High-performance graphene / natural latex composite material and preparation method thereof

Through the combination of casein-modified graphene and hollow silica microspheres, the problem of poor dispersion of antibacterial materials in latex foamed products is solved, and the antibacterial and mechanical properties of latex foamed products are improved, achieving more uniform hair Bubble effect.

CN118895019AInactive Publication Date: 2024-11-05JIANGSU AIDEFU LATEX PROD

Patent Information

Application Number
CN202411012617.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

After the addition of antibacterial materials, it is difficult to achieve good emulsification and dispersion effects of existing latex foaming products, resulting in uneven foaming performance and reduced material mechanical strength and durability.

Method used

Casein is used to modify graphene, oxygen-containing functional groups such as hydroxyl groups are introduced, non-ionic modification is performed using π-π conjugation interaction, and hollow silica microspheres and lactone-type sophora lipids to form a uniform Enhance the network and improve the dispersion and antibacterial properties of graphene.

Benefits of technology

The antibacterial and mechanical properties of composite materials are improved, foaming properties and mechanical strength are enhanced, and the uniform dispersion and stability of composite materials are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004964824790000091
    Figure BDA0004964824790000091
  • Figure BDA0004964824790000101
    Figure BDA0004964824790000101
  • Figure BDA0004964824790000121
    Figure BDA0004964824790000121
Patent Text Reader

Abstract

The invention relates to the technical field of foaming products, and particularly discloses a high-performance graphene / natural latex composite material and a preparation method thereof. The high-performance graphene / natural latex composite material comprises the following raw materials in parts by weight: 100 parts of natural latex; 10 parts of castor oil soap liquid; 5-8 parts of a filler; 0.2 to 0.3 part of potassium hydroxide; 0.2 to 0.3 part of a stabilizing agent; 10-12 parts of a vulcanizing agent; 1-2 parts of an accelerant; 3-4 parts of potassium oleate; the filler comprises graphene, and the graphene is casein modified graphene. The preparation method comprises the following steps: S1, preparing raw materials; s2, mixing the raw materials; and S3, foaming and forming. The composite material can be used for bed products such as mattresses, pillows and the like, and has the advantages of excellent foaming performance, excellent antibacterial property, excellent mechanical property and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of foamed products, and more specifically, to a high-performance graphene / natural latex composite material and a preparation method thereof. Background Art

[0002] Natural latex is obtained from the sap of rubber trees. It is prepared into latex foam products through foaming, gelling, vulcanization and other processes. The obtained latex foam products have good air permeability, elasticity and are not easy to deform. Latex foam products are usually used as mattresses, pillows and other bedding products, which can give bedding products excellent resilience and anti-mite and antibacterial effects.

[0003] In order to increase the functionality of bedding, materials such as graphene and negative ions are added to bedding to improve its antibacterial and antiviral properties. However, the above functional materials are often difficult to achieve a good emulsification and dispersion effect, which affects the foaming performance of the latex liquid, causing problems such as uneven foaming and internal defects in the product, and ultimately leading to a significant reduction in the mechanical strength and durability of the latex material. Therefore, how to obtain a latex foam product with excellent foaming performance and better antibacterial properties is an urgent problem to be solved. Summary of the invention

[0004] In order to improve the foaming performance and antibacterial properties of foam products, the present application provides a high-performance graphene / natural latex composite material and a preparation method thereof.

[0005] The present application provides a high-performance graphene / natural latex composite material, which adopts the following technical solution:

[0006] In a first aspect, the present application provides a high-performance graphene / natural latex composite material, comprising the following raw materials in parts by weight:

[0007] 100 parts of natural latex;

[0008] 10 parts of castor oil soap solution;

[0009] 5-8 parts of filler;

[0010] Potassium hydroxide 0.2-0.3 parts;

[0011] Stabilizer 0.2-0.3 parts;

[0012] 10-12 parts of vulcanizing agent;

[0013] 1-2 parts of accelerator;

[0014] 3-4 parts of potassium oleate;

[0015] The filler includes graphene, and the graphene is casein-modified graphene.

[0016] By adopting the above technical scheme, graphene is modified by casein, oxygen-containing functional groups such as hydroxyl groups can be introduced on the surface of graphene, and graphene can be non-ionic modified by utilizing π-π conjugated interaction. While maintaining the sp2 network structure of graphene, casein can be intercalated between graphene sheets, so that graphene can be evenly dispersed in latex, forming a uniform reinforced network in the composite material, and effectively improving the antibacterial and mechanical properties of the composite material.

[0017] Optionally, the graphene is prepared as follows: casein, borax, ammonia water and deionized water are mixed to obtain a casein solution, and graphene, the casein solution, KOH, a diffusant NF and water are mixed and dispersed at high speed to obtain modified graphene.

[0018] By adopting the above technical scheme, casein solution, KOH and diffusion agent NF are used to modify graphene, and π-π conjugated interaction can be used to non-ionic modify graphene, and the dispersibility of graphene can be stably improved. At the same time, casein solution, KOH and diffusion agent NF can also effectively improve the thermal stability of latex. High-speed dispersion is carried out during the modification process, and the modifier can fully intercalate the graphene structure and properly peel the graphene, further improving the dispersion uniformity of graphene in the composite material, so that the graphene can have uniform antibacterial and mechanical reinforcement properties.

[0019] Optionally, the graphene is prepared as follows: casein, borax, ammonia water and deionized water are mixed to obtain a casein solution, and graphene, casein solution, lactone-type sophorolipid, KOH, diffusant NF and water are mixed and dispersed at high speed to obtain modified graphene.

[0020] By adopting the above technical solution, lactone sophorolipids are added during the modification process, and lactone sophorolipids can be intercalated and loaded between graphene sheets, thereby improving the dispersion effect of graphene. In addition, lactone sophorolipids also have better antibacterial properties and foam stabilizing effects, which can effectively improve the antibacterial effect and foaming performance of the composite material.

[0021] Optionally, the filler further comprises hollow silica microspheres, and the hollow silica microspheres are micrometer-sized hollow silica microspheres.

[0022] By adopting the above technical solution, preferably using hollow silica microspheres as fillers, the hollow silica microspheres can be partially loaded on the graphene sheets, reducing the agglomeration between graphenes, improving the dispersion of graphenes, and increasing the bonding effect between graphene and latex, so that the composite material has better mechanical properties. And because the hollow silica is light in weight, it can be evenly dispersed during the foaming process, is not easy to settle and agglomerate, and can be used as a mechanical dispersion point in the composite material, further improving the resilience and mechanical properties of the composite material.

[0023] Optionally, the hollow silica microspheres are prepared as follows: micron-sized polystyrene microspheres and CTAB are added to an ethanol solution, ultrasonically dispersed to obtain a suspension, and then ammonia water is added for stirring; TEOS is added, the reaction is continuously stirred, and the obtained suspension is placed in a centrifuge for ultracentrifugation, the solid matter is retained, washed, dried, and heat-treated to obtain hollow silica microspheres.

[0024] By adopting the above technical scheme, the preparation method of silica microspheres was optimized, and mesoporous silica with a hollow structure was prepared using polystyrene microspheres and CTAB as templates. CTAB can hinder the agglomeration of polystyrene microspheres to obtain hollow silica with a uniform structure.

[0025] Optionally, the hollow silica microspheres are mercapto-modified hollow silica microspheres.

[0026] By adopting the above technical scheme, thiol groups are grafted onto silica microspheres, and the adsorption of thiol groups can be used to improve the loading effect of hollow silica on graphene, that is, the silica microspheres are used to fully disperse the graphene, reducing the possibility of graphene agglomeration, so that the composite material obtains uniform mechanical properties and antibacterial effects.

[0027] Optionally, the hollow silica microspheres are hollow silica microspheres loaded with silk fibroin.

[0028] By adopting the above technical solution, silk fibroin has a better adhesion effect. After silk fibroin is loaded on hollow silica microspheres, it can further improve the bonding effect between silica and graphene, and can improve the bonding effect between silica and natural latex, and further improve the mechanical properties of the composite material. In addition, silk fibroin can also be combined with lactone-type sophorolipids, further promoting the bonding effect between silica and graphene, and can form a foam-stabilizing structure to improve the foaming effect of the composite material.

[0029] Optionally, the hollow silica microspheres are loaded with antibacterial particles, and the antibacterial particles are selected from silver or gold.

[0030] By adopting the above technical solution, gold or silver is loaded on the surface of hollow silica microspheres. Gold or silver has strong antibacterial and bactericidal effects and is extremely safe. When added to composite materials, it can give the composite materials excellent antibacterial effects and safety. In addition, gold or silver has a long-lasting antibacterial effect, which can enable the composite materials to obtain a long-lasting and stable antibacterial effect.

[0031] Optionally, the filler further includes a protein filler, and the protein filler includes sericin, fibroin or collagen.

[0032] By adopting the above technical solution, sericin, silk fibroin or collagen has the advantages of excellent biocompatibility, stable performance and wide sources. After being added to the composite material, a cross-linked network structure can be formed in the composite material, so that the composite material has relatively excellent resilience. In addition, the lactone-type sophorolipid in the modified graphene can be combined with the protein filler to play a role in stabilizing the foam in the composite material, so that the composite material has a relatively excellent foaming effect.

[0033] In a second aspect, the present application provides a method for preparing a high-performance graphene / natural latex composite material, using the following technical solution:

[0034] A method for preparing a high-performance graphene / natural latex composite material comprises the following steps:

[0035] S1. Prepare raw materials: weigh natural latex, castor oil soap solution, filler, vulcanizing agent, accelerator, potassium oleate, potassium hydroxide and stabilizer respectively according to weight parts;

[0036] S2, mixing: placing the natural latex in a stirring device for stirring, adding castor oil soap solution, filler, vulcanizing agent, accelerator, potassium oleate, potassium hydroxide and stabilizer, continuing stirring and maturing to obtain a mixture;

[0037] S3, Foaming: Keep the mixture warm, add zinc oxide and coagulant, stir until foaming, pour into a mold, gel, vulcanize, demould and dry to obtain a composite material.

[0038] In summary, this application has the following beneficial effects:

[0039] 1. Since the present application uses casein to modify graphene and utilizes π-π conjugated interaction to perform non-ionic modification on graphene, while maintaining the sp2 network structure of graphene, casein can be intercalated between graphene sheets, so that graphene can be evenly dispersed in latex, forming a uniform reinforced network in the composite material, effectively improving the antibacterial and mechanical properties of the composite material.

[0040] 2. In the present application, hollow silica microspheres are preferably used as fillers. Hollow silica microspheres can be partially loaded on graphene sheets, reduce the agglomeration of graphene, improve the dispersibility of graphene, and increase the bonding effect between graphene and latex, so that the composite material has better mechanical properties. And because the weight of hollow silica is relatively light, it can be evenly dispersed during the foaming process, is not easy to settle and agglomerate, and can be used as a mechanical dispersion point in the composite material, further improving the resilience and mechanical properties of the composite material.

[0041] 3. The silk fibroin in the present application has a good adhesion effect. After the silk fibroin is loaded on the hollow silica microspheres, it can further improve the bonding effect between silica and graphene, and can improve the bonding effect between silica and natural latex, and further improve the mechanical properties of the composite material. In addition, the silk fibroin can also combine with the lactone-type sophorolipids, further promoting the bonding effect between silica and graphene, and can form a stable foam structure to improve the foaming effect of the composite material. DETAILED DESCRIPTION

[0042] The present application is further described in detail below with reference to the embodiments.

[0043] Preparation Example

[0044] Graphene Preparation Example

[0045] Preparation Example 1

[0046] 10g casein, 1.5g borax, 3.2g 28% ammonia water and 85.3g water were mixed to prepare a 10% casein solution. 3g 10% diffusion agent NF solution, 26g 10% KOH solution, 38g 10% casein solution, 2.5g graphene (specific surface area: 400-500m 2 / g) and 30.5g deionized water, grind for 60min, 1.5×10 4 r / min high speed dispersion to obtain modified graphene.

[0047] The grinding time and dispersion rate are optimized. Appropriate grinding time and dispersion rate can enable graphene to obtain a more suitable lamellar structure and particle size, and casein, diffusant NF, etc. can be fully loaded on graphene, effectively improving the dispersion effect of graphene in the composite material.

[0048] Preparation Example 2

[0049] 10g casein, 1.5g borax, 3.2g ammonia water with a mass fraction of 28% and 85.3g water were mixed to prepare a casein solution with a mass fraction of 10%. 3g 10% diffusion agent NF solution, 26g 10% KOH solution, 38g 10% casein solution, 2.5g graphene, 3g lactone type sophorolipid and 27.5g deionized water were ground for 60min, 1.5×10 4 r / min high speed dispersion to obtain modified graphene.

[0050] Hollow microsphere preparation example

[0051] Preparation Example 3

[0052] Take 0.15g of micron-sized polystyrene microspheres and 0.1g of CTAB and add them to 240mL of ethanol solution, ultrasonically disperse for 30min to obtain a suspension, then add 3mL of ammonia water (mass fraction is 28%) and stir; add 0.3mL of LTEOS, continue stirring and react for 20h, put the obtained suspension into a centrifuge for ultracentrifugation, retain the solid matter, wash and dry for 12h, and heat treat at 500℃ for 2h to obtain hollow silica microspheres.

[0053] Preparation Example 4

[0054] 1 g of the hollow silica microspheres prepared in Preparation Example 3 was dispersed in 100 mL of toluene solution, ultrasonically dispersed for 10 min, 2 mL of MPS was added, magnetically stirred, refluxed at 80 ° C for 18 h, cooled to room temperature, washed with water, and dried to obtain an intermediate product. 0.5 g of the intermediate product was dispersed in 50 mL of hydrogen peroxide, magnetically stirred for 48 h, washed with water, and dried to obtain thiol-modified hollow silica microspheres.

[0055] Preparation Example 5

[0056] 2 g of the thiol-modified hollow silica microspheres prepared in Preparation Example 3 were mixed with water to obtain a 2% silicon solution by mass, and stirred at room temperature for 30 min. Silk fibroin was mixed with water to obtain a 2% protein solution by mass, and the protein solution and the silicon solution were stirred at room temperature for 1 h, filtered, and dried to obtain hollow silica microspheres loaded with silk fibroin.

[0057] Preparation Example 6

[0058] 2 g of the thiol-modified hollow silica microspheres prepared in Preparation Example 4 were mixed with water to obtain a 2% silicon solution, and stirred at room temperature for 30 min. Silk fibroin was mixed with water to obtain a 2% protein solution, and the protein solution and the silicon solution were stirred at room temperature for 1 h, filtered, and dried to obtain hollow silica microspheres loaded with silk fibroin.

[0059] Preparation Example 7

[0060] Take 2g of the thiol-modified hollow silica microspheres prepared in Preparation Example 4 and disperse them in 1000mL of ethanol, ultrasonically disperse them, and obtain a silicon dispersion. Dissolve 0.36g of silver nitrate in 1000mL of water, ultrasonically disperse them, and obtain a silver solution. Mix the silver solution with the silicon dispersion, add 0.2g of PVP-K30, continue stirring for 20min, add 0.1g of NaBH4, react at room temperature for 15min, wash, centrifuge, retain the solids, and freeze-dry to obtain hollow silica microspheres loaded with antibacterial particles.

[0061] Preparation Example 8

[0062] Take 2g of the thiol-modified hollow silica microspheres prepared in Preparation Example 6 and disperse them in 1000mL of ethanol, ultrasonically disperse them, and obtain a silicon dispersion. Dissolve 0.36g of silver nitrate in 1000mL of water, ultrasonically disperse them, and obtain a silver solution. Mix the silver solution with the silicon dispersion, add 0.2g of PVP-K30, continue stirring for 20min, add 0.1g of NaBH4, react at room temperature for 15min, wash, centrifuge, retain the solids, and freeze-dry to obtain hollow silica microspheres loaded with antibacterial particles.

[0063] Example

[0064] Examples 1-3

[0065] On the one hand, the present application provides a high-performance graphene / natural latex composite material, comprising natural latex, castor oil soap solution, filler, potassium hydroxide, stabilizer, accelerator, vulcanizer and potassium oleate, and the specific mass is shown in the table below.

[0066] Among them, the natural latex is concentrated natural latex with a solid content of 60%, the castor oil soap liquid is castor oil soap liquid with a solid content of 25%, the potassium oleate is potassium oleate with a solid content of 20%, the vulcanizing agent is a vulcanization package with a solid content of 50%, the accelerator is accelerator DGP with a solid content of 40%, and the stabilizer is zinc oxide.

[0067] The filler is the graphene prepared in Preparation Example 1.

[0068] On the other hand, the present application provides a method for preparing a high-performance graphene / natural latex composite material, comprising the following steps:

[0069] S1. Prepare raw materials: weigh natural latex, castor oil soap solution, filler, vulcanizing agent, accelerator, potassium oleate, potassium hydroxide and stabilizer respectively according to weight parts;

[0070] S2, raw material mixing: placing natural latex in a stirring device for stirring, adding castor oil soap solution, filler, vulcanizing agent, accelerator, potassium oleate, potassium hydroxide and stabilizer, continuing stirring, ripening for 24 hours, and obtaining a mixture;

[0071] S3. Foaming molding: The mixed material is kept warm, stirred until foamed, poured into a mold, gelled at 55°C, vulcanized for 30 minutes, demoulded, and dried to obtain a composite material.

[0072] Table 1 Composition of Examples 1-3

[0073]

[0074]

[0075] Example 4

[0076] The difference from Example 3 is that the filler is the graphene prepared in Preparation Example 2.

[0077] Example 5

[0078] The difference from Example 3 is that the filler includes the graphene prepared in Preparation Example 2 and the hollow silica microspheres prepared in Preparation Example 3 in a mass ratio of 2:1.

[0079] Example 6

[0080] The difference from Example 3 is that the filler includes the graphene prepared in Preparation Example 2 and the mercapto-modified hollow silica microspheres prepared in Preparation Example 4 in a mass ratio of 2:1.

[0081] Example 7

[0082] The difference from Example 3 is that the filler includes the graphene prepared in Preparation Example 2 and the hollow silica microspheres loaded with silk fibroin prepared in Preparation Example 5 in a mass ratio of 2:1.

[0083] Example 8

[0084] The difference from Example 3 is that the filler includes the graphene prepared in Preparation Example 2 and the hollow silica microspheres loaded with silk fibroin prepared in Preparation Example 6 in a mass ratio of 2:1.

[0085] Example 9

[0086] The difference from Example 3 is that the filler includes the graphene prepared in Preparation Example 2 and the hollow silica microspheres loaded with antibacterial particles prepared in Preparation Example 7 in a mass ratio of 2:1.

[0087] Example 10

[0088] The difference from Example 3 is that the filler includes the graphene prepared in Preparation Example 2 and the hollow silica microspheres loaded with antibacterial particles prepared in Preparation Example 8 in a mass ratio of 2:1.

[0089] Embodiment 11

[0090] The difference from Example 3 is that the filler includes the graphene prepared in Preparation Example 2, the hollow silica microspheres loaded with silk fibroin prepared in Preparation Example 5, and silk fibroin in a mass ratio of 3:2:1.

[0091] Example 12

[0092] The difference from Example 3 is that the filler includes the graphene prepared in Preparation Example 2, the hollow silica microspheres loaded with silk fibroin prepared in Preparation Example 8, and silk fibroin in a mass ratio of 3:2:1.

[0093] Comparative Example

[0094] Comparative Example 1

[0095] The difference between this comparative example and Example 3 is that the filler in this comparative example is modified graphene (specific surface area: 400-500m 2 / g) composition.

[0096] Performance testing

[0097] (1) Mechanical properties test: Test the tensile properties and elongation at break of the composite material according to GB / T 528-1998 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber;

[0098] (2) Foaming performance test: Observe the integrity of the cells in a certain range of the test slice under a microscope (record the percentage of intact cells to all cells).

[0099] (3) Antibacterial performance test: The composite material was cut into 1 cm × 1 cm pieces, washed with ethanol and set aside. Escherichia coli and Staphylococcus aureus were activated and prepared into a concentration of 1 × 10 6 cfu / mL of bacterial suspension, and then put the cut sample in. Fix the conical flask containing the bacterial suspension and sample on an oscillating shaker, shake at 300 rpm for 2 minutes at 25°C, and then take 1.0mL of the bacterial suspension and dilute it to 100 times. Take 1.0mL after aspiration and shaking, inoculate it on the agar base, and culture it at 37°C for 48 hours under natural light, and then count it using the method in GB15979-2003 and calculate the inhibition rate.

[0100] Table 2 Performance test

[0101]

[0102] The antibacterial property test of the composite material in Example 3 showed that the antibacterial rate against Escherichia coli was 96.7%, and the antibacterial rate against Staphylococcus aureus was 96.5%.

[0103] The antibacterial property test of the composite material in Example 10 showed that the antibacterial rate against Escherichia coli was 99.9%, and the antibacterial rate against Staphylococcus aureus was 99.9%.

[0104] Combining the performance test comparison in Table 2, we can find that:

[0105] 1. By comparing Examples 1-3 with Comparative Example 1, it can be found that the tensile strength, elongation at break and foaming properties of the composite materials prepared in Examples 1-3 are improved, which means that casein is used to modify graphene in the present application, and the graphene is non-ionic modified by utilizing π-π conjugated interaction. While maintaining the sp2 network structure of graphene, casein can be intercalated between graphene sheets to form a uniform reinforced network in the composite material, thereby effectively improving the antibacterial and mechanical properties of the composite material.

[0106] 2. By comparing Example 4 with Example 3, it can be found that the tensile strength, elongation at break and foaming performance of the composite material prepared in Example 4 are all improved, which indicates that the present application adds lactone-type sophorolipids during the modification process, and the lactone-type sophorolipids can be intercalated between the graphene sheets, thereby improving the dispersion effect of graphene. In addition, the lactone-type sophorolipids also have better antibacterial properties and foam stabilizing effects, which can effectively improve the antibacterial effect and foaming performance of the composite material.

[0107] 3. By comparing Example 5 with Example 3, it can be found that the tensile strength, elongation at break and foaming performance of the composite material prepared in Example 5 are improved, which means that in the present application, the hollow silica microspheres can be partially loaded on the graphene sheets, thereby improving the dispersibility of the graphene and increasing the bonding effect between the graphene and the latex. In addition, the hollow silica is light in weight and evenly dispersed, and serves as a mechanical dispersion point in the composite material, further improving the resilience and mechanical properties of the composite material.

[0108] 4. By comparing Examples 6-8 with Example 3, it can be found that the tensile strength, elongation at break and foaming performance of the composite materials prepared in Examples 6-8 are all improved, which shows that the silk fibroin in the present application has a better adhesion effect. After the silk fibroin is loaded on the hollow silica microspheres, it can further improve the bonding effect between silica and graphene, and can improve the bonding effect between silica and natural latex, and further improve the mechanical properties of the composite material. In addition, the silk fibroin can also be combined with the lactone-type sophorolipids, further promoting the bonding effect between silica and graphene, and can form a stable foam structure to improve the foaming effect of the composite material.

[0109] 5. By comparing Examples 11-12 with Example 3, it can be found that the tensile strength, elongation at break and foaming performance of the composite material prepared in Example 4 are all improved, which shows that the silk fibroin in the present application has the advantages of excellent biocompatibility, stable performance and wide sources. After being added to the composite material, a cross-linked network structure can be formed in the composite material, so that the composite material has relatively excellent resilience. In addition, the lactone-type sophorolipid in the modified graphene can be combined with the silk fibroin, which plays a role in stabilizing foam in the composite material, so that the composite material has a relatively excellent foaming effect.

[0110] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A high-performance graphene / natural latex composite material, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of natural latex; 10 parts of castor oil soap solution; 5-8 parts of filler; Potassium hydroxide 0.2-0.3 parts; Stabilizer 0.2-0.3 parts; 10-12 parts of vulcanizing agent; 1-2 parts of accelerator; 3-4 parts of potassium oleate; The filler includes graphene, and the graphene is casein-modified graphene.

2. A high performance graphene / natural latex composite material according to claim 1, characterized in that: The preparation of the graphene is as follows: casein, borax, ammonia water and deionized water are mixed to obtain a casein solution, graphene, casein solution, KOH, diffusion agent NF and water are mixed, dispersed at high speed, filtered, solid matter is retained, and dried to obtain modified graphene.

3. A high performance graphene / natural latex composite material according to claim 2, characterized in that: The graphene is prepared as follows: casein, borax, ammonia water and deionized water are mixed to obtain a casein solution, graphene, casein solution, lactone type sophora biosurfactant, KOH, diffusion agent NF and water are mixed, dispersed at high speed, filtered, solid matter is retained, and dried to obtain modified graphene.

4. The high performance graphene / natural latex composite material according to claim 1, characterized in that: The filler also includes hollow silica microspheres, and the hollow silica microspheres are micron-sized hollow silica microspheres.

5. A high performance graphene / natural latex composite material according to claim 4, characterized in that: The hollow silica microspheres are prepared as follows: micron-sized polystyrene microspheres and CTAB are added to an ethanol solution, ultrasonically dispersed to obtain a suspension, and then ammonia water is added for stirring; TEOS is added, and the reaction is continuously stirred, and the obtained suspension is placed in a centrifuge for ultracentrifugation, and the solid matter is retained, washed, dried, and heat-treated to obtain the hollow silica microspheres.

6. The high performance graphene / natural latex composite material according to claim 5, characterized in that: The hollow silica microspheres are mercapto-modified hollow silica microspheres.

7. The high performance graphene / natural latex composite material according to claim 5, characterized in that: The hollow silica microspheres are hollow silica microspheres loaded with silk fibroin.

8. A high performance graphene / natural latex composite material according to claim 6 or 7, characterized in that: The hollow silica microspheres are loaded with antibacterial particles, which are selected from silver or gold.

9. The high performance graphene / natural latex composite material according to claim 7, characterized in that: The filler also includes a protein filler, and the protein filler includes sericin, fibroin or collagen.

10. A method for preparing a high-performance graphene / natural latex composite material according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Prepare raw materials: weigh natural latex, castor oil soap solution, filler, vulcanizing agent, accelerator, potassium oleate, potassium hydroxide and stabilizer respectively according to weight parts; S2, raw material mixing: placing natural latex in a stirring device for stirring, adding castor oil soap solution, filler, vulcanizing agent, accelerator, potassium oleate, potassium hydroxide and stabilizer, continuing stirring and maturing to obtain a mixture; S3, foaming molding: keep the mixture warm, stir until foaming, pour into a mold, gel, vulcanize, demould and dry to obtain a composite material.

Citation Information

Patent Citations

  • Graphene modified natural emulsion preparation method and high barrier condom

    CN105542248A

  • Graphene-modified natural latex polymer and modification method thereof

    CN105906854A

  • Antibacterial and mildewproof latex foam material and preparation method thereof

    CN106543491A

  • Method for modifying vulcanization package for natural latex by graphene

    CN111978570A

  • Latex pillow containing graphene quantum dots and preparation method thereof

    CN112778583A

Cited By

  • Anti-aging natural rubber latex composite and preparation method thereof

    CN120289882B