Anti-counterfeit printing process based on engraved gravure polishing and film covering
By using specific materials to prepare inks and optimizing process parameters in the engraving gravure printing and lamination printing processes, the problem of material compatibility and adhesion is solved, the anti-counterfeiting performance and mechanical properties of the printed matter are improved, and an environmentally friendly and efficient printing effect is achieved.
Patent Information
- Application Number
- CN202410430403.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-29
AI Technical Summary
When combining engraving gravure printing and lamination printing processes, there are issues with material compatibility, poor adhesion, and poor environmental friendliness, resulting in unstable mechanical properties of the final product.
Epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane and other materials are used to prepare the ink, and through polishing and coating processes, process parameters such as temperature, pressure, time, etc. are optimized to ensure that the ink is fully compatible with the coating. High adhesion and stability of the membrane.
It improves the anti-counterfeiting performance, wear resistance and weather resistance of printed matter, enhances the adhesion between ink and film, and improves the mechanical properties and environmental protection of the product.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of special printing technology, and in particular relates to an anti-counterfeiting printing process based on engraving gravure polishing and lamination. Background Art
[0002] Gravure printing is a commonly used anti-counterfeiting printing process, which plays an important role in preventing counterfeiting and improving product safety. Gravure printing uses the unevenness of the gravure to transmit patterns and texts, and is usually used in the production of bills, certificates, packaging and other high-demand fields. At the same time, lamination printing is also a common anti-counterfeiting process, which increases the durability and anti-counterfeiting effect of printed products by covering them with a layer of film. Combining these two processes can further improve the anti-counterfeiting performance, but it will also face some technical difficulties. Gravure printing technology is widely used in financial bills, identity documents and high-end product packaging. In terms of financial bills, gravure printing technology can achieve high-precision pattern and text printing, effectively preventing counterfeiting and tampering. At the same time, gravure printing is also often used in the production of identity documents. Its clear patterns and texts and durable quality improve the recognition and security of the documents. In terms of high-end product packaging, gravure printing is often used to print brand logos, product information, etc., and its high-quality printing effect enhances the image and value of the product. Gravure printing technology has a series of advantages. First, it can achieve high-precision printing effects with rich details and clear patterns. Secondly, gravure printing is highly durable, and the quality of printed products is long-lasting and stable, and it is not easy to fade or damage. In addition, gravure printing is suitable for large-scale production, with fast printing speeds, and can meet high production needs. However, gravure printing also has some disadvantages. First, the initial cost of gravure production is high, and more equipment and gravure production costs need to be invested. Secondly, the gravure production cycle is long, which is not suitable for short-term projects. In addition, gravure printing may not work well for flexible or curved surfaces.
[0003] On the other hand, the lamination printing process increases the durability and anti-counterfeiting effect of the printed matter by covering the surface of the printed matter with a thin film. Lamination printing is widely used in packaging, labels, posters and other fields. In terms of packaging, lamination printing can provide waterproof and scratch-resistant effects to protect the product from the external environment. In terms of labels and posters, lamination printing can increase its gloss and make the printed matter look more attractive. The advantages of lamination printing include high waterproof and wear resistance, easy cleaning, and the ability to increase gloss. However, lamination printing also has some disadvantages, such as high cost, environmental protection, easy to produce bubbles and wrinkles, etc. Combining the two processes of engraving gravure printing and lamination printing can further improve the anti-counterfeiting effect and the quality of printed matter. However, this combination will also face some technical difficulties. First, it is necessary to solve the compatibility problem of gravure printing and lamination printing materials to ensure the coordination and coordination between the two. Secondly, it is necessary to control the parameters in the lamination process, such as temperature, pressure, speed, etc., to ensure that the lamination material can be evenly coated on the surface of the printed matter and the curing effect is good. In addition, it is also necessary to consider the quality and stability of the printed matter after lamination to prevent problems such as bubbles and wrinkles. Finally, we also need to pay attention to environmental protection and sustainability, choose coating materials and processes that meet environmental protection requirements, and reduce the impact on the environment.
[0004] In summary, gravure printing and lamination printing are two common anti-counterfeiting printing processes, each of which has a series of advantages and disadvantages. Combining these two processes can improve the anti-counterfeiting effect and the quality of printed products, but there will also be some technical difficulties, such as: choosing suitable gravure materials, lamination materials and printing inks, it is necessary to consider their compatibility and interaction to ensure the quality and stability of printed products; it is necessary to consider the surface treatment process and post-treatment process suitable for the combination of the two; the control of the lamination process needs to reduce the negative impact on the products of the gravure printing process, etc. In particular, the adhesion between the surface obtained by gravure printing and the lamination surface at different positions is different, resulting in a significant reduction in the mechanical properties of the final product. The problem has not been solved. Through technical improvements and experimental research, solutions to these difficulties can be found, providing more possibilities for the development and application of anti-counterfeiting printing technology. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a process that organically combines the anti-counterfeiting printing process of engraving gravure polishing and laminating, and overcomes the technical difficulties of combining the two. The specific scheme is as follows:
[0006] An anti-counterfeiting printing process based on engraving gravure polishing and lamination includes the following steps:
[0007] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0008] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0009] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0010] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0011] Preferably, the ink described in S1, wherein each component, by mass, includes 50-60 parts of epoxy resin, 35-40 parts of methyl acrylate, 5-8 parts of hydroxypropionic acid resin, 5-8 parts of polymethacrylate-polyurethane, 2-3 parts of solvent, 2-3 parts of plasticizer, and 1-2 parts of antioxidant.
[0012] Preferably, the solvent comprises acetone, the plasticizer comprises xylene, and the antioxidant comprises tert-butyl hydroxyphenol.
[0013] Preferably, the gravure plate described in S1 is made of one or both of copper plate and nickel plate.
[0014] Preferably, the engraved gravure in S1 has an engraving depth of 0.15-0.2 mm and an engraving angle of 30°-45°.
[0015] Preferably, the engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 30°.
[0016] Preferably, in the printing described in S1, the printing thickness is 0.08-0.1 mm; the printing pressure is 50-60 N / cm 2 .
[0017] Preferably, after the printing in S1 is completed, the mixture is naturally dried at room temperature for 5 minutes and then heat treated at 40-50° C. for 5 minutes.
[0018] Preferably, in the polishing step S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5-6 g of abrasive paste is used per square meter of the gravure plate, the polishing head speed is 1200 rpm, and the polishing time is 2-3 minutes, until a mirror effect is achieved.
[0019] Preferably, the coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02-0.03 mm.
[0020] Preferably, in S3, the coating has a coating temperature of 80-150° C. and a coating pressure of 0.2-0.5 MPa.
[0021] Preferably, in S3, the lamination temperature is 80-85° C. and the lamination pressure is 0.2 MPa.
[0022] Beneficial Effects
[0023] The present invention
[0024] High anti-counterfeiting performance: Through the combination of engraving gravure printing and laminating technology, the uniqueness and difficulty of copying of printed products are achieved, greatly improving the anti-counterfeiting performance.
[0025] Good printing effect: the use of high viscosity, high adhesion ink and high-quality gravure ensures that the printed products are brightly colored and rich in layers.
[0026] Strong wear and weather resistance: The printed products after lamination treatment have good wear and weather resistance and can maintain the printing effect for a long time.
[0027] The present invention further improves the mechanical properties of products obtained through an anti-counterfeiting printing process based on engraving gravure polishing and lamination by improving the ink formula and optimizing the step parameters. The adhesion between the ink and the lamination is stronger, and the product performance is better. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0029] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0030] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.
[0031] According to our experimental data and experimental conclusions, the embodiments and comparative examples are designed according to the following logic:
[0032] With polymethacrylate-polyurethane:
[0033] Select low values for laminating temperature and laminating pressure, and match them with specific angles, depths, and thicknesses.
[0034] Other angles, thicknesses, and depths will not adhere to this temperature and pressure.
[0035] Other angles, thicknesses, and depths are not suitable for adhesion with the highest temperature and pressure, but adhesion increases with increasing temperature and pressure.
[0036] Without polymethacrylate-polyurethane: everything is normal
[0037] Examples 1-3 Common Examples Different parameters include polymethacrylate-polyurethane
[0038] After the printing described in Example 4S1 is completed, it is naturally dried at room temperature for 5 minutes and then heat treated at 40-50°C for 5 minutes.
[0039] The engraved gravure described in Example 5S1 has an engraving depth of 0.15 mm and an engraving angle of 30°.
[0040] The coating described in Examples 6 and 7S3 has a coating temperature of 80-85°C and a coating pressure of 0.2 MPa.
[0041] In embodiments 8 and 9, the engraved gravure described in S1 has an engraving depth of 0.15 mm and an engraving angle of 30°. In S3, the lamination temperature is 80-85° C. and the lamination pressure is 0.2 MPa.
[0042] Comparative Examples 1-5: Polymethacrylate-polyurethane is removed from Examples 5, 6, 7, 8, and 9.
[0043] Example 1 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0044] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0045] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0046] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0047] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0048] The ink described in S1, wherein each component, by mass, includes 50-60 parts of epoxy resin, 35-40 parts of methyl acrylate, 5-8 parts of hydroxypropionic acid resin, 5-8 parts of polymethacrylate-polyurethane, 2-3 parts of solvent, 2-3 parts of plasticizer, and 1-2 parts of antioxidant.
[0049] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0050] The gravure plate described in S1 is made of copper plate.
[0051] The engraved gravure in S1 has an engraving depth of 0.15-0.2 mm and an engraving angle of 30°-45°.
[0052] The engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 30°.
[0053] S1 printing, printing thickness is 0.08-0.1mm; printing pressure is 50-60N / cm 2 .
[0054] After the printing in S1 is completed, it is naturally dried at room temperature for 5 minutes and then heat treated at 40-50°C for 5 minutes.
[0055] For polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5-6g of abrasive paste is used per square meter of gravure, the polishing head speed is 1200rpm, and the polishing time is 2-3min. The mirror effect is achieved.
[0056] The coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02-0.03 mm.
[0057] The coating in S3 has a coating temperature of 80-150° C. and a coating pressure of 0.2-0.5 MPa.
[0058] The coating in S3 has a coating temperature of 80-85° C. and a coating pressure of 0.2 MPa.
[0059] Example 1 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0060] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0061] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0062] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0063] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0064] The ink described in S1, wherein the components, by mass, include 50 parts of epoxy resin, 40 parts of methyl acrylate, 8 parts of hydroxypropionic acid resin, 8 parts of polymethacrylate-polyurethane, 3 parts of solvent, 3 parts of plasticizer, and 2 parts of antioxidant.
[0065] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0066] The gravure plate described in S1 is made of copper plate.
[0067] The engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 35°.
[0068] The printing described in S1 has a printing thickness of 0.08 mm and a printing pressure of 50 N / cm 2 .
[0069] After the printing in S1 is completed, it is naturally dried at room temperature for 10 minutes.
[0070] For the polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5g of abrasive paste is used per square meter of the gravure, the polishing head speed is 1200rpm, and the polishing time is 2min. The mirror effect is achieved.
[0071] The coating described in S3 is a polyester film with a thickness of 0.02 mm.
[0072] The coating in S3 has a coating temperature of 100° C. and a coating pressure of 0.4 MPa.
[0073] Example 2 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0074] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0075] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0076] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0077] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0078] The ink described in S1, wherein the components, measured by mass, include 60 parts of epoxy resin, 35 parts of methyl acrylate, 5 parts of hydroxypropionic acid resin, 5 parts of polymethacrylate-polyurethane, 2 parts of solvent, 2 parts of plasticizer, and 1 part of antioxidant.
[0079] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0080] The gravure plate described in S1 is made of copper plate.
[0081] The engraved gravure in S1 has an engraving depth of 0.2 mm and an engraving angle of 45°.
[0082] The printing thickness of S1 is 0.1 mm and the printing pressure is 60 N / cm2 .
[0083] After the printing in S1 is completed, it is naturally dried at room temperature for 10 minutes.
[0084] For polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 6 g of abrasive paste is used per square meter of the gravure, the polishing head speed is 1200 rpm, and the polishing time is 3 minutes. The mirror effect is achieved.
[0085] The coating described in S3 is a polyester film with a thickness of 0.03 mm.
[0086] The coating in S3 has a coating temperature of 150° C. and a coating pressure of 0.5 MPa.
[0087] Example 3 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0088] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0089] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0090] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0091] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0092] The ink described in S1, wherein each component, by mass, includes 55 parts of epoxy resin, 35 parts of methyl acrylate, 5 parts of hydroxypropionic acid resin, 5 parts of polymethacrylate-polyurethane, 2 parts of solvent, 2 parts of plasticizer, and 1 part of antioxidant.
[0093] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0094] The gravure plate described in S1 is made of copper plate.
[0095] The engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 40°.
[0096] The printing thickness of S1 is 0.09 mm and the printing pressure is 55 N / cm 2 .
[0097] After the printing in S1 is completed, it is naturally dried at room temperature for 10 minutes.
[0098] For the polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5g of abrasive paste is used per square meter of the gravure, the polishing head speed is 1200rpm, and the polishing time is 2min. The mirror effect is achieved.
[0099] The coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02 mm.
[0100] The coating in S3 has a coating temperature of 120° C. and a coating pressure of 0.4 MPa.
[0101] Example 4 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0102] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0103] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0104] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0105] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0106] The ink described in S1, wherein each component, by mass, includes 55 parts of epoxy resin, 35 parts of methyl acrylate, 5 parts of hydroxypropionic acid resin, 5 parts of polymethacrylate-polyurethane, 2 parts of solvent, 2 parts of plasticizer, and 1 part of antioxidant.
[0107] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0108] The gravure plate described in S1 is made of copper plate.
[0109] The engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 40°.
[0110] The printing thickness of S1 is 0.09 mm and the printing pressure is 55 N / cm 2 .
[0111] After the printing in S1 is completed, it is naturally dried at room temperature for 5 minutes and then heat treated at 50°C for 5 minutes.
[0112] For the polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5g of abrasive paste is used per square meter of the gravure, the polishing head speed is 1200rpm, and the polishing time is 2min. The mirror effect is achieved.
[0113] The coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02 mm.
[0114] The coating in S3 has a coating temperature of 120° C. and a coating pressure of 0.4 MPa.
[0115] Example 5 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0116] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0117] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0118] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0119] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0120] The ink described in S1, wherein each component, by mass, includes 55 parts of epoxy resin, 35 parts of methyl acrylate, 5 parts of hydroxypropionic acid resin, 5 parts of polymethacrylate-polyurethane, 2 parts of solvent, 2 parts of plasticizer, and 1 part of antioxidant.
[0121] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0122] The gravure plate described in S1 is made of copper plate.
[0123] The engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 30°.
[0124] The printing thickness of S1 is 0.09 mm and the printing pressure is 55 N / cm 2 .
[0125] After the printing in S1 is completed, it is naturally dried at room temperature for 10 minutes.
[0126] For the polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5g of abrasive paste is used per square meter of the gravure, the polishing head speed is 1200rpm, and the polishing time is 2min. The mirror effect is achieved.
[0127] The coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02 mm.
[0128] The coating in S3 has a coating temperature of 120° C. and a coating pressure of 0.4 MPa.
[0129] Example 6 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0130] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0131] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0132] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0133] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0134] The ink described in S1, wherein each component, by mass, includes 55 parts of epoxy resin, 35 parts of methyl acrylate, 5 parts of hydroxypropionic acid resin, 5 parts of polymethacrylate-polyurethane, 2 parts of solvent, 2 parts of plasticizer, and 1 part of antioxidant.
[0135] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0136] The gravure plate described in S1 is made of copper plate.
[0137] The engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 40°.
[0138] The printing thickness of S1 is 0.09 mm and the printing pressure is 55 N / cm 2 .
[0139] After the printing in S1 is completed, it is naturally dried at room temperature for 10 minutes.
[0140] For the polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5g of abrasive paste is used per square meter of the gravure, the polishing head speed is 1200rpm, and the polishing time is 2min. The mirror effect is achieved.
[0141] The coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02 mm.
[0142] The coating in S3 has a coating temperature of 80° C. and a coating pressure of 0.2 MPa.
[0143] Example 7 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0144] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0145] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0146] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0147] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0148] The ink described in S1, wherein each component, by mass, includes 55 parts of epoxy resin, 35 parts of methyl acrylate, 5 parts of hydroxypropionic acid resin, 5 parts of polymethacrylate-polyurethane, 2 parts of solvent, 2 parts of plasticizer, and 1 part of antioxidant.
[0149] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0150] The gravure plate described in S1 is made of copper plate.
[0151] The engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 40°.
[0152] The printing thickness of S1 is 0.09 mm and the printing pressure is 55 N / cm 2 .
[0153] After the printing in S1 is completed, it is naturally dried at room temperature for 10 minutes.
[0154] For the polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5g of abrasive paste is used per square meter of the gravure, the polishing head speed is 1200rpm, and the polishing time is 2min. The mirror effect is achieved.
[0155] The coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02 mm.
[0156] The coating in S3 has a coating temperature of 85° C. and a coating pressure of 0.2 MPa.
[0157] Example 8 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0158] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0159] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0160] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0161] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0162] The ink described in S1, wherein each component, by mass, includes 55 parts of epoxy resin, 35 parts of methyl acrylate, 5 parts of hydroxypropionic acid resin, 5 parts of polymethacrylate-polyurethane, 2 parts of solvent, 2 parts of plasticizer, and 1 part of antioxidant.
[0163] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0164] The gravure plate described in S1 is made of copper plate.
[0165] The engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 30°.
[0166] The printing thickness of S1 is 0.09 mm and the printing pressure is 55 N / cm 2 .
[0167] After the printing in S1 is completed, it is naturally dried at room temperature for 10 minutes.
[0168] For the polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5g of abrasive paste is used per square meter of the gravure, the polishing head speed is 1200rpm, and the polishing time is 2min. The mirror effect is achieved.
[0169] The coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02 mm.
[0170] The coating in S3 has a coating temperature of 80° C. and a coating pressure of 0.2 MPa.
[0171] Example 9 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0172] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0173] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0174] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0175] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0176] The ink described in S1, wherein each component, by mass, includes 55 parts of epoxy resin, 35 parts of methyl acrylate, 5 parts of hydroxypropionic acid resin, 5 parts of polymethacrylate-polyurethane, 2 parts of solvent, 2 parts of plasticizer, and 1 part of antioxidant.
[0177] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0178] The gravure plate described in S1 is made of copper plate.
[0179] The engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 30°.
[0180] The printing thickness of S1 is 0.09 mm and the printing pressure is 55 N / cm 2 .
[0181] After the printing in S1 is completed, it is naturally dried at room temperature for 10 minutes.
[0182] For the polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5g of abrasive paste is used per square meter of the gravure, the polishing head speed is 1200rpm, and the polishing time is 2min. The mirror effect is achieved.
[0183] The coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02 mm.
[0184] The coating in S3 has a coating temperature of 85° C. and a coating pressure of 0.2 MPa.
[0185] Comparative Example 1 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0186] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0187] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0188] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0189] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0190] The ink described in S1, wherein the components, calculated by mass, include 55 parts of epoxy resin, 35 parts of methyl acrylate, 5 parts of hydroxypropionic acid resin, 2 parts of solvent, 2 parts of plasticizer, and 1 part of antioxidant.
[0191] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0192] The gravure plate described in S1 is made of copper plate.
[0193] The engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 30°.
[0194] The printing thickness of S1 is 0.09 mm and the printing pressure is 55 N / cm 2 .
[0195] After the printing in S1 is completed, it is naturally dried at room temperature for 10 minutes.
[0196] For the polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5g of abrasive paste is used per square meter of the gravure, the polishing head speed is 1200rpm, and the polishing time is 2min. The mirror effect is achieved.
[0197] The coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02 mm.
[0198] The coating in S3 has a coating temperature of 120° C. and a coating pressure of 0.4 MPa.
[0199] Comparative Example 2 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0200] S1. Printing gravure pattern: Printing ink on the engraved gravure to obtain a printed gravure pattern.
[0201] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0202] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0203] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0204] The ink described in S1, wherein the components, calculated by mass, include 55 parts of epoxy resin, 35 parts of methyl acrylate, 5 parts of hydroxypropionic acid resin, 2 parts of solvent, 2 parts of plasticizer, and 1 part of antioxidant.
[0205] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0206] The gravure plate described in S1 is made of copper plate.
[0207] The engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 40°.
[0208] The printing thickness of S1 is 0.09 mm and the printing pressure is 55 N / cm 2 .
[0209] After the printing in S1 is completed, it is naturally dried at room temperature for 10 minutes.
[0210] For the polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5g of abrasive paste is used per square meter of the gravure, the polishing head speed is 1200rpm, and the polishing time is 2min. The mirror effect is achieved.
[0211] The coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02 mm.
[0212] The coating in S3 has a coating temperature of 80° C. and a coating pressure of 0.2 MPa.
[0213] Comparative Example 3 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0214] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0215] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0216] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0217] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0218] The ink described in S1, wherein the components, calculated by mass, include 55 parts of epoxy resin, 35 parts of methyl acrylate, 5 parts of hydroxypropionic acid resin, 2 parts of solvent, 2 parts of plasticizer, and 1 part of antioxidant.
[0219] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0220] The gravure plate described in S1 is made of copper plate.
[0221] The engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 40°.
[0222] The printing thickness of S1 is 0.09 mm and the printing pressure is 55 N / cm 2 .
[0223] After the printing in S1 is completed, it is naturally dried at room temperature for 10 minutes.
[0224] For the polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5g of abrasive paste is used per square meter of the gravure, the polishing head speed is 1200rpm, and the polishing time is 2min. The mirror effect is achieved.
[0225] The coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02 mm.
[0226] The coating in S3 has a coating temperature of 85° C. and a coating pressure of 0.2 MPa.
[0227] Comparative Example 4 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0228] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0229] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0230] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0231] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0232] The ink described in S1, wherein the components, calculated by mass, include 55 parts of epoxy resin, 35 parts of methyl acrylate, 5 parts of hydroxypropionic acid resin, 2 parts of solvent, 2 parts of plasticizer, and 1 part of antioxidant.
[0233] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0234] The gravure plate described in S1 is made of copper plate.
[0235] The engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 30°.
[0236] The printing thickness of S1 is 0.09 mm and the printing pressure is 55 N / cm 2 .
[0237] After the printing in S1 is completed, it is naturally dried at room temperature for 10 minutes.
[0238] For the polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5g of abrasive paste is used per square meter of the gravure, the polishing head speed is 1200rpm, and the polishing time is 2min. The mirror effect is achieved.
[0239] The coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02 mm.
[0240] The coating in S3 has a coating temperature of 80° C. and a coating pressure of 0.2 MPa.
[0241] Comparative Example 5 Anti-counterfeiting printing process based on engraving gravure polishing and lamination:
[0242] S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure;
[0243] S2, gravure polishing: polishing the obtained printing gravure with a polishing machine;
[0244] S3, laminating treatment: laminating the polished gravure plate with a laminating machine;
[0245] The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
[0246] The ink described in S1, wherein the components, calculated by mass, include 55 parts of epoxy resin, 35 parts of methyl acrylate, 5 parts of hydroxypropionic acid resin, 2 parts of solvent, 2 parts of plasticizer, and 1 part of antioxidant.
[0247] The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
[0248] The gravure plate described in S1 is made of copper plate.
[0249] The engraved gravure in S1 has an engraving depth of 0.15 mm and an engraving angle of 30°.
[0250] The printing thickness of S1 is 0.09 mm and the printing pressure is 55 N / cm 2 .
[0251] After the printing in S1 is completed, it is naturally dried at room temperature for 10 minutes.
[0252] For the polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5g of abrasive paste is used per square meter of the gravure, the polishing head speed is 1200rpm, and the polishing time is 2min. The mirror effect is achieved.
[0253] The coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02 mm.
[0254] The coating in S3 has a coating temperature of 85° C. and a coating pressure of 0.2 MPa.
[0255] The performance of the anti-counterfeiting printing products obtained in all the above embodiments and comparative examples was tested, and the testing method was as follows:
[0256] GB / T 6742-2007: This is the implementation standard for the adhesion of screen printing UV ink. Among them, we use the sticking and pulling method to test the adhesion, that is, use the tape to stick and pull on the printed surface, and judge whether the adhesion meets the requirements by observing the area of the ink layer that is pulled off. Sticking and pulling method: Use a specific type of tape (3M tape) to stick on the anti-counterfeiting film (ink surface) coated with ink and quickly tear it off to observe whether there is ink residue on the tape. The less the residual ink, the better the adhesion.
[0257] ASTM quality reference standard: Use the 100-grid test method in the ASTM standard to test the adhesion between ink and film. The strength of adhesion is judged by evaluating the proportion or area of ink shedding. 100-grid test method: Draw a certain size of squares on the anti-counterfeiting film (ink surface) coated with ink, then stick and tear off with tape, and observe the shedding of ink in the squares. The less ink shedding, the better the adhesion.
[0258] Stretching method: Stretch the anti-counterfeiting film and observe whether the ink falls off or breaks. If the ink remains intact during the stretching process, it means that the adhesion is good. (The tensile strength data recorded is the tensile strength at which the ink begins to fall off or break) The results are shown in Table 1.
[0259] Table 1 Mechanical properties of the obtained products
[0260]
[0261] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
[0262] The present invention and its implementation methods are described above, and such description is not restrictive, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, they can design methods and embodiments similar to the technical solution without creativity, which should all fall within the protection scope of the present invention.
Claims
1. An anti-counterfeiting printing process based on engraving, gravure polishing and lamination, Features: The following steps are involved: S1. Printing gravure pattern: printing ink on the engraved gravure to obtain a printed gravure; S2, gravure polishing: polishing the obtained printing gravure with a polishing machine; S3, laminating treatment: laminating the polished gravure plate with a laminating machine; The ink described in S1 includes epoxy resin, methyl acrylate, hydroxypropionic acid resin, polymethacrylate-polyurethane, solvent, plasticizer, and antioxidant.
2. The anti-counterfeiting printing process based on engraving gravure polishing and lamination according to claim 1, Features: The ink described in S1, wherein each component, by mass, includes 50-60 parts of epoxy resin, 35-40 parts of methyl acrylate, 5-8 parts of hydroxypropionic acid resin, 5-8 parts of polymethacrylate-polyurethane, 2-3 parts of solvent, 2-3 parts of plasticizer, and 1-2 parts of antioxidant.
3. The anti-counterfeiting printing process based on engraving gravure polishing and lamination according to claim 1, Features: The solvent includes acetone, the plasticizer includes xylene, and the antioxidant includes tert-butyl hydroxyphenol.
4. The anti-counterfeiting printing process based on engraving gravure polishing and lamination according to claim 1, Features: The engraved gravure in S1 has an engraving depth of 0.15-0.2 mm and an engraving angle of 30°-45°.
5. The anti-counterfeiting printing process based on engraving gravure polishing and lamination according to claim 1, Features: S1 printing, printing thickness is 0.08-0.1mm; printing pressure is 50-60N / cm 2 .
6. The anti-counterfeiting printing process based on engraving gravure polishing and lamination according to claim 1, Features: After the printing in S1 is completed, it is naturally dried at room temperature for 5 minutes and then heat treated at 40-50°C for 5 minutes.
7. The anti-counterfeiting printing process based on engraving gravure polishing and lamination according to claim 1, Features: For the polishing described in S2, a diamond abrasive paste with a particle size of 1000 mesh is selected, 5-6 g of abrasive paste is used per square meter of gravure, the polishing head speed is 1200 rpm, and the polishing time is 2-3 min.
8. The anti-counterfeiting printing process based on engraving gravure polishing and lamination according to claim 1, Features: The coating in S3 is a polyester film or a polycarbonate film with a thickness of 0.02-0.03 mm.
9. The anti-counterfeiting printing process based on engraving gravure polishing and lamination according to claim 1, Features: The coating in S3 has a coating temperature of 80-150° C. and a coating pressure of 0.2-0.5 MPa.