High-strength high-barrier heat-resistant polylactic acid material and preparation method thereof
Through the refining and melting extrusion of a mixture of high molecular weight polylactic acid, modified mesh nanocellulose and PHBV, a high-strength, high-barrier, heat-resistant polylactic acid material is formed, which solves the problem of nano-polylactic acid composite materials taking into account strength, barrier properties and heat resistance. The problem of toughness achieves the efficient heat resistance and barrier properties of the material, avoids toxic hazards and annealing treatment, and is suitable for industrial production.
Patent Information
- Application Number
- CN202411117985.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing nanopolylactic acid composites are difficult to take into account strength, barrier properties, heat resistance and toughness, and nucleating agent strategies may cause residual toxic hazards.
The mixture of high molecular weight polylactic acid, modified mesh nanocellulose powder and PHBV is used for refining and melting and extruding to form high-strength, high-barrier, heat-resistant polylactic acid material, which is suppressed through a multi-interlocking network system and nanointerpenetrating network structure. The movement of polylactic acid chains promotes dense crystal structures and improves the heat resistance and barrier properties of the material.
It realizes high heat resistance, high barrier properties and high strength of polylactic acid materials, avoids traditional nucleating agents and annealing treatments, improves production efficiency and the overall mechanical properties of the material, and is suitable for industrial large-scale production.
Smart Images

Figure CN118895040A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of biodegradable polymer materials, and in particular to a high-strength, high-barrier, and heat-resistant polylactic acid material and a preparation method thereof. Background Art
[0002] Polylactic acid (PLA), a bioplastic synthesized from corn starch or biomass, has the advantages of high mechanical strength, good biocompatibility and good biodegradability. As a representative material for the development of the biodegradable materials industry, it has attracted much attention and has been widely used in packaging films, containers, textile fibers, medical stents, straws and tableware. However, pure PLA still has shortcomings such as brittle texture, poor toughness, low crystallinity, poor barrier properties and low heat resistance, which limit its practical application. The Vicat softening temperature of pure polylactic acid is only 50-60°C, and its barrier properties are far inferior to those of general plastics. Its heat-resistant defect limits its use in high-temperature occasions such as hot meals and drinks, microwave tableware, hot washing tableware, hot disinfection medical instruments, containers, and fabric ironing. Therefore, there is an urgent need to improve the heat resistance, strength and barrier properties of polylactic acid materials.
[0003] Nanocomposite material technology is a fast and convenient processing method to improve the comprehensive performance of polylactic acid. Bio-based nanomaterials such as nano starch and micro-nano cellulose are more promising because they are fully biodegradable. However, the studies reported on micro-nano cellulose modified polylactic acid composites are difficult to take into account the improvement of heat resistance, strength, barrier properties and toughness, and the nucleating agent strategy will also cause residual toxic hazards. Therefore, how to provide a nanocomposite material that has strength, barrier properties, heat resistance, toughness, and is fully biodegradable has become a problem that technicians in this field urgently need to solve. Summary of the invention
[0004] In view of this, the present invention provides a high-strength, high-barrier, heat-resistant polylactic acid material and a preparation method thereof, the purpose of which is to solve the technical problems existing in existing nano-polylactic acid composite materials such as difficulty in balancing strength, barrier properties, heat resistance and toughness.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a high-strength, high-barrier, and heat-resistant polylactic acid material, comprising the following steps:
[0007] S1, mixing high molecular weight polylactic acid, modified mesh nanocellulose powder and PHBV and kneading them to obtain a pre-dispersed mixture;
[0008] S2. The pre-dispersed mixture is melt-extruded, cooled and dried in sequence to obtain a high-strength, high-barrier and heat-resistant polylactic acid material.
[0009] Furthermore, in the step S1, the mass ratio of high molecular weight polylactic acid, modified mesh nanocellulose powder and PHBV is 70-85:1-5:15-30.
[0010] Furthermore, in step S1, the banburying temperature is 160-170° C., and the banburying time is 15-30 min.
[0011] Furthermore, in step S1, the average molecular weight of the high molecular weight polylactic acid is 80,000 to 100,000.
[0012] Furthermore, in step S1, the diameter of the modified mesh nanocellulose powder is ≤500 nm.
[0013] Furthermore, in the step S1, the high molecular weight polylactic acid, modified mesh nanocellulose powder and PHBV are dried before mixing; the drying temperature is 60 to 80° C., and the drying time is 4 to 12 hours.
[0014] Furthermore, in step S2, the temperature of melt extrusion is 170-190°C.
[0015] Furthermore, in step S2, the drying temperature is 60-80°C.
[0016] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:
[0017] 1. The present invention realizes a multi-interlocking network system by controlling the raw materials and their dosage to inhibit the movement of the polylactic acid molecular chain and its melt flow, and promotes the polylactic acid chain to fold into a dense crystalline structure. The dual mechanism gives the polylactic acid material excellent properties of high heat resistance, high barrier and high strength. Cotton-based mesh nanocellulose has a large specific surface area and can inhibit the free movement of the polylactic acid chain by forming a nano interpenetrating network with the polylactic acid molecular chain, replacing the traditional nucleating agent, achieving the effect of inducing rapid crystallization of polylactic acid and the overall mechanical enhancement of the material. In addition, it can increase the gas transmission path to improve the barrier property of the material.
[0018] 2. The modified cotton-based mesh nanocellulose has a hydrophobic surface, which improves the high-temperature melt processing performance of nanomaterials; at the same time, the modified performance improves the interface between the mesh nanocellulose particles and polylactic acid, achieves uniform distribution, and can transfer the rigidity of micro-nano cellulose to polylactic acid, thereby improving heat resistance, mechanical strength and oxygen / water vapor barrier properties.
[0019] 3. In general, industrial polylactic acid composite products must undergo a long annealing treatment of 6 to 24 hours, and can only increase the crystallinity to about 30 to 40%, with low production efficiency, and the heat resistance can often only reach about 100°C. The modified cotton-based mesh nanocellulose particles with a large specific surface area of the present invention act as a heterogeneous nucleating agent, which can induce rapid crystallization of polylactic acid, without the need for an annealing process step, to obtain highly heat-resistant polylactic acid, with high production efficiency and low energy consumption. The raw material formula and processing technology of the present invention are very suitable for industrial-scale production, replacing the role of traditional nucleating agents, cross-linking agents and annealing treatments to simply and quickly obtain perfect high crystallinity and heat resistance. The injection molding machine connected to the extruder end can be directly processed into degradable, high-barrier, high-toughness polylactic acid-based containers, films, fibers, brackets, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is the SEM image of the microstructure of modified cotton-based mesh nanocellulose;
[0021] Figure 2 This is a graph showing the mechanical tensile data of the high-strength, high-barrier, heat-resistant polylactic acid material prepared in Example 4;
[0022] Figure 3 The crystallization behaviors of pure polylactic acid and the high-strength, high-barrier, and heat-resistant polylactic acid material of Example 4 observed under a hot stage polarizing microscope, wherein A is pure polylactic acid and B is a high-strength, high-barrier, and heat-resistant polylactic acid material;
[0023] Figure 4 This is a diagram showing a sample of a medicine bottle that can be directly processed into a microwave-resistant and heat-resistant medicine bottle by connecting an injection molding machine to the extruder end in Example 4;
[0024] Figure 5 These are SEM images of the mechanical tensile fracture surfaces of the products, wherein Figure a is pure polylactic acid, Figure b is the polylactic acid material prepared in the comparative example, and Figure c is the high-strength, high-barrier, and heat-resistant polylactic acid material prepared in Example 3. DETAILED DESCRIPTION
[0025] The present invention provides a method for preparing a high-strength, high-barrier, and heat-resistant polylactic acid material, comprising the following steps:
[0026] S1, mixing high molecular weight polylactic acid, modified mesh nanocellulose powder and PHBV and kneading them to obtain a pre-dispersed mixture;
[0027] S2. The pre-dispersed mixture is melt-extruded, cooled and dried in sequence to obtain a high-strength, high-barrier and heat-resistant polylactic acid material.
[0028] In the present invention, in step S1, the mass ratio of high molecular weight polylactic acid, modified mesh nanocellulose powder and PHBV is 70-85:1-5:15-30, preferably 74-83:2-4:18-26, and more preferably 76-80:3:20-24.
[0029] In the present invention, in step S1, the banburying temperature is 160-170°C, preferably 162-168°C, and more preferably 164-166°C; the banburying time is 15-30 min, preferably 18-26 min, and more preferably 20-25 min.
[0030] In the present invention, in step S1, the average molecular weight of the high molecular weight polylactic acid is 80,000 to 100,000, preferably 90,000.
[0031] In the present invention, in step S1, the diameter of the modified mesh nanocellulose powder is ≤500nm, preferably ≤450nm, and more preferably ≤400nm; the modified mesh nanocellulose powder is preferably a modified cotton-based mesh nanocellulose powder, and the specific surface area is preferably 120m 2 / g, prepared according to reference (Industrial Crops & Products, 2023, 197, 116580.).
[0032] In the present invention, in the step S1, the high molecular weight polylactic acid, modified mesh nanocellulose powder and PHBV are dried before mixing; the drying temperature is 60 to 80°C, preferably 65 to 75°C, and more preferably 70°C; the drying time is 4 to 12 hours, preferably 6 to 10 hours, and more preferably 7 to 8 hours.
[0033] In the present invention, in the step S2, the temperature of melt extrusion is 170-190°C; a twin-screw extruder is preferably used for melt extrusion, and the aspect ratio of the twin-screw extruder is preferably 45, and the temperature of each zone is preferably: zone 1 170-180°C, zone 2 175-185°C, zone 3 180-190°C, zone 4 180-190°C, zone 5 180-190°C, zone 6 180-190°C, zone 7 180-190°C, and die head 180-190°C; the speed of the main engine is preferably 100-200rpm, and more preferably 150rpm.
[0034] In the present invention, the discharge end of the twin-screw extruder is connected to an injection molding machine, and the material can be directly processed into a high-strength, high-barrier, and heat-resistant polylactic acid material without the need for an annealing process. The high-strength, high-barrier, and heat-resistant polylactic acid material is a polylactic acid-based container, film, or fiber.
[0035] In the present invention, in step S2, the drying temperature is 60-80°C, preferably 65-75°C, and more preferably 70°C.
[0036] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0037] The modified mesh nanocellulose powders used in the following examples are all modified cotton-based mesh nanocellulose with a submicroscopic diameter of ≤500nm and a specific surface area of 120m 2 / g, prepared according to reference (Industrial Crops & Products, 2023, 197, 116580.), and its SEM microstructure is as follows Figure 1 As shown, its appearance is micrometer-scale and its interior is a rich nanofiber network.
[0038] Example 1
[0039] The preparation steps of a high-strength, high-barrier and heat-resistant polylactic acid material are as follows:
[0040] Weigh 700 grams of high molecular weight polylactic acid (average molecular weight of 90,000), 10 grams of modified cotton-based mesh nanocellulose powder and 300 grams of PHBV, place them in a 60°C oven and dry them for 4 hours; place all the dried raw materials in an internal mixer and mix them at 160°C for 30 minutes to obtain a pre-dispersed mixture.
[0041] The pre-dispersed mixture is added into a twin-screw extruder, extruded while being oriented while being melted, the extrudate is cooled, the pellets are collected, and dried at 60°C to obtain a high-strength, high-barrier, and heat-resistant polylactic acid material.
[0042] The length-to-diameter ratio of the twin-screw extruder is 45, and the heating program is: zone 1 170°C, zone 2 175°C, zone 3 180°C, zone 4 180°C, zone 5 180°C, zone 6 180°C, zone 7 180°C, and die head 190°C; the main engine speed is 150r / min.
[0043] The high-strength, high-barrier, heat-resistant polylactic acid material prepared in this embodiment has a heat-resistant deformation temperature of 148°C, a tensile strength of 58 MPa, an elongation at break of 50.7%, and an oxygen permeability of 15 cm 3 / (m 2 ·24h·0.1MPa), 23℃, 50%RH, water vapor transmission rate is 17g / (m 2 ·24h), 38°C, 100%RH.
[0044] Example 2
[0045] The preparation steps of a high-strength, high-barrier and heat-resistant polylactic acid material are as follows:
[0046] Weigh 700 grams of high molecular weight polylactic acid (average molecular weight of 90,000), 20 grams of modified cotton-based mesh nanocellulose powder and 300 grams of PHBV, place them in a 60°C oven and dry them for 12 hours; place all the dried raw materials in an internal mixer and mix them at 170°C for 20 minutes to obtain a pre-dispersed mixture.
[0047] The pre-dispersed mixture is added into a twin-screw extruder, extruded while being oriented while being melted, the extrudate is cooled, the pellets are collected, and dried at 60°C to obtain a high-strength, high-barrier, and heat-resistant polylactic acid material.
[0048] The length-to-diameter ratio of the twin-screw extruder is 45, and the temperature rising program is: zone 1 170°C, zone 2 175°C, zone 3 180°C, zone 4 180°C, zone 5 180°C, zone 6 180°C, zone 7 190°C, and die head 190°C; the main engine speed is 150r / min.
[0049] The high-strength, high-barrier, heat-resistant polylactic acid material prepared in this embodiment has a heat-resistant deformation temperature of 162°C, a tensile strength of 60 MPa, an elongation at break of 42%, and an oxygen permeability of 13 cm 3 / (m 2 ·24h·0.1Mpa), 23℃, 50%RH, water vapor transmission rate is 14g / (m 2 ·24h), 38°C, 100%RH.
[0050] Example 3
[0051] The preparation steps of a high-strength, high-barrier and heat-resistant polylactic acid material are as follows:
[0052] Weigh 800 grams of high molecular weight polylactic acid (average molecular weight of 90,000), 30 grams of modified cotton-based mesh nanocellulose powder and 220 grams of PHBV, place them in a 60°C oven and dry them for 8 hours; place all the dried raw materials in an internal mixer and mix them at 160°C for 30 minutes to obtain a pre-dispersed mixture.
[0053] The pre-dispersed mixture is added into a twin-screw extruder, extruded while being oriented while being melted, the extrudate is cooled, the pellets are collected, and dried at 60°C to obtain a high-strength, high-barrier, and heat-resistant polylactic acid material.
[0054] The length-to-diameter ratio of the twin-screw extruder is 45, and the temperature rising program is: zone 1 170°C, zone 2 175°C, zone 3 180°C, zone 4 180°C, zone 5 180°C, zone 6 180°C, zone 7 190°C, and die head 190°C; the main engine speed is 150r / min.
[0055] The high-strength, high-barrier, heat-resistant polylactic acid material prepared in this embodiment has a heat-resistant deformation temperature of 164°C, a tensile strength of 69 MPa, an elongation at break of 25%, and an oxygen permeability of 13 cm 3 / (m 2 ·24h·0.1MPa), 23℃, 50%RH, water vapor transmission rate is 14g / (m 2 ·24h), 38°C, 100%RH.
[0056] Example 4
[0057] The preparation steps of a high-strength, high-barrier and heat-resistant polylactic acid material are as follows:
[0058] Weigh 850 grams of high molecular weight polylactic acid (average molecular weight of 90,000), 40 grams of modified cotton-based mesh nanocellulose powder and 250 grams of PHBV, place them in a 60°C oven and dry them for 8 hours; place all the dried raw materials in an internal mixer and mix them at 160°C for 30 minutes to obtain a pre-dispersed mixture.
[0059] The pre-dispersed mixture is added into a twin-screw extruder, extruded while being oriented while being melted, the extrudate is cooled, the pellets are collected, and dried at 60°C to obtain a high-strength, high-barrier, and heat-resistant polylactic acid material.
[0060] The length-to-diameter ratio of the twin-screw extruder is 45, and the temperature rising program is: zone 1 170°C, zone 2 175°C, zone 3 180°C, zone 4 180°C, zone 5 180°C, zone 6 180°C, zone 7 190°C, and die head 190°C; the main engine speed is 150r / min.
[0061] The high-strength, high-barrier, heat-resistant polylactic acid material prepared in this embodiment has a heat-resistant deformation temperature of 164°C and an oxygen permeability of 13cm without annealing. 3 / (m 2 ·24h·0.1MPa), 23℃, 50%RH, water vapor transmission rate is 14g / (m 2 ·24h), 38°C, 100%RH.
[0062] Figure 2 This is a mechanical tensile data diagram of the high-strength, high-barrier, heat-resistant polylactic acid material prepared in this embodiment. Figure 2 It can be obtained that the tensile strength is between 59 and 63 MPa, and the elongation at break is between 45 and 50%.
[0063] Figure 3 The crystallization behavior of pure polylactic acid and the high-strength, high-barrier, and heat-resistant polylactic acid material of this embodiment observed under a hot stage polarizing microscope, wherein A is pure polylactic acid, B is a high-strength, high-barrier, and heat-resistant polylactic acid material. Figure 3It can be seen that pure PLA has large crystal size and slow crystallization, which is also one of the bottlenecks affecting PLA processing; while high-strength, high-barrier and heat-resistant PLA material has faster crystallization speed, smaller crystal size and larger crystal density, which will help provide more barrier paths and contribute to heat resistance.
[0064] The high-strength, high-barrier and heat-resistant polylactic acid material can be directly processed into microwave-resistant and heat-resistant medicine bottles by injection molding machines. The sample is shown in the following figure. Figure 4 shown.
[0065] Example 5
[0066] The preparation steps of a high-strength, high-barrier and heat-resistant polylactic acid material are as follows:
[0067] Weigh 700 grams of high molecular weight polylactic acid (average molecular weight of 90,000), 40 grams of modified cotton-based mesh nanocellulose powder and 300 grams of PHBV, place them in a 60°C oven and dry them for 8 hours; place all the dried raw materials in an internal mixer and mix them at 160°C for 30 minutes to obtain a pre-dispersed mixture.
[0068] The pre-dispersed mixture is added into a twin-screw extruder, extruded while being oriented while being melted, the extrudate is cooled, the pellets are collected, and dried at 60°C to obtain a high-strength, high-barrier, and heat-resistant polylactic acid material.
[0069] The length-to-diameter ratio of the twin-screw extruder is 45, and the temperature rising program is: zone 1 170°C, zone 2 175°C, zone 3 180°C, zone 4 180°C, zone 5 180°C, zone 6 180°C, zone 7 190°C, and die head 190°C; the main engine speed is 150r / min.
[0070] The high-strength, high-barrier, heat-resistant polylactic acid material prepared in this embodiment has a heat-resistant deformation temperature of 161°C, a tensile strength of 62 MPa, an elongation at break of 60%, and an oxygen permeability of 8 cm 3 / (m 2 ·24h·0.1MPa), 23℃, 50%RH, water vapor transmission rate is 16g / (m 2 ·24h), 38°C, 100%RH.
[0071] Comparative Example
[0072] The preparation steps of a polylactic acid material with only PHBV added are as follows:
[0073] Weigh 700 g of high molecular weight polylactic acid (average molecular weight of 90,000) and 300 g of PHBV, place them in a 60°C oven, and dry them for 8 hours; place all the dried raw materials in an internal mixer, and mix them at 160°C for 15 minutes to obtain a pre-dispersed mixture.
[0074] The pre-dispersed mixed material is added into a twin-screw extruder, and oriented and extruded while being melted. The extrudate is cooled, and the pellets are collected and dried at 60° C., thereby obtaining a polylactic acid material with only PHBV added.
[0075] The length-to-diameter ratio of the twin-screw extruder is 45, and the temperature rising program is: zone 1 170°C, zone 2 180°C, zone 3 180°C, zone 4 190°C, zone 5 190°C, zone 6 200°C, zone 7 190°C, die head 190°C; the main engine speed is 150r / min.
[0076] The polylactic acid material prepared in this comparative example with only PHBV added has a heat deformation temperature of 59°C, a tensile strength of 60 MPa, an elongation at break of 53%, and an oxygen permeability of 120 cm 3 / (m 2 ·24h·0.1MPa), 23℃, 50%RH, water vapor transmission rate is 45g / (m 2 ·24h), 38℃, 100%RH. Therefore, PHBV alone cannot achieve the benefits of improving heat resistance and barrier properties.
[0077] Figure 5 The SEM images of the mechanical tensile fracture surface of the product, wherein Figure a is pure polylactic acid, Figure b is the polylactic acid material prepared in the comparative example, and Figure c is the high-strength, high-barrier, and heat-resistant polylactic acid material prepared in Example 3. Figure 5 It can be seen that the mechanical tensile fracture surface of pure polylactic acid material is smooth, which is a typical brittle fracture feature; while the tensile fracture surface of the high-strength, high-barrier and heat-resistant polylactic acid material prepared by the present invention is an oriented fracture along the tensile direction, which is a typical ductile fracture feature.
[0078] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a high-strength, high-barrier, heat-resistant polylactic acid material, characterized in that: The following steps are involved: S1, mixing high molecular weight polylactic acid, modified mesh nanocellulose powder and PHBV and kneading them to obtain a pre-dispersed mixture; S2. The pre-dispersed mixture is melt-extruded, cooled and dried in sequence to obtain a high-strength, high-barrier and heat-resistant polylactic acid material.
2. The preparation method according to claim 1, characterized in that: In the step S1, the mass ratio of high molecular weight polylactic acid, modified mesh nanocellulose powder and PHBV is 70-85:1-5:15-30.
3. The preparation method according to claim 2, characterized in that: In the step S1, the banburying temperature is 160-170° C., and the banburying time is 15-30 min.
4. The preparation method according to any one of claims 1 to 3, characterized in that: In the step S1, the average molecular weight of the high molecular weight polylactic acid is 80,000 to 100,000.
5. The preparation method according to claim 4, characterized in that: In the step S1, the diameter of the modified mesh nanocellulose powder is ≤500 nm.
6. The preparation method according to claim 2, 3 or 5, characterized in that: In the step S1, the high molecular weight polylactic acid, modified mesh nanocellulose powder and PHBV are dried before mixing; the drying temperature is 60 to 80° C., and the drying time is 4 to 12 hours.
7. The preparation method according to claim 6, characterized in that: In the step S2, the temperature of the melt extrusion is 170-190°C.
8. The preparation method according to claim 7, characterized in that: In step S2, the drying temperature is 60-80°C.
Citation Information
Patent Citations
Food grade biodegradable polylactic acid-based composite material and application thereof
CN104072957A
Modified polylactic acid fiber and preparation method thereof
CN105220264A
Preparation method of polylactic acid / modified nanocellulose composite barrier material
CN108329490A
High-strength high-toughness polylactic acid material and preparation method thereof
CN111748181A
Full-biodegradable heat-resistant polylactic acid material and preparation method thereof
CN114957943A