Composite plastic hose as well as preparation method and application thereof

By incorporating modified hydrotalcite and nanocellulose into polyvinyl chloride resin, a stable double network structure is constructed, which solves the problem of insufficient thermal stability and mechanical properties of polyvinyl chloride materials and realizes composite plastics with both strength and toughness. Preparation of hose.

CN118852804AInactive Publication Date: 2024-10-29GUANGZHOU HUAXIN PLASTIC PROD CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410930341.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

PVC plastic pipes have poor performance at high and low temperatures, lack of elasticity, and are difficult to machine. They need to be modified to improve performance.

Method used

Incorporate composite modified hydrotalcite and composite modified nanocellulose into the polyvinyl chloride resin matrix, and improve the interlayer spacing of hydrotalcite and the strength of nanocellulose through calcination, silane coupling agent and sodium dodecyl sulfate modification. Elongation at break to build a stable double network interpenetrating structure.

Benefits of technology

Significantly improve the thermal stability and mechanical properties of polyvinyl chloride, obtain a composite plastic hose with both strength and toughness, and solve the problem of decomposition of polyvinyl chloride materials during the extrusion process and the low elongation at break of nanocellulose .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852804A_ABST
    Figure CN118852804A_ABST
Patent Text Reader

Abstract

The invention provides a composite plastic hose as well as a preparation method and application thereof. The composite plastic hose is prepared from polyvinyl chloride resin, acrylic resin, an ethylene-vinyl acetate copolymer, composite modified hydrotalcite, composite modified nano cellulose, a stabilizer, an antioxidant and a lubricant. The modified hydrotalcite is obtained by sequentially calcining hydrotalcite, modifying with a silane coupling agent and modifying with lauryl sodium sulfate; the composite modified nano-cellulose is of a double interpenetrating network structure composed of nano-cellulose and polyacrylamide, the surface of the nano-cellulose is coated with a polydopamine layer, and polyacrylamide is obtained through in-situ polymerization reaction of an acrylamide monomer. According to the invention, the composite modified hydrotalcite and the composite modified nanocellulose are doped into a polyvinyl chloride resin matrix, so that the composite plastic hose with both strength and toughness can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of plastic hoses and relates to a composite plastic hose and a preparation method and application thereof. Background Art

[0002] Plastic pipes have the advantages of light weight, high strength, simple manufacturing method, low economic cost, convenient processing and use, corrosion resistance, and long life. They gradually replace metal, cement and other pipes and become the main application pipes in urban construction, rural water network laying, electrical transmission and other fields. Polyvinyl chloride plastic pipes are an important polymer material that is particularly widely used among many plastic pipes. Polyvinyl chloride plastic pipes have excellent physical and chemical properties such as good flame retardant effect, strong acid and alkali resistance, high structural strength, and good electrical insulation. However, since the polyvinyl chloride resin material itself is a polar difficult to crystallize polymer, the branching degree is small, the relative density is low, about 1.4, the glass transition temperature is between 77℃ and 90℃, and when heated to about 170℃, the polyvinyl chloride material begins to decompose. Therefore, the existing polyvinyl chloride plastic pipes have poor high and low temperature resistance, insufficient elasticity, and great difficulty in mechanical processing. It is necessary to modify the polyvinyl chloride plastic pipe accordingly to improve its performance. Summary of the invention

[0003] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a composite plastic hose and a preparation method and application thereof. The present invention can obtain a composite plastic hose with both strength and toughness by adding composite modified hydrotalcite and composite modified nanocellulose into a polyvinyl chloride resin matrix. The present invention calcines, silane coupling agent modifies and sodium dodecyl sulfate modifies the hydrotalcite to achieve intercalation modification of the hydrotalcite, improves the interlayer spacing of the hydrotalcite, can significantly improve the thermal stability of polyvinyl chloride, and prevents polyvinyl chloride from decomposing during the extrusion process. The present invention modifies the nanocellulose with dopamine, and generates polyacrylamide through in-situ polymerization reaction, constructs a stable and dense double network interpenetrating structure, effectively solves the problem of low elongation at break of nanocellulose, and obtains composite modified nanocellulose with high strength and high toughness.

[0004] To achieve this object, the present invention adopts the following technical solutions:

[0005] In a first aspect, the present invention provides a composite plastic hose, the composite plastic hose comprising polyvinyl chloride resin, acrylic resin, ethylene-vinyl acetate copolymer, composite modified hydrotalcite, composite modified nanocellulose, stabilizer, antioxidant and lubricant;

[0006] The modified hydrotalcite is obtained by sequentially calcining, modifying with a silane coupling agent and modifying with sodium dodecyl sulfate.

[0007] The composite modified nanocellulose is a double interpenetrating network structure composed of nanocellulose and polyacrylamide. The surface of the nanocellulose is coated with a polydopamine layer, and the polyacrylamide is obtained by in-situ polymerization of acrylamide monomers.

[0008] The present invention can obtain a composite plastic hose with both strength and toughness by adding composite modified hydrotalcite and composite modified nanocellulose into a polyvinyl chloride resin matrix. The present invention calcines, modifies with a silane coupling agent and modifies with sodium dodecyl sulfate the hydrotalcite to achieve intercalation modification of the hydrotalcite, improves the interlayer spacing of the hydrotalcite, can significantly improve the thermal stability of polyvinyl chloride, and prevents the polyvinyl chloride from decomposing during the extrusion process. The present invention modifies the nanocellulose with dopamine, generates polyacrylamide through an in-situ polymerization reaction, constructs a stable and dense double network interpenetrating structure, effectively solves the problem of low elongation at break of the nanocellulose, and obtains a composite modified nanocellulose with high strength and high toughness.

[0009] As a preferred technical solution of the present invention, the composite plastic hose comprises the following components in parts by weight:

[0010]

[0011]

[0012] The weight proportion of polyvinyl chloride can be 40, 41, 42, 43, 44, 45, 46, 47, 48, 49 or 50 parts; the weight proportion of acrylic resin can be 20, 21, 22, 23, 24, 25, 26, 27, 28, 29 or 30 parts; the weight proportion of ethylene-vinyl acetate copolymer can be 5.0, 5.2, 5 .4 parts, 5.6 parts, 5.8 parts, 6.0 parts, 6.2 parts, 6.4 parts, 6.6 parts, 6.8 parts, 7.0 parts, 7.2 parts, 7.4 parts, 7.6 parts, 7.8 parts or 8.0 parts; the weight parts of the composite modified hydrotalcite can be 10 parts, 10.2 parts, 10.4 parts, 10.6 parts, 10.8 parts, 11 parts, 11.2 parts, 11.4 parts, 11.6 parts, 11.8 parts or 12 parts; The weight portion of the composite modified nanocellulose can be 2.0 parts, 2.1 parts, 2.2 parts, 2.3 parts, 2.4 parts, 2.5 parts, 2.6 parts, 2.7 parts, 2.8 parts, 2.9 parts or 3.0 parts; the weight portion of the stabilizer can be 1.0 parts, 1.5 parts, 2.0 parts, 2.5 parts, 3.0 parts, 3.5 parts, 4.0 parts, 4.5 parts or 5.0 parts; the weight portion of the antioxidant can be 0.1 parts, 0. .15 parts, 0.2 parts, 0.25 parts, 0.3 parts, 0.35 parts, 0.4 parts, 0.45 parts or 0.5 parts; the weight parts of the lubricant can be 0.5 parts, 0.55 parts, 0.6 parts, 0.65 parts, 0.7 parts, 0.75 parts, 0.8 parts, 0.85 parts, 0.9 parts, 0.95 parts or 1 parts, but are not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0013] The mechanical properties of the composite plastic hose are closely related to the addition amount of the composite modified hydrotalcite. When the addition amount of the composite modified hydrotalcite is low, the mechanical properties of the composite plastic hose gradually increase with the increase of the addition amount of the composite modified hydrotalcite. However, excessive composite modified hydrotalcite will cause the mechanical properties of the composite plastic hose to decrease. This is because when the addition amount of the composite modified hydrotalcite is 10 to 12 parts, the composite modified hydrotalcite is easier to be evenly dispersed in the resin matrix. When the addition amount of the composite modified hydrotalcite exceeds 12 parts, it is easy to agglomerate or aggregate in the resin matrix, thereby affecting the mechanical properties of the composite plastic hose.

[0014] When the composite modified nanocellulose is not added, the impact fracture surface of the resin matrix is ​​relatively smooth, and the resin matrix is ​​relatively brittle on a macroscopic scale. When 2 to 3 parts of composite modified nanocellulose are added to the resin matrix, the fracture surface of the composite plastic hose becomes rough and many evenly distributed small holes and protrusions appear, which is caused by the breakage or pulling out of the composite modified nanocellulose. Since the composite plastic hose undergoes a series of operations such as melting and stirring, melt extrusion, and injection molding during the preparation process, the composite modified nanocellulose is evenly dispersed in the resin matrix, ensuring the uniform distribution of small holes and protrusions, which is beneficial to the improvement of the mechanical properties of the composite plastic hose.

[0015] As the amount of composite modified nanocellulose added increases, the size of these small holes and protrusions gradually increases, the number gradually increases, and the distribution becomes uneven, which leads to a decrease in the mechanical properties of the composite plastic hose on a macro scale. When the amount of composite modified nanocellulose added exceeds 3 parts, the composite modified nanocellulose shows serious agglomeration in the resin matrix, and the holes and fracture surfaces left by the composite modified nanocellulose reach the micron level. Larger holes appear on the cross section of the composite plastic hose, and the stress-strain curve of the composite plastic hose shows the characteristics of brittle fracture.

[0016] The present invention can also significantly reduce the size of the spherulites of the composite plastic hose by adding the composite modified nanocellulose, which is beneficial to the improvement of the toughness of the composite plastic hose. The spherulites of the resin matrix without the addition of the composite modified nanocellulose are larger in size and the number of spherulites is smaller. This is because, when the composite modified nanocellulose does not exist in the resin melt, the spherulites of the resin melt have enough growth space and stop growing until the spherulites touch each other, so that large-sized and small-number spherulites can be obtained. After the composite modified nanocellulose is added, the composite modified nanocellulose plays the role of a heterogeneous nucleating agent in the resin matrix, which can promote the crystallization of the resin matrix, so that the number of spherulites of the composite plastic hose after injection molding is significantly increased, the size of the spherulites is greatly reduced, and the toughness of the composite plastic hose is significantly improved as the size of the spherulites is reduced.

[0017] When the addition amount of composite modified nanocellulose is between 2 and 3 parts, the nucleation ability of composite modified nanocellulose in the resin matrix is ​​the strongest, and the spherulite size of the composite plastic hose is the smallest. With the increase of the addition amount of composite modified nanocellulose, part of the composite modified nanocellulose agglomerates, resulting in a decrease in nucleation ability, which is not conducive to further reduction of the spherulite size.

[0018] The present invention can also significantly improve the impact strength of the composite plastic hose by adding the composite modified nanocellulose. With the increase of the added amount of the composite modified nanocellulose, the impact strength of the composite plastic hose shows a trend of first increasing and then decreasing. This is because, in terms of interface bonding, when the composite modified nanocellulose exceeds 3 parts, the composite modified nanocellulose will show serious agglomeration in the resin matrix, and the agglomeration of the composite modified nanocellulose will weaken the interface bonding force between the composite modified nanocellulose and the resin matrix. When the composite plastic hose is subjected to external force, stress concentration is easily generated, resulting in a reduction in the absorption of impact energy and a reduction in impact strength. In terms of crystallization behavior, the serious agglomeration of the composite modified nanocellulose in the resin matrix will reduce its nucleation ability, and the addition of the composite modified nanocellulose makes the spherulite structure of the resin matrix more perfect, but the improvement of the crystal structure is not conducive to the toughening modification of the resin matrix, and the toughness will be significantly reduced with the improvement of the degree of crystal perfection.

[0019] As a preferred technical solution of the present invention, the stabilizer is a calcium zinc stabilizer.

[0020] In some optional examples, the antioxidant includes any one of antioxidant 1010, antioxidant 1076, antioxidant 626, antioxidant 168 or antioxidant DLTP, or a combination of at least two thereof.

[0021] In some optional examples, the lubricant includes any one of stearic acid, zinc stearate, calcium stearate, polyethylene wax, or a combination of at least two thereof.

[0022] In a second aspect, the present invention provides a method for preparing the composite plastic hose according to the first aspect, the preparation method comprising:

[0023] (I) grinding and crushing hydrotalcite to obtain hydrotalcite powder, calcining the hydrotalcite powder at high temperature to obtain calcined hydrotalcite; mixing a silane coupling agent with an ethanol aqueous solution to obtain a silane coupling agent solution, immersing the calcined hydrotalcite in the silane coupling agent solution to form a hydrotalcite dispersion, heating and stirring the hydrotalcite dispersion to react, filtering and drying after the reaction to obtain silanized hydrotalcite; dispersing the silanized hydrotalcite in a sodium dodecyl sulfate solution, dispersing the mixture by ultrasonication to obtain a mixed solution, filtering and drying the mixed solution to obtain a composite modified hydrotalcite;

[0024] (II) dissolving dopamine in a Tris-hydrochloric acid buffer solution to obtain a dopamine solution, soaking the nanocellulose powder in the dopamine solution for a period of time, and then vacuum filtering and first freeze drying to obtain modified nanocellulose; mixing acrylamide monomer, N,N-methylenebisacrylamide and deionized water to obtain a monomer solution, adding the modified nanocellulose to the monomer solution, mixing evenly to obtain a reaction solution, adding potassium persulfate to the reaction solution, mixing and heating to cause a polymerization reaction, and after the reaction is completed, vacuum filtering and second freeze drying to obtain a composite modified nanocellulose;

[0025] (III) mixing polyvinyl chloride resin, acrylic resin, ethylene-vinyl acetate copolymer, the composite modified hydrotalcite obtained in step (I), the composite modified nanocellulose obtained in step (II), a stabilizer, an antioxidant and a lubricant, and then putting them into a mixer for high-temperature melting and high-speed stirring to obtain a mixed melt; sending the mixed melt into a screw extruder for extrusion granulation to obtain a plastic masterbatch; sending the plastic masterbatch into an injection molding machine for injection molding, and obtaining the composite plastic hose after cooling.

[0026] The present invention adds hydrotalcite to the resin matrix to increase the thermal decomposition temperature of polyvinyl chloride, ensure the smooth progress of melt extrusion, and prevent the mechanical strength of the composite plastic hose after molding from being adversely affected. This is because hydrotalcite is a layered double metal hydroxide, the ions in the layer plates are connected by covalent bonds, and the exchangeable anions are between the metal layers. Common anions between the hydrotalcite layers are CO3 2- and HCO3 - During the melt extrusion process of polyvinyl chloride, polyvinyl chloride will release HCl gas, which will darken the color of the resin matrix obtained after melt extrusion and reduce its strength. After adding hydrotalcite to the resin matrix, first, the CO3 2- and HCO3 - Alkaline ions can undergo ion exchange reaction with HCl produced by the degradation of polyvinyl chloride, and can well absorb the HCl gas produced by the thermal decomposition of polyvinyl chloride. Secondly, the layer of hydrotalcite will adsorb HCl gas to form metal chloride, which effectively slows down the autocatalytic degradation of HCl, thereby preventing the catalytic effect of HCl on the thermal decomposition of polyvinyl chloride, and can effectively improve the thermal stability of polyvinyl chloride and prevent polyvinyl chloride from thermal decomposition due to excessively high temperature during the melt extrusion process.

[0027] The present invention performs calcination treatment on the hydrotalcite before modifying the hydrotalcite with a silane coupling agent. During the calcination process, the hydrotalcite removes all water and interlayer anions of the hydrotalcite, leaving only the composite metal oxide, and the layered structure of the hydrotalcite is completely destroyed. This structural characteristic enables the anions in the sodium dodecyl sulfate solution to re-enter the interlayer of the hydrotalcite when the hydrotalcite is re-added to the sodium dodecyl sulfate solution, so as to achieve intercalation modification of the hydrotalcite, increase the interlayer distance of the hydrotalcite, and facilitate the adsorption of HCl gas between the layers of the hydrotalcite.

[0028] In order to improve the dispersibility and compatibility of hydrotalcite in the resin matrix, the present invention adopts a silane coupling agent and a sodium dodecyl sulfate solution to carry out a joint modification treatment on the calcined hydrotalcite, organically modify the surface of the calcined hydrotalcite by the silane coupling agent, change the hydrophilicity of its surface by chemical adsorption and chemical bonding, improve the distribution uniformity, activation degree and effective action area of ​​the calcined hydrotalcite in the resin matrix, and help the composite modified hydrotalcite absorb more HCl gas and inhibit the degradation of polyvinyl chloride. The organic anions in the sodium dodecyl sulfate are used to intercalate the silanized hydrotalcite, increase the interlayer distance of the silanized hydrotalcite, and increase the active reaction sites, which can effectively improve the thermal stability and mechanical enhancement of the composite modified hydrotalcite finally prepared. In addition, a large amount of sodium dodecyl sulfate is adsorbed on the surface of the composite modified hydrotalcite, which changes the surface of the composite modified hydrotalcite from hydrophilic to hydrophobic, alleviates the agglomeration phenomenon between the composite modified hydrotalcite, and enhances the interfacial compatibility between the composite modified hydrotalcite and polyvinyl chloride; in addition, the sodium dodecyl sulfate that falls off after the composite modified hydrotalcite structure collapses can also react with HCl.

[0029] Nanocellulose has a high degree of crystallinity and a close network structure formed by physical entanglement between filaments, so that the composite plastic hose prepared from it has extremely high tensile strength. However, nanocellulose has poor elongation at break while having high strength. Using unmodified nanocellulose as a reinforcing filler will not only improve the tensile strength of the resin matrix, but also have an adverse effect on the elongation at break of the resin matrix. To this end, the present invention utilizes the large number of hydroxyl functional groups contained in nanocellulose and the characteristics of being easy to combine with other materials. Based on the performance characteristics of high specific strength and specific modulus, nanocellulose is used as a reinforcing phase to be compounded with polydopamine, thereby improving the tensile strength, bending strength and impact strength of the composite plastic hose of nanocellulose.

[0030] The present invention uses potassium persulfate as an initiator, N,N-methylenebisacrylamide as a cross-linking agent, and nanocellulose as a reinforcement. Through acrylamide monomer free radical polymerization, in the polymerization process, a composite modified nanocellulose is prepared through the electrostatic effect and hydrogen bonding between the modified nanocellulose and acrylamide. The addition of polyacrylamide well makes up for the defect of low elongation at break of nanocellulose. This is because, on the one hand, polyacrylamide is a linear macromolecular compound, which has a variety of active functional groups and can form hydrogen bonds with the modified nanocellulose through affinity adsorption. On the other hand, the cations ionized by polyacrylamide in the aqueous solution are easy to produce strong electrostatic adsorption with a large amount of negative charges in the modified nanocellulose, thereby reducing the spacing between the modified nanocellulose fibrils, making it easier to produce hydrogen bonding, thereby improving the tensile strength of the composite plastic hose. On the other hand, during the in situ polymerization reaction, rigid nanocellulose is used as the first network and flexible dispersed polyacrylamide is used as the second network. Under the action of electrostatics and hydrogen bonds, the modified nanocellulose and polyacrylamide molecular chains penetrate each other to form a stable and dense double-network interpenetrating structure, and finally a composite modified nanocellulose with both high strength and high toughness is prepared.

[0031] The present invention can effectively improve the toughness of the composite plastic hose by adding an appropriate amount of composite modified nanocellulose into the resin matrix. In terms of crystallization behavior, the composite modified nanocellulose plays the role of a heterogeneous nucleating agent in the resin matrix, thereby increasing the nucleation density of the resin matrix, thereby reducing the size of spherulites, while accelerating the crystallization process and reducing the crystallinity of the resin matrix. In terms of interface bonding, the composite modified nanocellulose is hydrogen-bonded with the resin matrix. When a small amount of composite modified nanocellulose is added, the agglomeration phenomenon of the composite modified nanocellulose is not obvious, and many cavities are evenly distributed at the interface with the resin matrix. When the composite plastic hose is impacted by an external force, these tiny cavities help the composite plastic hose absorb impact energy, thereby improving the impact strength of the composite plastic hose.

[0032] As a preferred technical solution of the present invention, in step (I), the particle size of the hydrotalcite powder is 30 to 40 μm, for example, it can be 30 μm, 31 μm, 32 μm, 33 μm, 34 μm, 35 μm, 36 μm, 37 μm, 38 μm, 39 μm or 40 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] In some optional examples, the heating rate of the high-temperature calcination of the hydrotalcite powder is 3 to 5°C / min, for example, it can be 3.0°C / min, 3.2°C / min, 3.4°C / min, 3.6°C / min, 3.8°C / min, 4.0°C / min, 4.2°C / min, 4.4°C / min, 4.6°C / min, 4.8°C / min or 5.0°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] In some optional examples, the heating temperature for high-temperature calcination of the hydrotalcite powder is 500-600°C, for example, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C or 600°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] In some optional examples, the holding time of the high-temperature calcination of the hydrotalcite powder is 5 to 8 hours, for example, it can be 5.0h, 5.2h, 5.4h, 5.6h, 5.8h, 6.0h, 6.2h, 6.4h, 6.6h, 6.8h, 7.0h, 7.2h, 7.4h, 7.6h, 7.8h or 8.0h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] In some optional examples, in the silane coupling agent solution, the ratio of the silane coupling agent to the ethanol aqueous solution is (0.1-0.5) g:1 mL, for example, it can be 0.1 g:1 mL, 0.15 g:1 mL, 0.2 g:1 mL, 0.25 g:1 mL, 0.3 g:1 mL, 0.35 g:1 mL, 0.4 g:1 mL, 0.45 g:1 mL or 0.5 g:1 mL, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] In some optional examples, the mass ratio of the calcined hydrotalcite to the silane coupling agent in the silane coupling agent solution is 1:(0.02-0.03), for example, it can be 1:0.02, 1:0.021, 1:10.022, 1:0.023, 1:0.024, 1:0.025, 1:0.026, 1:0.027, 1:0.028, 1:0.029 or 1:0.03, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] In some optional examples, the heating temperature of the hydrotalcite dispersion is 80-90°C, for example, it can be 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C or 90°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] In some optional examples, the insulation time of the hydrotalcite dispersion is 10 to 20 minutes, for example, it can be 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes, 15 minutes, 16 minutes, 17 minutes, 18 minutes, 19 minutes or 20 minutes, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] As a preferred technical solution of the present invention, in step (I), the concentration of sodium dodecyl sulfate in the sodium dodecyl sulfate solution is 2 to 5 g / L, for example, it can be 2.0 g / L, 2.5 g / L, 3.0 g / L, 3.5 g / L, 4.0 g / L, 4.5 g / L or 5.0 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] In some optional examples, before dispersing the silanized hydrotalcite in the sodium dodecyl sulfate solution, an aqueous ammonia solution is added dropwise to the sodium dodecyl sulfate solution to adjust the pH value of the sodium dodecyl sulfate solution to 8-9, for example, 8.0, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9 or 9.0, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] The present invention specifically limits the pH value of the sodium dodecyl sulfate solution to 8-9. This is because hydrotalcite is weakly alkaline and has a large number of hydroxyl groups in its structure, which are easily neutralized and decomposed in an acidic environment, destroying the layered structure of hydrotalcite and weakening its thermal stability to polyvinyl chloride. When the pH value is higher than 9, it is not conducive to surface modification, and the OH in the solution - Too many ions will affect the modification treatment effect of sodium dodecyl sulfate solution.

[0043] In some optional examples, the mass fraction of the aqueous ammonia solution is 15 to 20 wt%, for example, it can be 15 wt%, 15.5 wt%, 16 wt%, 16.5 wt%, 17 wt%, 17.5 wt%, 18 wt%, 18.5 wt%, 19 wt%, 19.5 wt% or 20 wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] In some optional examples, the ratio of the silanized hydrotalcite to the sodium dodecyl sulfate solution is 1g:(5-8)mL, for example, 1g:5.0mL, 1g:5.5mL, 1g:6.0mL, 1g:6.5mL, 1g:7.0mL, 1g:7.5mL or 1g:8.0mL, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] The present invention specifically limits the ratio of silanized hydrotalcite to sodium dodecyl sulfate solution to 1g: (5-8) mL. As the amount of sodium dodecyl sulfate solution increases, the thermal stability of the composite modified hydrotalcite finally prepared shows a trend of first increasing and then decreasing. This is because when the amount of sodium dodecyl sulfate solution is lower than the lower limit of the range defined by the present invention, sodium dodecyl sulfate cannot be fully wrapped on the surface of the silanized hydrotalcite, so that the improvement of the thermal stability of the silanized hydrotalcite is limited. However, when the amount of sodium dodecyl sulfate solution exceeds the upper limit of the range defined by the present invention, sodium dodecyl sulfate is easy to form a multi-layer physically adsorbed interface thin layer on the surface of the silanized hydrotalcite, thereby affecting the surface properties of the silanized hydrotalcite and causing its thermal stability to decrease.

[0046] In some optional instances, the ultrasonic power used in the ultrasonic dispersion is 500-800 W, for example, it can be 500 W, 520 W, 540 W, 560 W, 580 W, 600 W, 620 W, 640 W, 660 W, 680 W, 700 W, 720 W, 740 W, 760 W, 780 W or 800 W, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0047] In some optional examples, the ultrasonic dispersion time is 30 to 40 min, for example, 30 min, 31 min, 32 min, 33 min, 34 min, 35 min, 36 min, 37 min, 38 min, 39 min or 40 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] As a preferred technical solution of the present invention, in step (II), the concentration of dopamine in the dopamine solution is 1 to 5 g / L, for example, it can be 1.0 g / L, 1.5 g / L, 2.0 g / L, 2.5 g / L, 3.0 g / L, 3.5 g / L, 4.0 g / L, 4.5 g / L or 5.0 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0049] In some optional examples, the concentration of the Tris-hydrochloric acid buffer solution is 30-40 g / L, for example, it can be 30 g / L, 31 g / L, 32 g / L, 33 g / L, 34 g / L, 35 g / L, 36 g / L, 37 g / L, 38 g / L, 39 g / L or 40 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0050] In some optional examples, before immersing the nanocellulose powder in the dopamine solution, an alkali solution is added to the dopamine solution to adjust the pH value of the dopamine solution to 8-9, for example, 8.0, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9 or 9.0, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0051] In some optional examples, the mass ratio of the nanocellulose powder to dopamine in the dopamine solution is (4-5):1, for example, it can be 4.0:1, 4.1:1, 4.2:1, 4.3:1, 4.4:1, 4.5:1, 4.6:1, 4.7:1, 4.8:1, 4.9:1 or 5.0:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0052] In some optional examples, the immersion time of the nanocellulose in the dopamine solution is 12 to 24 hours, for example, it can be 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours or 24 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0053] In some optional examples, the first freeze-drying temperature is -80 to -70°C, for example, it can be -80°C, -79°C, -78°C, -77°C, -76°C, -75°C, -74°C, -73°C, -72°C, -71°C or -70°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0054] In some optional examples, the first freeze-drying time is 12 to 24 hours, for example, it can be 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours or 24 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0055] As a preferred technical solution of the present invention, in step (II), the concentration of acrylamide monomer in the monomer solution is 90-100 g / L, for example, it can be 90 g / L, 91 g / L, 92 g / L, 93 g / L, 94 g / L, 95 g / L, 96 g / L, 97 g / L, 98 g / L, 99 g / L or 100 g / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0056] In some optional examples, the concentration of N,N-methylenebisacrylamide in the monomer solution is 4 to 5 g / L, for example, 4.0 g / L, 4.1 g / L, 4.2 g / L, 4.3 g / L, 4.4 g / L, 4.5 g / L, 4.6 g / L, 4.7 g / L, 4.8 g / L, 4.9 g / L or 5.0 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0057] In some optional examples, the mass ratio of the modified nanocellulose to the acrylamide monomer in the monomer solution is 1:(50-60), for example, it can be 1:50, 1:51, 1:52, 1:53, 1:54, 1:55, 1:56, 1:57, 1:58, 1:59 or 1:60, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0058] In some optional examples, before adding potassium persulfate to the reaction solution, alkaline solution is added dropwise to the reaction solution to adjust the pH value of the reaction solution to 7-8, for example, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9 or 8.0, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0059] In some optional examples, the mass ratio of the potassium persulfate to the acrylamide monomer in the reaction solution is (0.005-0.015):1, for example, it can be 0.005:1, 0.006:1, 0.007:1, 0.008:1, 0.009:1, 0.01:1, 0.011:1, 0.012:1, 0.013:1, 0.014:1 or 0.015:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0060] In some optional examples, the polymerization reaction temperature is 40-50°C, for example, 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C or 50°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0061] In some optional examples, the polymerization reaction time is 6 to 10 hours, for example, it can be 6.0 hours, 6.5 hours, 7.0 hours, 7.5 hours, 8.0 hours, 8.5 hours, 9.0 hours, 9.5 hours or 10.0 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0062] In some optional examples, the second freeze-drying temperature is -30 to -20°C, for example, -30°C, -29°C, -28°C, -27°C, -26°C, -25°C, -24°C, -23°C, -22°C, -21°C or -20°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0063] In some optional examples, the second freeze-drying time is 10 to 20 hours, for example, it can be 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours or 20 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0064] As a preferred technical solution of the present invention, in step (III), the temperature of the high temperature smelting is 160-170°C, for example, it can be 160°C, 161°C, 162°C, 163°C, 164°C, 165°C, 166°C, 167°C, 168°C, 169°C or 170°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0065] In some optional examples, the high temperature smelting time is 10 to 15 minutes, for example, it can be 10 minutes, 10.5 minutes, 11 minutes, 11.5 minutes, 12 minutes, 12.5 minutes, 13 minutes, 13.5 minutes, 14 minutes, 14.5 minutes or 15 minutes, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0066] In some optional examples, the rotation speed of the high-speed stirring is 800-1000 rpm, for example, it can be 800 rpm, 820 rpm, 840 rpm, 860 rpm, 880 rpm, 900 rpm, 920 rpm, 940 rpm, 960 rpm, 980 rpm or 1000 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0067] In some optional examples, the barrel of the screw extruder is divided into a first zone, a second zone, a third zone, a fourth zone and a fifth zone with different temperatures along the material flow direction.

[0068] In some optional examples, the temperature of the first zone is 140-150°C, for example, it can be 140°C, 141°C, 142°C, 143°C, 144°C, 145°C, 146°C, 147°C, 148°C, 149°C or 150°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0069] In some optional examples, the temperature of the second zone is 155-165°C, for example, it can be 155°C, 156°C, 157°C, 158°C, 159°C, 160°C, 161°C, 162°C, 163°C, 164°C or 165°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0070] In some optional examples, the temperature of the third zone is 165-175°C, for example, it can be 165°C, 166°C, 167°C, 168°C, 169°C, 170°C, 171°C, 172°C, 173°C, 174°C or 175°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0071] In some optional instances, the temperature of the fourth zone is 175-185°C, for example, it can be 175°C, 176°C, 177°C, 178°C, 179°C, 180°C, 181°C, 182°C, 183°C, 184°C or 185°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0072] In some optional instances, the temperature of the fifth zone is 170-180°C, for example, it can be 170°C, 171°C, 172°C, 173°C, 174°C, 175°C, 176°C, 177°C, 178°C, 179°C or 180°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0073] In some optional examples, the screw speed of the screw extruder is 100-200 rpm, for example, it can be 100 rpm, 110 rpm, 120 rpm, 130 rpm, 140 rpm, 150 rpm, 160 rpm, 170 rpm, 180 rpm, 190 rpm or 200 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0074] In some optional examples, before injection molding, the plastic masterbatch is dried, and the drying temperature is 80-90°C, for example, it can be 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C or 90°C; the drying time is 8-10h, for example, it can be 8.0h, 8.2h, 8.4h, 8.6h, 8.8h, 9.0h, 9.2h, 9.4h, 9.6h, 9.8h or 10.0h, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0075] In some optional instances, the injection molding temperature of the injection molding machine is 170-180°C, for example, it can be 170°C, 171°C, 172°C, 173°C, 174°C, 175°C, 176°C, 177°C, 178°C, 179°C or 180°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0076] In some optional instances, the injection molding pressure of the injection molding machine is 50-60 MPa, for example, it can be 50 MPa, 51 MPa, 52 MPa, 53 MPa, 54 MPa, 55 MPa, 56 MPa, 57 MPa, 58 MPa, 59 MPa or 60 MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0077] In some optional instances, the holding time of the injection molding machine is 3 to 5 minutes, for example, it can be 3.0 minutes, 3.2 minutes, 3.4 minutes, 3.6 minutes, 3.8 minutes, 4.0 minutes, 4.2 minutes, 4.4 minutes, 4.6 minutes, 4.8 minutes or 5.0 minutes, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0078] In a third aspect, the present invention provides an application of the composite plastic hose described in the first aspect, wherein the composite plastic hose is used for a cosmetic packaging bottle.

[0079] Compared with the prior art, the present invention has the following beneficial effects:

[0080] The present invention can obtain a composite plastic hose with both strength and toughness by adding composite modified hydrotalcite and composite modified nanocellulose into a polyvinyl chloride resin matrix. The present invention calcines, modifies with a silane coupling agent and modifies with sodium dodecyl sulfate the hydrotalcite to achieve intercalation modification of the hydrotalcite, improves the interlayer spacing of the hydrotalcite, can significantly improve the thermal stability of polyvinyl chloride, and prevents the polyvinyl chloride from decomposing during the extrusion process. The present invention modifies the nanocellulose with dopamine, generates polyacrylamide through an in-situ polymerization reaction, constructs a stable and dense double network interpenetrating structure, effectively solves the problem of low elongation at break of the nanocellulose, and obtains a composite modified nanocellulose with high strength and high toughness. BRIEF DESCRIPTION OF THE DRAWINGS

[0081] Figure 1 A process flow chart of the preparation of the composite plastic hose provided in Examples 1-11 of the present invention;

[0082] Figure 2 is the scanning electron microscope image of the unmodified hydrotalcite;

[0083] Figure 3 This is a scanning electron microscope image of the composite modified hydrotalcite prepared in Example 1 of the present invention;

[0084] Figure 4 : are infrared spectra of unmodified hydrotalcite and the composite modified hydrotalcite prepared in Example 1;

[0085] Figure 5 This is a scanning electron microscope image of the composite modified nanocellulose prepared in Example 1 of the present invention;

[0086] Figure 6 The infrared spectra of nanocellulose, polyacrylamide and the composite modified nanocellulose prepared in Example 1 of the present invention are shown. DETAILED DESCRIPTION

[0087] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and their accompanying drawings. The embodiments recorded herein are specific embodiments of the present invention, which are used to illustrate the concept of the present invention; these descriptions are explanatory and exemplary and should not be construed as limitations on the embodiments of the present invention and the scope of protection of the present invention. In addition to the embodiments recorded herein, those skilled in the art can also adopt other obvious technical solutions based on the contents disclosed in the claims of this application and its specification, including technical solutions that adopt any obvious replacements and modifications to the embodiments recorded herein.

[0088] Example 1

[0089] This embodiment provides a method for preparing a composite plastic hose, such as Figure 1As shown, the preparation method specifically comprises the following steps:

[0090] (1) grinding and pulverizing the magnesium-aluminum hydrotalcite to obtain a hydrotalcite powder with a D90 particle size of 30 μm, heating the hydrotalcite powder to 500° C. at a heating rate of 3° C. / min for high-temperature calcination for 8 h to obtain a calcined hydrotalcite;

[0091] The silane coupling agent KH550 and the ethanol aqueous solution are mixed in a ratio of 0.1 g:1 mL to obtain a silane coupling agent solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 9:1; the calcined hydrotalcite is immersed in the silane coupling agent solution to form a hydrotalcite dispersion, the mass ratio of the calcined hydrotalcite to the silane coupling agent KH550 in the silane coupling agent solution is 1:0.02, the hydrotalcite dispersion is heated to 80° C. and kept warm for 20 min, stirred during the heating process to react, and after the reaction is completed, filtered and dried to obtain a silanized hydrotalcite;

[0092] A 15 wt % ammonia solution was added dropwise to the sodium dodecyl sulfate solution to adjust the pH value of the sodium dodecyl sulfate solution to 8, the silanized hydrotalcite was dispersed in the sodium dodecyl sulfate solution with a concentration of 2 g / L, the ratio of the silanized hydrotalcite to the sodium dodecyl sulfate solution was 1 g:5 mL, and ultrasonic dispersion was performed at an ultrasonic power of 500 W for 40 min to obtain a mixed solution, and the mixed solution was filtered and dried to obtain a composite modified hydrotalcite;

[0093] (2) dissolving dopamine in a 30 g / L Tris-hydrochloric acid buffer solution to obtain a 1 g / L dopamine solution, and adding a 15 wt % ammonia solution to the dopamine solution to adjust the pH value of the dopamine solution to 8; soaking the nanocellulose powder in the dopamine solution for 12 h, wherein the mass ratio of the nanocellulose powder to the dopamine in the dopamine solution is 4:1, and then vacuum filtering and first freeze drying to obtain modified nanocellulose, wherein the first freeze drying temperature is -80°C and the first freeze drying time is 12 h;

[0094] acrylamide monomer, N,N-methylenebisacrylamide and deionized water are mixed and stirred to obtain a monomer solution, wherein the concentration of acrylamide monomer in the monomer solution is 90 g / L, and the concentration of N,N-methylenebisacrylamide is 4 g / L; modified nanocellulose is added to the monomer solution, and the mass ratio of the modified nanocellulose to the acrylamide monomer in the monomer solution is 1:50, and the mixture is uniformly mixed to obtain a reaction solution;

[0095] A 15 wt % ammonia solution was added dropwise to the reaction solution to adjust the pH value of the reaction solution to 7, potassium persulfate was added to the reaction solution, the mass ratio of potassium persulfate to acrylamide monomer in the reaction solution was 0.005:1, the mixture was stirred and heated to 40° C. for polymerization reaction for 10 h, and after the reaction, vacuum filtration and second freeze drying were performed to obtain composite modified nanocellulose, wherein the temperature of the second freeze drying was −30° C., and the time of the second freeze drying was 10 h;

[0096] (3) 40 parts of polyvinyl chloride resin (S51649, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 35 parts of acrylic resin (S51652, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 6.5 parts of ethylene-vinyl acetate copolymer (S45075, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 10 parts of the composite modified hydrotalcite obtained in step (1), 2.5 parts of the composite modified nanocellulose obtained in step (2), 5 parts of calcium zinc stabilizer (CF128, purchased from Hubei Chengfeng Chemical Co., Ltd.), 0.5 parts of antioxidant 1010 and 0.5 parts of stearic acid were mixed and put into a mixer, and mixed and melted for 15 minutes at a temperature of 160° C. and a stirring speed of 1000 rpm to obtain a mixed melt;

[0097] The mixed melt is sent into a screw extruder for extrusion granulation to obtain a plastic masterbatch, wherein the temperature of the first zone of the screw extruder is 140° C., the temperature of the second zone is 155° C., the temperature of the third zone is 165° C., the temperature of the fourth zone is 175° C., the temperature of the fifth zone is 170° C., and the screw speed is 100 rpm;

[0098] The plastic masterbatch is dried at a temperature of 80° C. for 10 hours; the dried plastic masterbatch is sent to an injection molding machine for injection molding at a temperature of 170° C., an injection pressure of 60 MPa, and a holding time of 3 minutes, and the composite plastic hose is obtained after cooling.

[0099] Figure 2 and Figure 3 The scanning electron microscope images of the unmodified hydrotalcite and the composite modified hydrotalcite prepared in this example are shown in FIG. Figure 2 and Figure 3 It can be seen that the microscopic morphology of the hydrotalcite before and after modification is basically unchanged, both showing the hexagonal structure of the classic hydroxide, with the layers overlapping and a width of about 50 to 100 nm. However, the particles of the unmodified hydrotalcite are smaller and the agglomeration phenomenon is more obvious. The agglomeration phenomenon of the composite modified hydrotalcite prepared in Example 1 has been improved to a certain extent, and the dispersibility is better. This is because the silane coupling agent and sodium dodecyl sulfate are adsorbed on the surface of the hydrotalcite, which changes its hydrophilicity to hydrophobicity and makes it easier to disperse.

[0100] Figure 4 is the infrared spectrum of the unmodified hydrotalcite and the composite modified hydrotalcite prepared in this example. Figure 4 It can be seen that the infrared spectra of unmodified hydrotalcite and composite modified hydrotalcite are both between 3400 and 3500 cm -1 The -OH stretching vibration peak appeared at 1360 cm -1 CO3 appeared 2- However, unlike the unmodified hydrotalcite, the infrared spectrum curve of the composite modified hydrotalcite is at 2800-2900cm -1 The stretching vibration absorption peaks of -CH3 and -CH2- appeared at 1100cm -1 SO4 appears nearby 2- This shows that sodium dodecyl sulfate has successfully modified the surface of hydrotalcite by adsorption.

[0101] Figure 5 This is a scanning electron microscope image of the composite modified nanocellulose prepared in this example. It can be seen from the image that a double interpenetrating porous network structure is formed inside the composite modified nanocellulose, which is beneficial to improving the bending strength and impact strength of the composite plastic hose.

[0102] Figure 6 The infrared spectra of nanocellulose, polyacrylamide and the composite modified nanocellulose prepared in this embodiment are shown in Figure 2. From the infrared spectrum curve of nanocellulose, it can be seen that 3443cm -1 The stretching vibration peak of OH is at 2892 cm -1 The peak at 3190cm is the stretching vibration peak of the CH bond. -1 The stretching vibration peak of amino group is 1673cm -1 The absorption peak of the carbonyl group in the amide group is 1613 cm -1 The NH bending vibration peak is at 1720cm. From the infrared spectrum curve of the composite modified nanocellulose, it can be seen that the composite modified nanocellulose retains the characteristic peak of nanocellulose and has a -1 、1665cm -1 and 1611cm -1 Three new characteristic absorption peaks appeared at 1162 cm-1, which were attributed to the asymmetric stretching vibration of the -CONH2 functional group of the polyacrylamide main chain, indicating that polyacrylamide was successfully grafted onto the nanocellulose main chain. -1 The absorption peak at is the stretching vibration peak of COC, which indicates that more COC functional groups are formed when polyacrylamide is grafted onto the main chain of nanocellulose.

[0103] Example 2

[0104] This embodiment provides a method for preparing a composite plastic hose, such as Figure 1 As shown, the preparation method specifically comprises the following steps:

[0105] (1) grinding and pulverizing the magnesium aluminum hydrotalcite to obtain a hydrotalcite powder with a D90 particle size of 32 μm, heating the hydrotalcite powder to 520° C. at a heating rate of 3.5° C. / min for high temperature calcination for 7 h to obtain a calcined hydrotalcite;

[0106] The silane coupling agent KH550 and the ethanol aqueous solution are mixed in a ratio of 0.2 g:1 mL to obtain a silane coupling agent solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 9:1; the calcined hydrotalcite is immersed in the silane coupling agent solution to form a hydrotalcite dispersion, the mass ratio of the calcined hydrotalcite to the silane coupling agent KH550 in the silane coupling agent solution is 1:0.022, the hydrotalcite dispersion is heated to 82° C. and kept warm for 18 min, stirred during the heating process to react, and after the reaction is completed, filtered and dried to obtain a silanized hydrotalcite;

[0107] A 16 wt % ammonia solution was added dropwise to the sodium dodecyl sulfate solution to adjust the pH value of the sodium dodecyl sulfate solution to 8.2, the silanized hydrotalcite was dispersed in the sodium dodecyl sulfate solution with a concentration of 3 g / L, the ratio of the silanized hydrotalcite to the sodium dodecyl sulfate solution was 1 g:6 mL, and ultrasonic dispersion was performed at an ultrasonic power of 600 W for 38 min to obtain a mixed solution, and the mixed solution was filtered and dried to obtain a composite modified hydrotalcite;

[0108] (2) dissolving dopamine in a Tris-hydrochloric acid buffer solution having a concentration of 32 g / L to obtain a dopamine solution having a concentration of 2 g / L, and adding a 16 wt % ammonia solution to the dopamine solution to adjust the pH value of the dopamine solution to 8.2; soaking the nanocellulose powder in the dopamine solution for 15 h, wherein the mass ratio of the nanocellulose powder to the dopamine in the dopamine solution is 4.2:1, and then vacuum filtering and first freeze drying to obtain modified nanocellulose, wherein the first freeze drying temperature is -78°C and the first freeze drying time is 15 h;

[0109] acrylamide monomer, N,N-methylenebisacrylamide and deionized water are mixed and stirred to obtain a monomer solution, wherein the concentration of acrylamide monomer in the monomer solution is 92 g / L, and the concentration of N,N-methylenebisacrylamide is 4.2 g / L; modified nanocellulose is added to the monomer solution, and the mass ratio of the modified nanocellulose to the acrylamide monomer in the monomer solution is 1:52, and the mixture is uniformly mixed to obtain a reaction solution;

[0110] A 16 wt % ammonia solution was added dropwise to the reaction solution to adjust the pH value of the reaction solution to 7.2, potassium persulfate was added to the reaction solution, the mass ratio of potassium persulfate to acrylamide monomer in the reaction solution was 0.008:1, the mixture was mixed and stirred and heated to 42° C. for polymerization for 9 h, and after the reaction was completed, vacuum filtration and a second freeze drying were performed to obtain composite modified nanocellulose, wherein the second freeze drying temperature was −28° C. and the second freeze drying time was 12 h;

[0111] (3) 40 parts of polyvinyl chloride resin (S51649, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 33 parts of acrylic resin (S51652, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 8 parts of ethylene-vinyl acetate copolymer (S45075, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 12 parts of the composite modified hydrotalcite obtained in step (1), 3 parts of the composite modified nanocellulose obtained in step (2), 3.3 parts of calcium zinc stabilizer (CF128, purchased from Hubei Chengfeng Chemical Co., Ltd.), 0.1 parts of antioxidant 1076 and 0.6 parts of stearic acid were mixed and put into a mixer, and mixed and melted at a temperature of 162° C. and a stirring condition of 950 rpm for 13 min to obtain a mixed melt;

[0112] The mixed melt is sent into a screw extruder for extrusion granulation to obtain a plastic masterbatch, wherein the temperature of the first zone of the screw extruder is 142° C., the temperature of the second zone is 158° C., the temperature of the third zone is 168° C., the temperature of the fourth zone is 178° C., the temperature of the fifth zone is 172° C., and the screw speed is 120 rpm;

[0113] The plastic masterbatch is dried at a temperature of 82° C. and a drying time of 9.5 h. The dried plastic masterbatch is sent to an injection molding machine for injection molding at a temperature of 172° C., an injection pressure of 58 MPa, and a holding time of 3.5 min. After cooling, the composite plastic hose is obtained.

[0114] Example 3

[0115] This embodiment provides a method for preparing a composite plastic hose, such as Figure 1 As shown, the preparation method specifically comprises the following steps:

[0116] (1) pulverizing and grinding the magnesium aluminum hydrotalcite to obtain a hydrotalcite powder with a D90 particle size of 35 μm, heating the hydrotalcite powder to 550° C. at a heating rate of 4° C. / min for high-temperature calcination for 7 h to obtain a calcined hydrotalcite;

[0117] The silane coupling agent KH550 and the ethanol aqueous solution are mixed in a ratio of 0.3 g:1 mL to obtain a silane coupling agent solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 9:1; the calcined hydrotalcite is immersed in the silane coupling agent solution to form a hydrotalcite dispersion, the mass ratio of the calcined hydrotalcite to the silane coupling agent KH550 in the silane coupling agent solution is 1:0.025, the hydrotalcite dispersion is heated to 85° C. and kept warm for 15 min, stirred during the heating process to react, and after the reaction is completed, filtered and dried to obtain a silanized hydrotalcite;

[0118] A 17 wt % ammonia solution was added dropwise to the sodium dodecyl sulfate solution to adjust the pH value of the sodium dodecyl sulfate solution to 8.5, the silanized hydrotalcite was dispersed in the sodium dodecyl sulfate solution with a concentration of 4 g / L, the ratio of the silanized hydrotalcite to the sodium dodecyl sulfate solution was 1 g:6 mL, and ultrasonic dispersion was performed at an ultrasonic power of 600 W for 35 min to obtain a mixed solution, and the mixed solution was filtered and dried to obtain a composite modified hydrotalcite;

[0119] (2) dissolving dopamine in a 35 g / L Tris-hydrochloric acid buffer solution to obtain a 3 g / L dopamine solution, and adding a 17 wt % ammonia solution to the dopamine solution to adjust the pH value of the dopamine solution to 8.5; soaking the nanocellulose powder in the dopamine solution for 20 h, wherein the mass ratio of the nanocellulose powder to the dopamine in the dopamine solution is 4.5:1, and then vacuum filtering and first freeze drying to obtain modified nanocellulose, wherein the first freeze drying temperature is -75°C and the first freeze drying time is 20 h;

[0120] acrylamide monomer, N,N-methylenebisacrylamide and deionized water are mixed and stirred to obtain a monomer solution, wherein the concentration of acrylamide monomer in the monomer solution is 95 g / L, and the concentration of N,N-methylenebisacrylamide is 4.5 g / L; modified nanocellulose is added to the monomer solution, and the mass ratio of the modified nanocellulose to the acrylamide monomer in the monomer solution is 1:55, and the mixture is uniformly mixed to obtain a reaction solution;

[0121] A 17 wt % ammonia solution was added dropwise to the reaction solution to adjust the pH value of the reaction solution to 7.5, potassium persulfate was added to the reaction solution, the mass ratio of potassium persulfate to acrylamide monomer in the reaction solution was 0.01:1, the mixture was mixed and stirred and heated to 45° C. for polymerization reaction for 8 h, and after the reaction, vacuum filtration and second freeze drying were performed to obtain composite modified nanocellulose, wherein the temperature of the second freeze drying was −25° C., and the time of the second freeze drying was 15 h;

[0122] (3) 45 parts of polyvinyl chloride resin (S51649, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 35 parts of acrylic resin (S51652, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 5 parts of ethylene-vinyl acetate copolymer (S45075, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 11 parts of the composite modified hydrotalcite obtained in step (1), 2 parts of the composite modified nanocellulose obtained in step (2), 1 part of calcium zinc stabilizer (CF128, purchased from Hubei Chengfeng Chemical Co., Ltd.), 0.3 parts of antioxidant 626 and 0.7 parts of zinc stearate were mixed and put into a mixer, and mixed and melted for 12 minutes at a temperature of 165° C. and a stirring condition of 900 rpm to obtain a mixed melt;

[0123] The mixed melt is sent into a screw extruder for extrusion granulation to obtain a plastic masterbatch, wherein the temperature of the first zone of the screw extruder is 145° C., the temperature of the second zone is 160° C., the temperature of the third zone is 170° C., the temperature of the fourth zone is 180° C., the temperature of the fifth zone is 175° C., and the screw speed is 150 rpm;

[0124] The plastic masterbatch is dried at a temperature of 85° C. and a drying time of 9 hours; the dried plastic masterbatch is sent to an injection molding machine for injection molding at an injection molding temperature of 175° C., an injection molding pressure of 55 MPa, and a holding time of 4 minutes, and the composite plastic hose is obtained after cooling.

[0125] Example 4

[0126] This embodiment provides a method for preparing a composite plastic hose, such as Figure 1 As shown, the preparation method specifically comprises the following steps:

[0127] (1) grinding and pulverizing the magnesium-aluminum hydrotalcite to obtain a hydrotalcite powder with a D90 particle size of 338 μm, heating the hydrotalcite powder to 580° C. at a heating rate of 4.5° C. / min for high-temperature calcination for 6 h to obtain a calcined hydrotalcite;

[0128] The silane coupling agent KH550 and the ethanol aqueous solution are mixed in a ratio of 0.4 g:1 mL to obtain a silane coupling agent solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 9:1; the calcined hydrotalcite is immersed in the silane coupling agent solution to form a hydrotalcite dispersion, the mass ratio of the calcined hydrotalcite to the silane coupling agent KH550 in the silane coupling agent solution is 1:0.028, the hydrotalcite dispersion is heated to 88° C. and kept warm for 12 minutes, stirred during the heating process to react, and after the reaction is completed, filtered and dried to obtain a silanized hydrotalcite;

[0129] 18 wt % ammonia solution was added dropwise to the sodium dodecyl sulfate solution to adjust the pH value of the sodium dodecyl sulfate solution to 8.8, the silanized hydrotalcite was dispersed in the sodium dodecyl sulfate solution with a concentration of 4 g / L, the ratio of the silanized hydrotalcite to the sodium dodecyl sulfate solution was 1 g:7 mL, ultrasonic dispersion was performed at an ultrasonic power of 700 W for 32 min to obtain a mixed solution, and the mixed solution was filtered and dried to obtain a composite modified hydrotalcite;

[0130] (2) dissolving dopamine in a Tris-hydrochloric acid buffer solution having a concentration of 38 g / L to obtain a dopamine solution having a concentration of 4 g / L, and adding 18 wt % ammonia solution to the dopamine solution to adjust the pH value of the dopamine solution to 8.8; soaking the nanocellulose powder in the dopamine solution for 22 hours, wherein the mass ratio of the nanocellulose powder to the dopamine in the dopamine solution is 4.8:1, and then vacuum filtering and first freeze drying to obtain modified nanocellulose, wherein the first freeze drying temperature is -72°C and the first freeze drying time is 22 hours;

[0131] acrylamide monomer, N,N-methylenebisacrylamide and deionized water are mixed and stirred to obtain a monomer solution, wherein the concentration of acrylamide monomer in the monomer solution is 98 g / L, and the concentration of N,N-methylenebisacrylamide is 4.8 g / L; modified nanocellulose is added to the monomer solution, and the mass ratio of the modified nanocellulose to the acrylamide monomer in the monomer solution is 1:58, and the mixture is uniformly mixed to obtain a reaction solution;

[0132] 18 wt % ammonia solution was added dropwise to the reaction solution to adjust the pH value of the reaction solution to 7.8, potassium persulfate was added to the reaction solution, the mass ratio of potassium persulfate to acrylamide monomer in the reaction solution was 0.012:1, mixed and stirred and heated to 48° C. for polymerization reaction for 7 h, and after the reaction was completed, vacuum filtration and second freeze drying were performed to obtain composite modified nanocellulose, wherein the temperature of the second freeze drying was -22° C., and the time of the second freeze drying was 18 h;

[0133] (3) 48 parts of polyvinyl chloride resin (S51649, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 32 parts of acrylic resin (S51652, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 5 parts of ethylene-vinyl acetate copolymer (S45075, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 10 parts of the composite modified hydrotalcite obtained in step (1), 2.2 parts of the composite modified nanocellulose obtained in step (2), 1.6 parts of calcium zinc stabilizer (CF128, purchased from Hubei Chengfeng Chemical Co., Ltd.), 0.4 parts of antioxidant 168 and 0.8 parts of calcium stearate were mixed and put into a mixer, and mixed and melted at a temperature of 168° C. and a stirring condition of 850 rpm for 11 minutes to obtain a mixed melt;

[0134] The mixed melt is sent into a screw extruder for extrusion granulation to obtain a plastic masterbatch, wherein the temperature of the first zone of the screw extruder is 148° C., the temperature of the second zone is 162° C., the temperature of the third zone is 172° C., the temperature of the fourth zone is 182° C., the temperature of the fifth zone is 178° C., and the screw speed is 180 rpm;

[0135] The plastic masterbatch is dried at a temperature of 88° C. and a drying time of 8.5 h. The dried plastic masterbatch is sent to an injection molding machine for injection molding at a temperature of 178° C., an injection pressure of 52 MPa, and a holding time of 4.5 min. After cooling, the composite plastic hose is obtained.

[0136] Example 5

[0137] This embodiment provides a method for preparing a composite plastic hose, such as Figure 1 As shown, the preparation method specifically comprises the following steps:

[0138] (1) grinding and pulverizing the magnesium aluminum hydrotalcite to obtain a hydrotalcite powder with a D90 particle size of 40 μm, heating the hydrotalcite powder to 600° C. at a heating rate of 3° C. / min for high temperature calcination for 5 h to obtain a calcined hydrotalcite;

[0139] The silane coupling agent KH550 and the ethanol aqueous solution are mixed in a ratio of 0.5 g:1 mL to obtain a silane coupling agent solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 9:1; the calcined hydrotalcite is immersed in the silane coupling agent solution to form a hydrotalcite dispersion, the mass ratio of the calcined hydrotalcite to the silane coupling agent KH550 in the silane coupling agent solution is 1:0.03, the hydrotalcite dispersion is heated to 90° C. and kept warm for 10 min, stirred during the heating process to react, and after the reaction is completed, filtered and dried to obtain a silanized hydrotalcite;

[0140] Add 20 wt % ammonia solution dropwise to the sodium dodecyl sulfate solution to adjust the pH value of the sodium dodecyl sulfate solution to 9, disperse the silanized hydrotalcite in the sodium dodecyl sulfate solution with a concentration of 5 g / L, the ratio of the silanized hydrotalcite to the sodium dodecyl sulfate solution is 1 g:8 mL, ultrasonic dispersion is performed at an ultrasonic power of 800 W for 30 min to obtain a mixed solution, and the mixed solution is filtered and dried to obtain a composite modified hydrotalcite;

[0141] (2) dissolving dopamine in a 40 g / L Tris-hydrochloric acid buffer solution to obtain a 5 g / L dopamine solution, and adding a 20 wt % ammonia solution to the dopamine solution to adjust the pH value of the dopamine solution to 9; soaking the nanocellulose powder in the dopamine solution for 24 hours, wherein the mass ratio of the nanocellulose powder to the dopamine in the dopamine solution is 5:1, and then vacuum filtering and first freeze drying to obtain modified nanocellulose, wherein the first freeze drying temperature is -70°C and the first freeze drying time is 24 hours;

[0142] acrylamide monomer, N,N-methylenebisacrylamide and deionized water are mixed and stirred to obtain a monomer solution, wherein the concentration of acrylamide monomer in the monomer solution is 100 g / L, and the concentration of N,N-methylenebisacrylamide is 5 g / L; modified nanocellulose is added to the monomer solution, and the mass ratio of the modified nanocellulose to the acrylamide monomer in the monomer solution is 1:60, and the mixture is uniformly mixed to obtain a reaction solution;

[0143] A 20 wt % ammonia solution was added dropwise to the reaction solution to adjust the pH value of the reaction solution to 8, potassium persulfate was added to the reaction solution, the mass ratio of potassium persulfate to acrylamide monomer in the reaction solution was 0.015:1, the mixture was mixed and stirred and heated to 50° C. for polymerization reaction for 6 h, and after the reaction, vacuum filtration and second freeze drying were performed to obtain composite modified nanocellulose, wherein the second freeze drying temperature was -20° C. and the second freeze drying time was 20 h;

[0144] (3) 50 parts of polyvinyl chloride resin (S51649, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 30 parts of acrylic resin (S51652, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 5 parts of ethylene-vinyl acetate copolymer (S45075, purchased from Shanghai Yuanye Biotechnology Co., Ltd.), 10 parts of the composite modified hydrotalcite obtained in step (1), 2 parts of the composite modified nanocellulose obtained in step (2), 1.9 parts of calcium zinc stabilizer (CF128, purchased from Hubei Chengfeng Chemical Co., Ltd.), 0.1 parts of antioxidant DLTP and 1 part of polyethylene wax were mixed and put into a mixer, and mixed and melted for 10 minutes at a temperature of 170° C. and a stirring condition of 800 rpm to obtain a mixed melt;

[0145] The mixed melt is sent into a screw extruder for extrusion granulation to obtain a plastic masterbatch, wherein the temperature of the first zone of the screw extruder is 150° C., the temperature of the second zone is 165° C., the temperature of the third zone is 175° C., the temperature of the fourth zone is 185° C., the temperature of the fifth zone is 180° C., and the screw speed is 200 rpm;

[0146] The plastic masterbatch is dried at a temperature of 90° C. and a drying time of 8 hours; the dried plastic masterbatch is sent to an injection molding machine for injection molding at an injection molding temperature of 180° C., an injection molding pressure of 50 MPa, and a holding time of 5 minutes, and the composite plastic hose is obtained after cooling.

[0147] Example 6

[0148] This embodiment provides a method for preparing a composite plastic hose, which differs from Embodiment 1 in that, in step (1), the ratio of silylated hydrotalcite to sodium dodecyl sulfate solution is adjusted to 1 g:3 mL, and other process parameters and operation steps are exactly the same as those in Embodiment 1.

[0149] Example 7

[0150] This embodiment provides a method for preparing a composite plastic hose, which differs from Embodiment 1 in that, in step (1), the ratio of silanized hydrotalcite to sodium dodecyl sulfate solution is adjusted to 1 g:10 mL, and other process parameters and operation steps are exactly the same as those in Embodiment 1.

[0151] Example 8

[0152] This embodiment provides a method for preparing a composite plastic hose, which is different from Embodiment 1 in that in step (3), the weight of the composite modified hydrotalcite is adjusted to 8 parts, and the other process parameters and operation steps are exactly the same as those in Embodiment 1.

[0153] Example 9

[0154] This embodiment provides a method for preparing a composite plastic hose, which differs from Embodiment 1 in that in step (3), the weight portion of the composite modified hydrotalcite is adjusted to 15 parts, and the other process parameters and operation steps are exactly the same as those in Embodiment 1.

[0155] Example 10

[0156] This embodiment provides a method for preparing a composite plastic hose, which differs from Embodiment 1 in that, in step (3), the weight portion of the composite modified nanocellulose is adjusted to 1 part, and the other process parameters and operation steps are exactly the same as those in Embodiment 1.

[0157] Embodiment 11

[0158] This embodiment provides a method for preparing a composite plastic hose, which differs from Embodiment 1 in that, in step (3), the weight portion of the composite modified nanocellulose is adjusted to 4 parts, and the other process parameters and operation steps are exactly the same as those in Embodiment 1.

[0159] Comparative Example 1

[0160] This comparative example provides a method for preparing a composite plastic hose, which differs from Example 1 in that step (1) is omitted, and in step (3) the composite modified hydrotalcite is replaced by unmodified hydrotalcite, and other process parameters and operation steps are exactly the same as those in Example 1.

[0161] Comparative Example 2

[0162] This comparative example provides a method for preparing a composite plastic hose, which differs from Example 1 in that step (2) is omitted, and in step (3) the composite modified nanocellulose is replaced by unmodified nanocellulose, and other process parameters and operating steps are exactly the same as those in Example 1.

[0163] The tensile strength, bending strength and impact strength of the composite plastic hoses prepared in Examples 1-11 and Comparative Examples 1-2 were tested, and the specific test steps are as follows:

[0164] (1) Tensile strength test

[0165] The tensile properties of plastics are an important indicator for measuring the performance of plastic products and one of the most basic and important properties of plastic mechanical properties. The tensile strength is the maximum tensile stress that the spline can withstand when it is subjected to tension until it breaks. The greater the tensile strength, the stronger and tougher the material, and the better the performance.

[0166] According to the national standard GB / T1040-2006, the dumbbell-shaped standard spline made by injection molding is stretched at a speed of 5mm / min. The calculation formula is as follows:

[0167]

[0168] In the formula, σ t is the tensile strength (MPa), P is the maximum load (N), b is the strip width (mm), and d is the strip thickness (mm).

[0169] (2) Bending strength test

[0170] The bending test is mainly used to test the performance of materials under bending load. In engineering, bending tests are often used to evaluate the bending performance and plastic deformation of materials. According to the national standard GB / T9341-2000, the standard spline made by injection molding is used at a speed of 5mm / min. The calculation formula is as follows:

[0171]

[0172] In the formula, σ f is the bending strength (MPa), F is the applied force (N), l is the span (mm), b is the spline width (mm), and d is the spline thickness (mm).

[0173] (3) Impact strength test

[0174] Impact performance test refers to the impact strength of materials measured under the action of impact load. Impact strength is used to evaluate the ability of materials to resist impact or to judge the brittleness or toughness of materials. It reflects the ability of different materials to resist high-speed impact. The cantilever beam impact test is a common test method to measure the brittleness or toughness of materials. The spline notch impact strength refers to the ratio of the energy absorbed by the notch test during the cantilever beam impact destruction process to the original cross-sectional area of ​​the spline notch. According to the national standard GB / T1843-1996, the standard splines made by injection molding are: length 80±2mm, thickness 10±0.2mm, width 4±0.2mm, V-notch depth 2mm, notch bottom radius 0.25±0.05mm. The calculation formula is as follows:

[0175]

[0176] In the formula, α iN is the notched impact strength (KJ / m 2 ), W is the capacity absorbed by the damaged spline after correction (J), d is the spline thickness (mm), b n is the remaining width at the bottom of the spline notch (mm).

[0177] The test results are shown in Table 1.

[0178] Table 1

[0179]

[0180]

[0181] It can be seen from the test data provided in Table 1 that the tensile strength, elongation at break and impact strength of the composite plastic hoses prepared in Examples 1-5 are higher than those in Examples 6-11, and significantly higher than those in Comparative Examples 1 and 2, which indicates that the preparation method provided by the present invention greatly improves the tensile strength, elongation at break and impact strength of the composite matrix by incorporating a suitable proportion of composite modified hydrotalcite and a suitable proportion of composite modified nanocellulose into the resin matrix.

[0182] It can be seen from the test data provided by Examples 1, 6 and 7 that the tensile strength, elongation at break and impact strength of the composite plastic hoses prepared in Examples 6 and 7 are lower than those in Example 1. This is because the amount of sodium dodecyl sulfate solution used in Example 6 is too low, while the amount of sodium dodecyl sulfate solution used in Example 7 is too high, which affects the tensile strength, elongation at break and impact strength of the composite plastic hose.

[0183] It can be seen from the test data provided by Examples 1, 8 and 9 that the tensile strength, elongation at break and impact strength of the composite plastic hoses prepared in Examples 8 and 9 are lower than those in Example 1. This is because the amount of composite modified hydrotalcite added in Example 8 is too low, while the amount of composite modified hydrotalcite added in Example 9 is too high, which affects the tensile strength, elongation at break and impact strength of the composite plastic hose.

[0184] It can be seen from the test data provided by Example 1, Example 10 and Example 11 that the tensile strength, elongation at break and impact strength of the composite plastic hoses prepared in Example 10 and Example 11 are lower than those in Example 1. This is because the amount of composite modified nanocellulose added in Example 10 is too low, while the amount of composite modified nanocellulose added in Example 11 is too high, which affects the tensile strength, elongation at break and impact strength of the composite plastic hose.

[0185] It can be seen from the test data provided by Example 1 and Comparative Example 1 that the tensile strength, elongation at break and impact strength of the composite plastic hose prepared in Comparative Example 1 are significantly lower than those in Example 1. This is because the hydrotalcite was not modified in Comparative Example 1, which affected the uniformity of the dispersion of the hydrotalcite in the resin matrix, making it easy for the hydrotalcite to agglomerate in the resin matrix, affecting the tensile strength, elongation at break and impact strength of the composite plastic hose.

[0186] It can be seen from the test data provided by Example 1 and Comparative Example 2 that the tensile strength, elongation at break and impact strength of the composite plastic hose prepared in Comparative Example 2 are significantly lower than those in Example 1. This is because the nanocellulose was not modified in Comparative Example 2, which affected the uniformity of the dispersion of the nanocellulose in the resin matrix, making it easy for the nanocellulose to agglomerate in the resin matrix, affecting the tensile strength, elongation at break and impact strength of the composite plastic hose.

[0187] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A composite plastic hose, characterized in that: The composite plastic hose comprises polyvinyl chloride resin, acrylic resin, ethylene-vinyl acetate copolymer, composite modified hydrotalcite, composite modified nanocellulose, stabilizer, antioxidant and lubricant; The modified hydrotalcite is obtained by sequentially calcining, modifying with a silane coupling agent and modifying with sodium dodecyl sulfate. The composite modified nanocellulose is a double interpenetrating network structure composed of nanocellulose and polyacrylamide. The surface of the nanocellulose is coated with a polydopamine layer, and the polyacrylamide is obtained by in-situ polymerization of acrylamide monomers.

2. The composite plastic hose according to claim 1, characterized in that: The composite plastic hose comprises the following components in parts by weight:

3. The composite plastic hose according to claim 1, characterized in that: The stabilizer is a calcium zinc stabilizer; The antioxidant includes any one of antioxidant 1010, antioxidant 1076, antioxidant 626, antioxidant 168 or antioxidant DLTP, or a combination of at least two thereof; The lubricant includes any one of stearic acid, zinc stearate, calcium stearate, and polyethylene wax, or a combination of at least two of them.

4. A method for preparing a composite plastic hose according to any one of claims 1 to 3, characterized in that: The preparation method comprises: (I) grinding and crushing hydrotalcite to obtain hydrotalcite powder, calcining the hydrotalcite powder at high temperature to obtain calcined hydrotalcite; mixing a silane coupling agent with an ethanol aqueous solution to obtain a silane coupling agent solution, immersing the calcined hydrotalcite in the silane coupling agent solution to form a hydrotalcite dispersion, heating and stirring the hydrotalcite dispersion to react, filtering and drying after the reaction to obtain silanized hydrotalcite; dispersing the silanized hydrotalcite in a sodium dodecyl sulfate solution, dispersing the mixture by ultrasonication to obtain a mixed solution, filtering and drying the mixed solution to obtain a composite modified hydrotalcite; (II) dissolving dopamine in a Tris-hydrochloric acid buffer solution to obtain a dopamine solution, soaking the nanocellulose powder in the dopamine solution for a period of time, and then vacuum filtering and first freeze drying to obtain modified nanocellulose; mixing acrylamide monomer, N,N-methylenebisacrylamide and deionized water to obtain a monomer solution, adding the modified nanocellulose to the monomer solution, mixing evenly to obtain a reaction solution, adding potassium persulfate to the reaction solution, mixing and heating to cause a polymerization reaction, and after the reaction is completed, vacuum filtering and second freeze drying to obtain composite modified nanocellulose; (III) mixing polyvinyl chloride resin, acrylic resin, ethylene-vinyl acetate copolymer, the composite modified hydrotalcite obtained in step (I), the composite modified nanocellulose obtained in step (II), a stabilizer, an antioxidant and a lubricant, and then putting them into a mixer for high-temperature melting and high-speed stirring to obtain a mixed melt; sending the mixed melt into a screw extruder for extrusion granulation to obtain a plastic masterbatch; sending the plastic masterbatch into an injection molding machine for injection molding, and obtaining the composite plastic hose after cooling.

5. The preparation method according to claim 4, characterized in that: In step (I), the particle size of the hydrotalcite powder is 30 to 40 μm; The heating rate of the high-temperature calcination of the hydrotalcite powder is 3 to 5°C / min; The heating temperature of the high-temperature calcination of the hydrotalcite powder is 500-600°C; The high temperature calcination holding time of the hydrotalcite powder is 5 to 8 hours; In the silane coupling agent solution, the ratio of the silane coupling agent to the ethanol aqueous solution is (0.1-0.5) g:1 mL; The mass ratio of the calcined hydrotalcite to the silane coupling agent in the silane coupling agent solution is 1:(0.02-0.03); The heating temperature of the hydrotalcite dispersion is 80-90°C; The heat preservation time of the hydrotalcite dispersion is 10 to 20 minutes.

6. The preparation method according to claim 4, characterized in that: In step (I), the concentration of sodium dodecyl sulfate in the sodium dodecyl sulfate solution is 2 to 5 g / L; Before dispersing the silanized hydrotalcite in the sodium dodecyl sulfate solution, adding an aqueous ammonia solution dropwise to the sodium dodecyl sulfate solution to adjust the pH value of the sodium dodecyl sulfate solution to 8 to 9; The mass fraction of the ammonia solution is 15-20wt%; The ratio of the silanized hydrotalcite to the sodium dodecyl sulfate solution is 1 g: (5-8) mL; The ultrasonic power used in the ultrasonic dispersion is 500-800W; The ultrasonic dispersion time is 30 to 40 minutes.

7. The preparation method according to claim 4, characterized in that: In step (II), the concentration of dopamine in the dopamine solution is 1 to 5 g / L; The concentration of the Tris-hydrochloric acid buffer solution is 30-40 g / L; Before soaking the nanocellulose powder in the dopamine solution, adding an alkali solution to the dopamine solution to adjust the pH value of the dopamine solution to 8-9; The mass ratio of the nanocellulose powder to the dopamine in the dopamine solution is (4-5):1; The nanocellulose is immersed in the dopamine solution for 12 to 24 hours; The first freeze-drying temperature is -80 to -70°C; The first freeze-drying time is 12 to 24 hours.

8. The preparation method according to claim 4, characterized in that: In step (II), the concentration of acrylamide monomer in the monomer solution is 90-100 g / L; The concentration of N,N-methylenebisacrylamide in the monomer solution is 4 to 5 g / L; The mass ratio of the modified nanocellulose to the acrylamide monomer in the monomer solution is 1:(50-60); Before adding potassium persulfate to the reaction solution, adding alkali solution dropwise to the reaction solution to adjust the pH value of the reaction solution to 7-8; The mass ratio of the potassium persulfate to the acrylamide monomer in the reaction solution is (0.005-0.015):1; The polymerization reaction temperature is 40-50°C; The polymerization reaction time is 6 to 10 hours; The second freeze drying temperature is -30 to -20°C; The second freeze-drying time is 10 to 20 hours.

9. The preparation method according to claim 4, characterized in that: In step (III), the high temperature smelting temperature is 160-170°C; The high temperature smelting time is 10 to 15 minutes; The rotation speed of the high-speed stirring is 800-1000 rpm; The barrel of the screw extruder is divided into a first zone, a second zone, a third zone, a fourth zone and a fifth zone with different temperatures along the material flow direction; The temperature of the first zone is 140-150°C; The temperature of the second zone is 155-165°C; The temperature of the third zone is 165-175°C; The temperature of the fourth zone is 175-185°C; The temperature of the fifth zone is 170-180°C; The screw speed of the screw extruder is 100-200 rpm; Before injection molding, the plastic masterbatch is dried at a temperature of 80 to 90° C. and a drying time of 8 to 10 hours; The injection molding temperature of the injection molding machine is 170-180°C; The injection molding pressure of the injection molding machine is 50-60MPa; The pressure holding time of the injection molding machine is 3 to 5 minutes.

10. Use of the composite plastic hose according to any one of claims 1 to 3, characterized in that: The composite plastic hose is used for cosmetic packaging bottles.

Citation Information

Cited By

  • Heat-resistant polyethylene composite packaging film and preparation method thereof

    CN119974717A

  • Polypropylene composition as well as preparation method and application thereof

    CN121086399A

  • Preparation process of heat-seal type seedling pot paper with controllable degradation speed

    CN122812114A

  • A process for preparing heat-sealed seedling pot paper with controllable degradation rate

    CN122812114B