Spinel structure high-temperature-resistant aerogel thermal insulation material and preparation method thereof
By using zirconia nanofiber membrane and hydrothermal reaction technology in magnesium-aluminum spinel aerogel materials, the spinel structure is formed, and the problem of insufficient temperature resistance of oxide aerogels in high temperature environments is solved, and the Low thermal conductivity and high strength of materials at high temperatures.
Patent Information
- Application Number
- CN202410945695.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
AI Technical Summary
The existing oxide aerogel materials are insufficient in high temperature environments, especially the melting point of silicon oxide and alumina aerogels are low and have poor structural stability, making it difficult to meet the heat insulation needs of spacecraft. Magnesium aluminum spinel In the preparation method of aerogel material, the temperature resistance is insufficient due to differences in metal activity.
Using zirconia nanofiber membrane as support, magnesium-aluminum spinel precursor sol is synthesized through hydrothermal reaction, and layer by layer during liquid nitrogen pre-freezing and high-temperature calcination to form a spinel structure aerogel thermal insulation Materials, polyethylene oxide and mineralizers are used to regulate reactions and structures.
It improves the temperature resistance and structural strength of magnesium-aluminum spinel aerogel composite material, reduces thermal conductivity, enhances the mechanical properties and thermal insulation properties of the material, and is suitable for high-temperature environment applications.
Smart Images

Figure BDA0004945553740000141 
Figure BDA0004945553740000151
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of magnesium-aluminum spinel composite thermal insulation materials, and in particular relates to a spinel structure high-temperature resistant aerogel thermal insulation material and a preparation method thereof. Background Art
[0002] Aerogel is a typical three-dimensional network structure material with the characteristics of light weight and low thermal conductivity. It is widely used in extreme environments such as metallurgy, high-temperature catalysis, and aerospace. Oxide aerogels, such as silicon oxide and aluminum oxide aerogels, are resistant to high temperatures and oxidation and are widely used in the field of thermal insulation of various aerospace vehicles. As the external ambient temperature of aircraft continues to rise, existing oxide aerogels have been difficult to meet application requirements. Silicon oxide has a low melting point, and the temperature resistance of the prepared aerogel is less than 1000°C; aluminum oxide and zirconium oxide aerogel materials undergo high-temperature crystal transformation, and their structural stability is poor, so they have not been widely used.
[0003] Magnesium aluminum spinel has the characteristics of high melting point and no crystal transformation. It is widely used in the field of heat resistance and fire resistance. It is a material solution to break through the excellent temperature resistance of oxide aerogel. However, at present, aerogels with magnesium aluminum spinel crystal structure are mostly prepared by sol-gel method. Due to the large difference in the activity of the two-component metals, the hydrolysis and polycondensation reactions are difficult to match, making the prepared materials insufficient in temperature resistance. It is urgent to seek new technical routes to synthesize magnesium aluminum spinel aerogel insulation materials with excellent performance.
[0004] In summary, it is very necessary to provide a spinel structure high temperature resistant aerogel insulation material and a preparation method thereof. Summary of the invention
[0005] In order to solve one or more technical problems existing in the prior art, the present invention provides a spinel structure high temperature resistant aerogel insulation material and a preparation method thereof.
[0006] In a first aspect, the present invention provides a method for preparing a spinel structure high temperature resistant aerogel thermal insulation material, the method comprising the following steps:
[0007] (1) uniformly dispersing nano-alumina sol and nano-magnesium oxide with water to obtain a dispersion, and then adding a structure modifier and a mineralizer to the dispersion to perform a hydrothermal reaction to obtain a composite precursor sol;
[0008] (2) adding polyethylene oxide to the composite precursor sol and mixing them uniformly to obtain an impregnation solution;
[0009] (3) placing the zirconium oxide nanofiber membrane in the impregnation liquid for impregnation and swelling to obtain an impregnation and swelling nanofiber membrane;
[0010] (4) Multiple impregnated and swollen nanofiber membranes are stacked layer by layer, pre-frozen in liquid nitrogen and freeze-dried, and then calcined at high temperature to obtain a spinel structure high temperature resistant aerogel insulation material.
[0011] Preferably, the molar ratio of aluminum contained in the nano-alumina sol to magnesium contained in the nano-magnesium oxide is (0.95-1.1):1; and / or the sum of the mass percentages of nano-alumina and nano-magnesium oxide contained in the dispersion is 5-15%.
[0012] Preferably, the structure modifier is an organic weak acid; preferably, the organic weak acid is acetic acid solution, oxalic acid solution, oxalic acid solution and citric acid solution; preferably, the concentration of the organic weak acid is 0.1-5 mol / L.
[0013] Preferably, the mineralizer is one or more of ammonium fluoride powder, aluminum fluoride powder, and lithium fluoride powder.
[0014] Preferably, the mass amount of the structure modifier is 3-5% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol; and / or the mass amount of the mineralizer is 1-2% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol.
[0015] Preferably, the temperature of the hydrothermal reaction is 180-300° C., and the time of the hydrothermal reaction is 12-48 hours.
[0016] Preferably, the mass amount of the polyethylene oxide is 0.1-1% of the mass amount of the composite precursor sol.
[0017] Preferably, the thickness of the zirconium oxide nanofiber membrane is 0.2-1 mm.
[0018] Preferably, the temperature of the high-temperature calcination is 1200-1500° C., and the time of the high-temperature calcination is 1-3 hours.
[0019] In a second aspect, the present invention provides a spinel structure high temperature resistant aerogel thermal insulation material prepared by the preparation method described in the first aspect of the present invention.
[0020] Compared with the prior art, the present invention has at least the following beneficial effects:
[0021] The present invention uses a zirconia nanofiber membrane as a support, which ensures the synchronous contraction of the reinforcement and the precursor aerogel during the high-temperature aluminum-magnesium spinel crystal control process, avoiding the cracking of the structure and the problem of strength reduction; the present invention uses nano-alumina sol and nano-magnesium oxide as precursors, effectively regulates the reaction activity, and avoids the uncontrollability of metal salt hydrolysis and polycondensation; the composite precursor sol is synthesized by hydrothermal reaction, the reaction conditions are mild and the reaction process is controllable, and the mineralizer and structure modifier are introduced into the reaction process, which effectively controls the particle size and structure of the material, so that the material generates a magnesium-aluminum spinel structure with low thermal conductivity at low temperature. The method of the present invention can improve the temperature resistance of oxide aerogel, effectively regulate the material pore structure, reduce the thermal conductivity of the material, and the synchronous contraction scheme also improves the structural strength of the composite material, which lays a good foundation for the application of magnesium-aluminum spinel aerogel composite insulation materials. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] In a first aspect, the present invention provides a method for preparing a spinel structure high temperature resistant aerogel thermal insulation material, the method comprising the following steps:
[0024] (1) using water to evenly disperse nano-alumina sol (also known as nano-aluminum sol) and nano-magnesium oxide (magnesium oxide nanopowder) to obtain a dispersion, then adding a structure modifier and a mineralizer to the dispersion and performing a hydrothermal reaction to obtain a composite precursor sol (also referred to as magnesium aluminum spinel precursor sol); the present invention does not specifically limit the source of the nano-alumina sol, and can use products that can be directly purchased on the market or products synthesized by existing methods; in the present invention, the solid content of the nano-alumina sol is 20-25wt%; in the present invention, specifically, for example, nano-alumina sol is used as an aluminum source, nano-magnesium oxide is used as a magnesium source, and they are added to water at a magnesium-aluminum molar ratio of 1:1, and then an organic weak acid is introduced as a structure modifier, and a mineralizer is added at the same time, and a high-temperature hydrothermal reaction is performed to prepare the composite precursor sol; the present invention does not specifically limit the source of the magnesium oxide nanopowder, etc., and can use products that can be directly purchased or products synthesized by existing methods;
[0025] (2) adding polyethylene oxide (also known as polyethylene oxide, abbreviated as PEO) to the composite precursor sol and mixing them uniformly to obtain an impregnation solution; in the present invention, for example, a certain mass of polymer auxiliary agent PEO is weighed and added to the composite precursor sol, stirred and mixed uniformly to prepare an impregnation solution; the present invention has no particular limitation on polyethylene oxide, and a product that can be directly purchased on the market can be used; in the present invention, the polyethylene oxide is used as a gelling auxiliary agent;
[0026] (3) placing the zirconium oxide nanofiber membrane in the impregnation liquid for impregnation swelling to obtain an impregnation swelling nanofiber membrane; in the present invention, during the impregnation swelling, the zirconium oxide nanofiber membrane can be completely immersed in the impregnation liquid; in the present invention, in order to obtain a plurality of impregnation swelling nanofiber membranes, for example, a plurality of zirconium oxide nanofiber membranes can be placed in the impregnation liquid at the same time for impregnation swelling; in the present invention, the impregnation swelling time can be, for example, 4 to 8 hours;
[0027] (4) Multiple (two or more) impregnated and swollen nanofiber membranes are stacked layer by layer, pre-frozen in liquid nitrogen and freeze-dried, and then calcined at high temperature to obtain a spinel structure high temperature resistant aerogel insulation material; in the present invention, the freeze drying can be carried out under conventional freeze drying conditions, and the freeze drying temperature can be, for example, -40°C to -50°C, and the freeze drying time can be, for example, 48 to 96 hours; in the present invention, for example, they can be stacked layer by layer until a preset thickness of 10 to 20 mm is reached; in the present invention, after the impregnation and swelling is completed, the impregnated and swollen nanofiber membrane is taken out, and the excess solution (impregnation liquid) on the surface is absorbed with a dry paper towel; the impregnated and swollen nanofiber membranes are stacked layer by layer, pre-frozen in liquid nitrogen, freeze-dried, and then calcined at high temperature to obtain a high-strength magnesium-aluminum spinel structure nanofiber reinforced aerogel composite material, which is the spinel structure high temperature resistant aerogel insulation material described in the present invention.
[0028] The present invention adopts zirconium oxide nanofiber membrane as a support body, which ensures the synchronous shrinkage of the reinforcement body and the precursor aerogel during the control process of high-temperature aluminum-magnesium spinel crystal form (magnesium-aluminum spinel crystal form), avoiding the cracking of the structure and the problem of strength reduction; the present invention uses highly active nano-alumina sol and nano-magnesium oxide as magnesium-aluminum spinel precursors. Compared with other active components, nano-scale magnesium-aluminum spinel precursor sol can be generated under hydrothermal conditions, which is convenient for fiber impregnation, effectively regulates the reaction activity, and avoids the uncontrollability of metal salt hydrolysis and condensation; the composite precursor sol is synthesized by hydrothermal reaction, the reaction conditions are mild and the reaction process is controllable, and at the same time, mineralizers and structure modifiers are introduced into the reaction process, which effectively controls the particle size and structure of the material, so that the material generates a magnesium-aluminum spinel structure with low thermal conductivity at low temperature. The present invention finds that mineralizers can be used to achieve homogeneous doping of aluminum and magnesium elements, reduce the activation energy of the hydrothermal reaction of magnesium and aluminum, promote the growth and development of crystals, and thus control the particle size and structure of the material. The structure modulator can regulate the morphology of nanoparticles, promote the ripening and rearrangement of particles under hydrothermal reaction conditions, and regulate the morphology and structure of the material. The present invention improves the mechanical properties and thermal insulation properties of aerogel thermal insulation materials by optimizing the particle size and structure of the material, thereby making it have better performance in a high temperature environment. The method of the present invention can improve the temperature resistance of oxide aerogels, effectively regulate the pore structure of the material, and reduce the thermal conductivity of the material. At the same time, the synchronous shrinkage scheme also improves the structural strength of the composite material, laying a good foundation for the application of magnesium-aluminum spinel aerogel composite thermal insulation materials.
[0029] According to some preferred embodiments, the molar ratio of the aluminum contained in the nano-alumina sol to the magnesium contained in the nano-magnesium oxide is (0.95-1.1):1, preferably 1:1; and / or the sum of the mass percentages of nano-alumina and nano-magnesium oxide in the dispersion is 5-15% (for example, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%). In the present invention, preferably, the sum of the mass percentages of nano-alumina and nano-magnesium oxide in the dispersion is 5-15%. This concentration can make the system have good dispersibility and is not prone to agglomeration and sedimentation.
[0030] According to some preferred embodiments, the structure modulator is an organic weak acid, including monobasic, dibasic and tribasic acids; preferably, the organic weak acid is acetic acid solution (acetic acid aqueous solution), oxalic acid solution (oxalic acid aqueous solution), oxalic acid solution (oxalic acid aqueous solution) and citric acid solution (citric acid aqueous solution), these organic weak acids can regulate the morphology of nanoparticles, promote the ripening and rearrangement of particles under hydrothermal reaction conditions, and adjust the morphology and structure of the material; preferably, the concentration of the organic weak acid is 0.1-5 mol / L (for example, 0.1, 0.5, 0.8, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5 or 5 mol / L).
[0031] According to some preferred embodiments, the mineralizer is one or more of ammonium fluoride powder, aluminum fluoride powder, and lithium fluoride powder; in the present invention, unlike the catalyst such as ammonium fluoride solution used to promote the gel reaction, the present invention uses solid ammonium fluoride powder, aluminum fluoride powder, lithium fluoride powder, etc. as mineralizers. The present invention finds that the mineralizer can provide a stable and continuous mineralization effect during the hydrothermal reaction, which helps to control the particle size and structure of the material, ensure the uniformity of the material structure, and the uniform pore structure enables the aerogel insulation material to have better insulation effect and structural stability at high temperatures.
[0032] According to some preferred embodiments, the mass amount of the structure modifier is 3-5% (e.g., 3%, 3.5%, 4%, 4.5% or 5%) of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol; and / or the mass amount of the mineralizer is 1-2% (e.g., 1%, 1.5% or 2%) of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol; in the present invention, by strictly controlling the amount of the structure modifier and the mineralizer within an appropriate range, the key parameters such as the microstructure, particle size, and porosity of the material can be effectively regulated, thereby obtaining a spinel structure high-temperature resistant aerogel insulation material with excellent performance; the present invention finds that the structure modifier can regulate the crystal morphology and microstructure of the material during the hydrothermal reaction process to ensure that the material has uniform nanoscale dispersion and pore structure, and an appropriate amount of the structure modifier can enhance the mechanical properties of the material, so that it maintains good strength and toughness in a high temperature environment, through By regulating the porosity and pore size distribution, the structure modifier can improve the thermal insulation performance of the aerogel and reduce heat conduction. If the amount of the structure modifier is too little, it may make the pore structure difficult to optimize, reduce the thermal insulation performance and mechanical properties, and cause the material to be easily unstable or fail in a high temperature environment. If the amount of the structure modifier is too much, it may lead to excessive modulation, forming uneven phase separation or introducing too many defects, thereby affecting the overall performance of the material. The present invention finds that the mineralizer promotes the uniform growth and arrangement of nanocrystals during the hydrothermal reaction to ensure the uniformity and stability of the material structure. An appropriate amount of mineralizer helps to control the particle size and morphology of the material and prevent the particles from being too large or uneven, thereby improving the mechanical properties and thermal insulation properties of the material. If the amount of the mineralizer is too little, it may not be enough to effectively promote crystal growth and particle size control. If the amount of the mineralizer is too much, it may cause excessive mineralization, excessive or uneven crystal growth, the formation of coarse grains or uneven phase distribution, and reduce the performance of the material.
[0033] According to some preferred embodiments, the temperature of the hydrothermal reaction is 180-300°C (180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C or 300°C), and the time of the hydrothermal reaction is 12-48h (for example, 12, 24, 36 or 48h); in the present invention, preferably, the temperature of the hydrothermal reaction is 180-300°C, and sols with different particle sizes and different morphologies can be generated; in the present invention, preferably, the temperature of the hydrothermal reaction is 180-300°C. If the temperature is too low, no good mineralization reaction will occur, and if the temperature is too high, the reaction conditions are harsh and it is difficult to control the morphology and structure.
[0034] According to some preferred embodiments, the mass amount of the polyethylene oxide is 0.1-1% (e.g., 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%) of the mass amount of the composite precursor sol.
[0035] According to some preferred embodiments, the thickness of the zirconia nanofiber membrane is 0.2 to 1 mm (for example, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1 mm); in the present invention, preferably, the thickness of the zirconia nanofiber membrane is 0.2 mm-1 mm, which is convenient for quick and effective impregnation.
[0036] According to some preferred embodiments, the liquid nitrogen pre-freezing is freezing under liquid nitrogen for 10 to 60 minutes; and / or the temperature of the high-temperature calcination is 1200 to 1500°C (for example, 1200°C, 1300°C, 1400°C or 1500°C), and the time of the high-temperature calcination is 1 to 3 hours (for example, 1, 2 or 3 hours). In the present invention, preferably, the temperature of the high-temperature calcination is 1200 to 1500°C to ensure the formation of magnesium-aluminum spinel while achieving synchronous shrinkage of the fiber and the organic skeleton, thereby ensuring the matching degree of the insulation material components; in the present invention, the high-temperature calcination is carried out in an air atmosphere.
[0037] In a second aspect, the present invention provides a spinel structure high temperature resistant aerogel thermal insulation material prepared by the preparation method described in the first aspect of the present invention.
[0038] The present invention will be further described below by way of examples, but the protection scope of the present invention is not limited to these embodiments.
[0039] Example 1
[0040] (1) Weigh 20 g of nano-alumina sol (nano-alumina solid content of 25 wt%) and 4 g of nano-magnesium oxide (aluminum-magnesium molar ratio of 1:1), add them to water and disperse them evenly to obtain a dispersion, wherein the sum of the mass percentages of nano-alumina and nano-magnesium oxide in the dispersion is 5%; then add 0.5 mol / L acetic acid aqueous solution as a structure modifier and ammonium fluoride powder as a mineralizer to the dispersion, and perform a hydrothermal reaction at a high temperature of 180° C. for 24 h to prepare a composite precursor sol; the mass amount of the acetic acid aqueous solution is 4% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol; the mass amount of the ammonium fluoride powder is 1.5% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol.
[0041] (2) Adding polyethylene oxide (PEO) to the composite precursor sol system obtained above and stirring and mixing uniformly to obtain an impregnation solution; wherein the mass ratio of polyethylene oxide (PEO) to the composite precursor sol is 1:99.
[0042] (3) placing a 0.2 mm thick zirconium oxide nanofiber membrane in the impregnation solution obtained in step (2) for immersion and swelling for 5 hours to obtain an impregnated and swollen nanofiber membrane.
[0043] (4) The impregnated swollen nanofiber membrane is taken out from the impregnation liquid, and the excess solution on the surface is absorbed; 50 impregnated swollen nanofiber membranes with the excess solution on the surface absorbed are stacked layer by layer, and then quickly pre-frozen in liquid nitrogen for 30 minutes to form, and then freeze-dried for 72 hours, and then calcined at 1200°C for 2 hours to obtain a spinel structure high-temperature resistant aerogel insulation material.
[0044] Example 2
[0045] (1) Weigh 30 g of nano-alumina sol (nano-alumina solid content is 25 wt%) and 6 g of nano-magnesium oxide (aluminum-magnesium molar ratio is 1:1), add them to water and disperse them evenly to obtain a dispersion, wherein the sum of the mass percentages of nano-alumina and nano-magnesium oxide in the dispersion is 10%; then add a 2 mol / L citric acid aqueous solution as a structure modifier and a mineralizer aluminum fluoride powder to the dispersion, and perform a hydrothermal reaction at a high temperature of 250° C. for 12 h to prepare a composite precursor sol; the mass amount of the citric acid aqueous solution is 4% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol; the mass amount of the aluminum fluoride powder is 1.5% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol.
[0046] (2) Adding polyethylene oxide (PEO) to the composite precursor sol system obtained above and stirring and mixing uniformly to obtain an impregnation solution; wherein the mass ratio of polyethylene oxide (PEO) to the composite precursor sol is 0.1:99.
[0047] (3) placing a zirconia nanofiber membrane with a thickness of 1 mm in the impregnation solution obtained in step (2) for immersion and swelling for 5 hours to obtain an impregnated and swollen nanofiber membrane.
[0048] (4) The impregnated swollen nanofiber membrane is taken out from the impregnation liquid, and the excess solution on the surface is absorbed; 10 impregnated swollen nanofiber membranes with the excess solution on the surface absorbed are stacked layer by layer, and then quickly pre-frozen in liquid nitrogen for 30 minutes to form, and then freeze-dried for 72 hours, and then calcined at 1500°C for 2 hours to obtain a spinel structure high-temperature resistant aerogel insulation material.
[0049] Example 3
[0050] (1) Weigh 30 g of nano-alumina sol (nano-alumina solid content of 25 wt%) and 6 g of nano-magnesium oxide (aluminum-magnesium molar ratio of 1:1), add them to water and disperse them evenly to obtain a dispersion, wherein the sum of the mass percentages of nano-alumina and nano-magnesium oxide in the dispersion is 15%; then add 5 mol / L oxalic acid aqueous solution as a structure modifier and a mineralizer lithium fluoride powder to the dispersion, and perform a hydrothermal reaction at a high temperature of 300° C. for 24 h to prepare a composite precursor sol; the mass amount of the oxalic acid aqueous solution is 4% of the sum of the mass amounts of nano-alumina and nano-magnesium oxide contained in the nano-alumina sol; the mass amount of the lithium fluoride powder is 1.5% of the sum of the mass amounts of nano-alumina and nano-magnesium oxide contained in the nano-alumina sol.
[0051] (2) Adding polyethylene oxide (PEO) to the composite precursor sol system obtained above and stirring and mixing uniformly to obtain an impregnation solution; wherein the mass ratio of polyethylene oxide (PEO) to the composite precursor sol is 0.2:99.
[0052] (3) placing a 0.5 mm thick zirconium oxide nanofiber membrane in the impregnation solution obtained in step (2) for immersion and swelling for 5 hours to obtain an impregnated and swollen nanofiber membrane.
[0053] (4) The impregnated swollen nanofiber membrane is taken out from the impregnation liquid, and the excess solution on the surface is absorbed; 20 impregnated swollen nanofiber membranes with the excess solution on the surface absorbed are stacked layer by layer, and then quickly pre-frozen in liquid nitrogen for 30 minutes to form, and then freeze-dried for 72 hours, and then calcined at 1400°C for 2 hours to obtain a spinel structure high-temperature resistant aerogel insulation material.
[0054] Example 4
[0055] (1) Weigh 30 g of nano-alumina sol (nano-alumina solid content of 25 wt%) and 6 g of nano-magnesium oxide (aluminum-magnesium molar ratio of 1:1), add them to water and disperse them evenly to obtain a dispersion, wherein the sum of the mass percentages of nano-alumina and nano-magnesium oxide in the dispersion is 15%; then add 5 mol / L oxalic acid aqueous solution as a structure modifier and a mineralizer lithium fluoride powder to the dispersion, and perform a hydrothermal reaction at a high temperature of 240° C. for 48 h to prepare a composite precursor sol; the mass amount of the oxalic acid aqueous solution is 4% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol; the mass amount of the lithium fluoride powder is 1.5% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol.
[0056] (2) Adding polyethylene oxide (PEO) to the composite precursor sol system obtained above and stirring and mixing uniformly to obtain an impregnation solution; wherein the mass ratio of polyethylene oxide (PEO) to the composite precursor sol is 0.2:99.
[0057] (3) placing a 0.5 mm thick zirconium oxide nanofiber membrane in the impregnation solution obtained in step (2) for immersion and swelling for 5 hours to obtain an impregnated and swollen nanofiber membrane.
[0058] (4) The impregnated swollen nanofiber membrane is taken out from the impregnation liquid, and the excess solution on the surface is absorbed; 20 impregnated swollen nanofiber membranes with the excess solution on the surface absorbed are stacked layer by layer, and then quickly pre-frozen in liquid nitrogen for 30 minutes to form, and then freeze-dried for 72 hours, and then calcined at 1400°C for 2 hours to obtain a spinel structure high-temperature resistant aerogel insulation material.
[0059] Example 5
[0060] (1) Weigh 30 g of nano-alumina sol (nano-alumina solid content of 25 wt%) and 6 g of nano-magnesium oxide (aluminum-magnesium molar ratio of 1:1), add them to water and disperse them evenly to obtain a dispersion, wherein the sum of the mass percentages of nano-alumina and nano-magnesium oxide in the dispersion is 15%; then add 5 mol / L acetic acid aqueous solution as a structure modifier and a mineralizer ammonium fluoride powder to the dispersion, and perform a hydrothermal reaction at a high temperature of 240° C. for 24 h to prepare a composite precursor sol; the mass amount of the acetic acid aqueous solution is 4% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol; the mass amount of the ammonium fluoride powder is 1.5% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol.
[0061] (2) Adding polyethylene oxide (PEO) to the composite precursor sol system obtained above and stirring and mixing uniformly to obtain an impregnation solution; wherein the mass ratio of polyethylene oxide (PEO) to the composite precursor sol is 0.2:99.
[0062] (3) placing a 0.5 mm thick zirconium oxide nanofiber membrane in the impregnation solution obtained in step (2) for immersion and swelling for 5 h to obtain an impregnated and swollen nanofiber membrane;
[0063] (4) The impregnated swollen nanofiber membrane is taken out from the impregnation liquid, and the excess solution on the surface is absorbed; 20 impregnated swollen nanofiber membranes with the excess solution on the surface absorbed are stacked layer by layer, and then quickly pre-frozen in liquid nitrogen for 30 minutes to form, and then freeze-dried for 72 hours, and then calcined at 1400°C for 2 hours to obtain a spinel structure high-temperature resistant aerogel insulation material.
[0064] Example 6
[0065] Example 6 is substantially the same as Example 5, except that:
[0066] (1) Weigh 30 g of nano-alumina sol (nano-alumina solid content of 25 wt%) and 6 g of nano-magnesium oxide (aluminum-magnesium molar ratio of 1:1), add them to water and disperse them evenly to obtain a dispersion, wherein the sum of the mass percentages of nano-alumina and nano-magnesium oxide in the dispersion is 15%; then add 5 mol / L acetic acid aqueous solution as a structure modifier and ammonium fluoride powder as a mineralizer to the dispersion, and perform hydrothermal reaction at a high temperature of 240° C. for 24 h to prepare a composite precursor sol; the mass amount of the acetic acid aqueous solution is 2% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol; the mass amount of the ammonium fluoride powder is 0.5% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol.
[0067] Example 7
[0068] Example 7 is substantially the same as Example 5, except that:
[0069] (1) Weigh 30 g of nano-alumina sol (nano-alumina solid content of 25 wt%) and 6 g of nano-magnesium oxide (aluminum-magnesium molar ratio of 1:1), add them to water and disperse them evenly to obtain a dispersion, wherein the sum of the mass percentages of nano-alumina and nano-magnesium oxide in the dispersion is 15%; then add 5 mol / L acetic acid aqueous solution as a structure modifier and ammonium fluoride powder as a mineralizer to the dispersion, and perform a hydrothermal reaction at a high temperature of 240° C. for 24 h to prepare a composite precursor sol; the mass amount of the acetic acid aqueous solution is 8% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol; the mass amount of the ammonium fluoride powder is 4% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol.
[0070] Comparative Example 1
[0071] (1) Weigh 30 g of nano-alumina sol (nano-alumina solid content of 25 wt%) and 6 g of nano-magnesium oxide (aluminum-magnesium molar ratio of 1:1), add them to water and disperse them evenly to obtain a dispersion, wherein the sum of the mass percentages of nano-alumina and nano-magnesium oxide in the dispersion is 15%; then add 5 mol / L acetic acid aqueous solution as a structure modifier and a mineralizer ammonium fluoride powder to the dispersion, and perform a hydrothermal reaction at a high temperature of 240° C. for 24 h to prepare a composite precursor sol; the mass amount of the acetic acid aqueous solution is 4% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol; the mass amount of the ammonium fluoride powder is 1.5% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol.
[0072] (2) preparing a polyethylene oxide aqueous dispersion, wherein the polyethylene oxide aqueous dispersion contains polyethylene oxide at a mass fraction of 0.3%; placing a zirconia nanofiber membrane with a thickness of 1 mm in the polyethylene oxide aqueous dispersion for immersion and swelling for 5 hours, then taking out the zirconia nanofiber membrane from the polyethylene oxide aqueous dispersion, and then stacking 10 zirconia nanofiber membranes after immersion and swelling layer by layer and immersing them in the composite precursor sol system obtained in step (1) for 5 hours to obtain a mixed system; wherein the total mass of the 10 zirconia nanofiber membranes after immersion and swelling accounts for 50% of the total mass of the composite precursor sol system.
[0073] (3) The mixed system obtained in step (2) is quickly pre-frozen in liquid nitrogen for 30 minutes to form a shape, then freeze-dried for 72 hours, and then calcined at 1000° C. for 2 hours to obtain a spinel structure high-temperature resistant aerogel insulation material.
[0074] Comparative Example 2
[0075] (1) Weigh 30 g of nano-alumina sol (nano-alumina solid content of 25 wt%) and 6 g of nano-magnesium oxide (aluminum-magnesium molar ratio of 1:1), add them to water and disperse them evenly to obtain a dispersion, wherein the sum of the mass percentages of nano-alumina and nano-magnesium oxide in the dispersion is 15%; then add 5 mol / L acetic acid aqueous solution as a structure modifier and ammonium fluoride powder as a mineralizer to the dispersion, and perform hydrothermal reaction at a high temperature of 100° C. for 24 h to prepare a composite precursor sol; the mass amount of the acetic acid aqueous solution is 4% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol; the mass amount of the ammonium fluoride powder is 1.5% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol.
[0076] (2) preparing a polyethylene oxide aqueous dispersion, wherein the polyethylene oxide aqueous dispersion contains polyethylene oxide at a mass fraction of 0.3%; placing a 3 mm thick zirconium oxide nanofiber membrane in the polyethylene oxide aqueous dispersion for immersion and swelling for 5 hours, then taking out the zirconium oxide nanofiber membrane from the polyethylene oxide aqueous dispersion, and then stacking the three immersed and swollen zirconium oxide nanofiber membranes layer by layer and immersing them in the composite precursor sol system obtained in step (1) for 5 hours to obtain a mixed system; wherein the total mass of the three immersed and swollen zirconium oxide nanofiber membranes accounts for 50% of the total mass of the composite precursor sol system.
[0077] (3) The mixed system obtained in step (2) is quickly pre-frozen with liquid nitrogen for 30 minutes to form, then freeze-dried for 72 hours, and then calcined at 1200° C. for 2 hours to obtain a spinel structure high-temperature resistant aerogel insulation material.
[0078] Comparative Example 3
[0079] Comparative Example 3 is substantially the same as Example 5, except that:
[0080] (1) Weigh 30 g of nano-alumina sol (nano-alumina solid content of 25 wt%) and 6 g of nano-magnesium oxide (aluminum-magnesium molar ratio of 1:1), add them to water and disperse them evenly to obtain a dispersion, wherein the sum of the mass percentages of nano-alumina and nano-magnesium oxide in the dispersion is 15%; then add 5 mol / L acetic acid aqueous solution as a structure modifier to the dispersion and perform a hydrothermal reaction at a high temperature of 240° C. for 24 h to prepare a composite precursor sol; the mass amount of the acetic acid aqueous solution is 4% of the sum of the mass amounts of nano-alumina and nano-magnesium oxide contained in the nano-alumina sol.
[0081] Comparative Example 4
[0082] Comparative Example 4 is substantially the same as Example 5, except that:
[0083] (4) The impregnated swollen nanofiber membrane is taken out from the impregnation liquid, and the excess solution on the surface is absorbed; 20 impregnated swollen nanofiber membranes with the excess solution on the surface absorbed are stacked layer by layer, and then quickly pre-frozen in liquid nitrogen for 30 minutes to form, and then freeze-dried for 72 hours, and then calcined at 1000°C for 2 hours to obtain a spinel structure high-temperature resistant aerogel insulation material.
[0084] Comparative Example 5
[0085] Comparative Example 5 is substantially the same as Example 5, except that:
[0086] (4) The impregnated swollen nanofiber membrane is taken out from the impregnation liquid, and the excess solution on the surface is absorbed; 20 impregnated swollen nanofiber membranes with the excess solution on the surface absorbed are stacked layer by layer, and then quickly pre-frozen in liquid nitrogen for 30 minutes to form, and then freeze-dried for 72 hours, and then calcined at 1600°C for 2 hours to obtain a spinel structure high-temperature resistant aerogel insulation material.
[0087] The thermal conductivity at 200°C, the single-sided shrinkage at 1400°C (the volume shrinkage after single-sided radiation heating at 1400°C for 2 hours) and the compressive strength at 1400°C when the deformation was 10% were measured for the materials prepared in the embodiments of the present invention and the comparative examples. The results are shown in Table 1. It can be seen from Table 1 that the materials prepared in the preferred embodiments of the present invention have low thermal conductivity and good temperature resistance, and have high mechanical strength at high temperatures, while the thermal insulation materials in the comparative examples have a large high-temperature thermal conductivity and insufficient temperature resistance.
[0088] Table 1
[0089]
[0090]
[0091] In Table 1, the symbol “-” indicates that the performance indicator does not exist.
[0092] Parts of the present invention that are not described in detail are well known to those skilled in the art.
[0093] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a spinel structure high temperature resistant aerogel thermal insulation material, characterized in that: The method comprises the following steps: (1) uniformly dispersing nano-alumina sol and nano-magnesium oxide with water to obtain a dispersion, and then adding a structure modifier and a mineralizer to the dispersion to perform a hydrothermal reaction to obtain a composite precursor sol; (2) adding polyethylene oxide to the composite precursor sol and mixing them uniformly to obtain an impregnation solution; (3) placing the zirconium oxide nanofiber membrane in the impregnation liquid for impregnation and swelling to obtain an impregnation and swelling nanofiber membrane; (4) Multiple impregnated and swollen nanofiber membranes are stacked layer by layer, pre-frozen in liquid nitrogen and freeze-dried, and then calcined at high temperature to obtain a spinel structure high temperature resistant aerogel insulation material.
2. The preparation method according to claim 1, characterized in that: The molar ratio of the aluminum contained in the nano-alumina sol to the magnesium contained in the nano-magnesium oxide is (0.95-1.1):1; and / or The sum of the mass percentages of nano-aluminum oxide and nano-magnesium oxide contained in the dispersion is 5-15%.
3. The preparation method according to claim 1, characterized in that: The structure modifier is an organic weak acid; Preferably, the organic weak acid is acetic acid solution, oxalic acid solution, oxalic acid solution and citric acid solution; Preferably, the concentration of the organic weak acid is 0.1 to 5 mol / L.
4. The preparation method according to claim 1, characterized in that: The mineralizer is one or more of ammonium fluoride powder, aluminum fluoride powder, and lithium fluoride powder.
5. The preparation method according to claim 1, characterized in that: The mass amount of the structure modifier is 3-5% of the sum of the mass amounts of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol; and / or The mass dosage of the mineralizer is 1-2% of the sum of the mass dosages of the nano-alumina and the nano-magnesium oxide contained in the nano-alumina sol.
6. The preparation method according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 180-300° C., and the time of the hydrothermal reaction is 12-48 hours.
7. The preparation method according to claim 1, characterized in that: The mass amount of the polyethylene oxide is 0.1-1% of the mass amount of the composite precursor sol.
8. The preparation method according to claim 1, characterized in that: The thickness of the zirconium oxide nanofiber membrane is 0.2-1 mm.
9. The preparation method according to claim 1, characterized in that: The temperature of the high-temperature calcination is 1200-1500° C., and the time of the high-temperature calcination is 1-3 hours.
10. A spinel structure high temperature resistant aerogel thermal insulation material prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of high-temperature-resistant low-temperature-synthesis blocky spinel aerogel material
CN106478134A
Method for preparing fiber-reinforced high-temperature-resistant magnesium aluminum spinel aerogel
CN107805064A
Infrared shielding coating modified fiber reinforced aerogel thermal insulation material and preparation method thereof
CN110698101A
High-temperature-resistant magnesium aluminate spinel aerogel and preparation method thereof
CN118005055A
Method for Manufacturing an Aerogel-Containing Composite and Composite Produced by that Method
US20130119294A1
Cited By
Preparation method of high-performance alumina fiber reinforced ceramic matrix composite material
CN119797904A
Flexible high-temperature-resistant aerogel composite material and preparation method thereof
CN121850692A