the thermosetting polyamic acid precursor solution and the thermoplastic polyamic acid precursor solution, and the transfer speed is 0.1 to 50 m / min, preferably 0.5 to 30 m / min; The thickness of the first substrate layer and the second substrate layer is 0.5 to 10 μm, preferably 1 to 7 μm, and more preferably 2 to 4 μm; The temperature of the first pre-drying and the second pre-drying is 80-200°C, preferably 100-180°C, and more preferably 120-160°C.
9. The method for preparing a polyimide catheter according to claim 7, It is characterized in that The high temperature curing treatment includes drying and imidizing the first substrate layer, the second substrate layer and the adhesive layer using a multi-stage high temperature heating process; The process conditions of the high temperature curing treatment include first heating up in stages and then annealing; The range of the staged heating is 200-700°C, and the heat treatment time of each stage is 1-100 minutes; the temperature range of the annealing is 150-500°C, and the annealing time is 1-100 minutes; Preferably, the staged heating includes heat treatment at 300°C, 360°C, 420°C and 480°C for 3 min respectively; the annealing includes annealing at 400°C, 300°C and 200°C for 3 min respectively; The high temperature treatment temperature range is preferably 200-700° C., more preferably 250-600° C., and the treatment time is preferably 1-100 min, more preferably 2-40 min.
10. Use of the polyimide catheter according to claim 5 as a medical device, especially an interventional minimally invasive surgical device.
Citation Information
Cited By
Catheter tip and forming method thereof
CN119656450A
Woven reinforced tearable sheath structure and manufacturing method
CN119818802A
A braided reinforced tearable sheath structure and manufacturing method
CN119818802B
Medical polyimide bent catheter for improving lubricating property of inner wall as well as preparation method and application of medical polyimide bent catheter
CN120695268A
Antibacterial thermoplastic polyimide resin for medical catheter as well as preparation method and application of antibacterial thermoplastic polyimide resin
CN120865547A