Preparation method and application of nickel-based metal framework-graphite flake electrode material
Through the solvothermal preparation of nickel-based metal frame and graphite sheet composite material, the problems of poor conductivity and high cost of existing electrode materials are solved, and efficient and stable preparation of acid oxidation potential water is achieved, providing an economical solution.
Patent Information
- Application Number
- CN202410938835.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
AI Technical Summary
In the existing acid oxidation potential water preparation device, platinum titanium and ruthenium titanium electrodes have problems of surface cracks, poor binding force and high cost, and the conductivity of the metal organic framework is poor, which affects its application in the field of electrocatalytics.
The nickel-based metal frame and graphite sheet composite material is used to grow nickel-based metal frame in situ on the surface of graphite sheet by solvothermal method, and the graphite sheet is treated with acetone, ethanol, water ultrasonic treatment and nitric acid soaking to improve conductivity and stability. Combined with a carbon conductive substrate, a nickel-based metal frame-graphite sheet electrode material with high specific surface area and porosity was prepared.
It improves the conductivity and electrocatalytic activity of the nickel-based metal framework, reduces costs, enhances the stability and cyclic stability of the electrode, and provides a cost-effective and efficient preparation solution for acid oxidation potential water.
Smart Images

Figure CN118895526A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrocatalytic production, and in particular to a preparation method and application of a nickel-based metal skeleton-graphite sheet electrode material. Background Art
[0002] Acidic oxidizing potential water, as a new type of environmentally friendly bactericide with high safety, good bactericidal effect, no residue, no secondary pollution, and continuous production, has become a hot topic in the field of disinfection and sterilization research and has been widely used in medical and health care, food safety, and agricultural production. Acidic oxidizing potential water is a colorless and transparent liquid with a chlorine taste, and its main active ingredient is effective chlorine (Cl2, HClO, ClO-, etc.). In the preparation device of acidic oxidizing potential water, the electrolytic anode is the most important component for preparing acidic oxidizing potential water. Among them, the most commonly used are platinum titanium electrodes and ruthenium titanium electrodes, but these electrodes have many cracks on the coating surface, poor bonding with the titanium substrate, and coating shedding. Developing new electrodes with the advantages of high electrolysis efficiency, anti-oxidation corrosion, long service life, and low cost is the future development direction.
[0003] Metal organic framework (MOF) is a kind of framework material formed by metal atoms or ions and organic ligands bridged by organic chains. It has good crystallinity, structural controllability and pore size adjustability, and has good electrochemical metal active sites. Different from traditional porous materials, metal organic framework has a high specific surface area (more than 10000m 2 / g) and high porosity (free volume reaches 90%). Therefore, metal organic framework (MOF) materials are considered to be a promising electrochemical electrode material. Among them, nickel-based metal frameworks have become a hot topic of research due to their electrochemical reaction active sites, rich oxidation states and high density. For example, nickel chloride hexahydrate and trimesic acid were used as raw materials to prepare MOF materials in a mixed solvent of N,N-dimethylformamide (DMF) and deionized water with a volume ratio of 1:1. The MOF materials were coated on the surface of copper foam to make electrode materials. At a current density of 10 mA cm -2The lower overpotential is 287mV. The research results show that the rich oxidation state of the nickel-based metal skeleton and the framework structure of the metal skeleton are the key to its excellent electrocatalytic activity and stability. However, the conductivity of a single metal organic skeleton is poor compared with other traditional conductive materials, which greatly affects the application and development of metal organic frameworks in the field of electrocatalysis. In the process of research, it was found that combining the organic metal skeleton with a conductive substrate can not only improve the conductivity and stability but also obtain more electrocatalytic activity, thereby reducing the problem of weak conductivity of the metal organic skeleton. Carbon materials are the earliest and most mature electrode materials in industrialization. Compared with other conductive materials, carbon materials have a large specific surface area, a wide range of material sources and low cost. Its corrosion resistance in acidic environments is more prominent and has excellent stability. This reduces the use of precious metals in the preparation of acidic oxidation potential water devices to a certain extent, reduces costs, and is conducive to the development and application of the field of electrolysis of water. For example, a nickel-based MOF nanosheet / CNF composite material was prepared by one-step solvent thermal development using a carbon nanotube film (CNF) as the substrate. The composite of the carbon nanotube film improves the conductivity of the nickel-based metal skeleton and reduces the aggregation of MOF during the electrochemical process. The results show that the synthesized nickel-based MOF nanosheet / CNF composite material has a high conductivity at a current density of 10 mA / cm 2 It shows a low overpotential of 221mV at a current density of 10mA / cm 2 After 500 CV cycles, the potential increased by only 8mV, and the surface had excellent cycle stability. It can be seen that the composite carbon conductive material based on the synthesis of nickel-based metal skeletons not only improves the electrocatalytic activity, conductivity and stability of the material in the preparation of acidic oxidizing potential water anode catalyst materials, but also reduces the cost, making it more conducive to the preparation of acidic oxidizing potential water. Therefore, it is of practical significance to conduct in-depth research on the preparation of composite materials of nickel-based MOF materials and carbon conductive substrate materials. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the shortcomings of the prior art, the present invention provides a preparation method and application of a nickel-based metal skeleton-graphite sheet electrode material. The preparation process of the nickel-based metal skeleton-graphite sheet electrode described in the present invention is simple, easy to operate, and has strong repeatability. It provides a feasible solution for acidic oxidizing potential water and has a lower economic cost.
[0006] (II) Technical solution
[0007] To achieve the above objectives, the present invention is implemented by the following technical scheme: a method for preparing a nickel-based metal skeleton-graphite sheet electrode material, specifically comprising the following steps:
[0008] S1. Graphite sheet pretreatment: firstly, ultrasonically treat the graphite sheet with acetone, ethanol and water in sequence for 15 minutes, then soak the graphite sheet with nitric acid for 24 hours, then wash the graphite sheet with ultrapure water, and dry the washed graphite sheet in a vacuum drying oven at 80° C. for 12 hours to obtain a pretreated graphite sheet substrate;
[0009] S2. Prepare solution: Weigh a certain mass of nickel chloride hexahydrate NiCl2·6H2O and terephthalic acid, mix them in 35 mL of N,N-dimethylformamide, stir for 3 min to form a uniform solution, slowly add 2.5 mL of water and 2.5 mL of ethanol to the above solution and stir for 30 min to obtain the solution required for the reaction;
[0010] S3. Preparation of composite electrode material (Ni-MOF / GPH): The pretreated graphite sheet and the prepared solution were transferred to a 50 mL reactor and sealed. After being placed in an oven for solvothermal reaction, the obtained green electrode was washed several times with ultrapure water and ethanol respectively, and then dried in a vacuum drying oven at 60°C for 12 h to obtain a nickel-based metal skeleton-graphite sheet electrode material (Ni-MOF / GPH).
[0011] Preferably, the nitric acid in step S1 is concentrated nitric acid, and the size of the graphite sheet is 30 mm×15 mm×1 mm.
[0012] Preferably, the mass of nickel chloride hexahydrate NiCl2·6H2O weighed in step S2 is 0.2370 g, and the mass of terephthalic acid is 0.1660 g.
[0013] Preferably, in step S3, the temperature of the oven is 120° C., the reaction time is 12 h, and the temperature of the vacuum drying oven is 60° C., and the drying time is 12 h.
[0014] The present invention also provides an application of a nickel-based metal skeleton-graphite sheet electrode material in the preparation of oxidizing potential water, which specifically comprises the following steps:
[0015] T1. In a self-made electrolytic cell, a sodium chloride solution is used as an electrolyte, a nickel-based metal skeleton-graphite sheet electrode material is used as a working electrode, and a graphite sheet electrode is used as a counter electrode, and then electrolysis is performed to produce acidic oxidizing potential water;
[0016] T2. Use the iodine titration method to detect the content of available chlorine, i.e. ACC, in water.
[0017] Preferably, in step T1, the concentration of the electrolyzed sodium chloride solution is 0.5-5.0 g / L, the time is 20 min, and the electrolysis voltage is 16 V.
[0018] Preferably, the volume of the electrolytic cell in step T1 is 500 mL.
[0019] Preferably, the iodine titration method in step T2 specifically comprises the following steps:
[0020] E1. Take acidic electrolyzed water, add potassium iodide solution and sulfuric acid solution and place in the dark for reaction;
[0021] E2. Add distilled water and titrate with sodium thiosulfate standard solution until it is close to the end point and turns light yellow. Add starch indicator and the blue-purple solution turns into a colorless solution, which is the titration end point.
[0022] E3. Record the volume of sodium thiosulfate consumed and calculate the data according to the following formula:
[0023]
[0024] Where: C—concentration of total oxidizing substances, in terms of Cl2 (mg / L);
[0025] C 标 —Concentration of sodium thiosulfate standard solution (mol / L);
[0026] V2—the volume of sodium thiosulfate standard solution consumed by the water sample (ml);
[0027] V1—the volume of sodium thiosulfate standard solution consumed in the blank (ml);
[0028] V 水 —Volume of acidic oxidizing potential water (ml);
[0029] M—molar mass of chlorine (35453 mg / mol).
[0030] Preferably, in step E1, the concentration of the potassium iodide solution is 10%, the concentration of the sulfuric acid solution is 20%, and the dark reaction time is 10 minutes.
[0031] Preferably, in step E2, the starch indicator is 10 g / L, the sodium thiosulfate standard solution is 0.01 mol / L, the water sample is 10 ml, the potassium iodide solution is 10 ml, the sulfuric acid solution is 10 ml, and the distilled water is 20 ml.
[0032] (III) Beneficial effects
[0033] The present invention provides a preparation method and application of a nickel-based metal skeleton-graphite sheet electrode material. Compared with the prior art, it has the following beneficial effects:
[0034] (1) The preparation method and application of the nickel-based metal skeleton-graphite sheet electrode material. The prepared nickel-based metal skeleton-graphite sheet electrode uses a solvent-thermal method to grow the nickel-based metal skeleton in situ on the surface of the graphite sheet, so that the conductivity of the nickel-based metal skeleton is improved. The high activity, high specific surface area and large porosity of the in-situ grown nickel-based metal skeleton greatly increase the electrochemical activity of the composite electrode material. Compared with the electrodeposition method, the solvent-thermal method creates a relatively high temperature and high pressure environment by heating and pressurizing the reaction system during the synthesis process, so that the metal ions grow in situ on the conductive substrate with good dispersion, good crystal shape and controllable, and the synthesized composite electrode material has strong binding force.
[0035] (2) The preparation method and application of the nickel-based metal skeleton-graphite sheet electrode material. The prepared nickel-based metal skeleton-graphite sheet electrode is pretreated by ultrasonic treatment with acetone, ethanol, and water, and soaked in concentrated nitric acid to carboxylate the graphite sheet, so that the pore size and void distribution of the graphite sheet are uniform, thereby improving the bonding strength between the substrate and the nickel-based metal skeleton, thereby enhancing the stability of the electrode.
[0036] (3) The preparation method and application of the nickel-based metal skeleton-graphite sheet electrode material. Compared with precious metals, the material selected by the present invention has lower cost and better catalytic activity in the field of acidic oxidizing potential water production, and can achieve efficient preparation of acidic oxidizing potential water.
[0037] In summary, the preparation process of the nickel-based metal skeleton-graphite sheet electrode described in the present invention is simple, easy to operate, and highly repeatable, and provides a feasible solution for acidic oxidizing potential water with low economic cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 For the present invention Figure 1 (a) is the X-ray diffraction (XRD) diagram of the nickel-based metal skeleton-graphite sheet electrode monomer nickel-based metal skeleton (Ni-MOF) of the present invention, Figure (b) is the X-ray diffraction (XRD) diagram of the nickel-based metal skeleton-graphite sheet electrode synthesized in different proportions, and Figure (c) is the X-ray diffraction (XRD) diagram of Ni-MOF / GPH, Ni-MOF / CC, and Ni-MOF / CNF;
[0039] Figure 2 The scanning electron microscope (SEM) images of the graphite sheet before and after pretreatment and the synthesized nickel-based metal skeleton-graphite sheet of the present invention;
[0040] Figure 3 Graph showing the effective chlorine concentration of acidic oxidizing potential water produced by electrolysis of Example 1, Comparative Example 1 and Comparative Example 2 at different electrolyte concentrations of the present invention;
[0041] Figure 4Graphs showing pH values of acidic oxidizing potential water produced by electrolysis of Example 1, Comparative Example 1 and Comparative Example 2 at different electrolyte concentrations of the present invention. DETAILED DESCRIPTION
[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] See also Figure 1-4 The present invention provides nine technical solutions: a method for preparing a nickel-based metal skeleton-graphite sheet electrode material and its application, specifically including the following embodiments:
[0044] Example 1
[0045] This embodiment provides a method for preparing a nickel-based metal skeleton-graphite sheet electrode material, comprising the following steps:
[0046] (1) A 30 mm × 15 mm × 1 mm graphite sheet material was selected, and the graphite sheet was first ultrasonically treated with acetone, ethanol, and water in sequence for 15 min, then soaked in concentrated nitric acid at room temperature for 24 h, and then washed with ultrapure water. The washed graphite sheet was vacuum dried at 80 ° C for 12 h to obtain a pretreated graphite sheet.
[0047] (2) Weigh 0.2370 g of nickel chloride hexahydrate (NiCl2·6H2O) and 0.1660 g of terephthalic acid, mix in 35 mL of N,N-dimethylformamide (DMF), and stir for 3 min to form a uniform solution. Slowly add 2.5 mL of water and 2.5 mL of ethanol to the above solution and stir for 30 min to obtain the desired solution.
[0048] (3) The pretreated graphite sheet and the prepared solution were transferred to a 50 mL reactor and sealed. After being placed in a 120°C oven for solvothermal reaction for 12 hours, the obtained green electrode was washed several times with ultrapure water and ethanol, respectively, and then vacuum dried at 60°C for 12 hours to obtain the nickel-based metal skeleton-graphite sheet electrode material (Ni-MOF / GPH).
[0049] The nickel-based metal skeleton-graphite sheet electrode material (Ni-MOF / GPH) obtained in this example was subjected to X-ray diffraction and scanning electron microscopy analysis. The results are as follows: Figure 1 (b) and Figure 2 shown. Figure 1 (b) is the X-ray diffraction pattern of the nickel-based metal skeleton-graphite sheet electrode material in Example 1, Figure 2is a scanning electron microscope image of the nickel-based metal skeleton-graphite sheet electrode material in Example 1, Figure 1 and Figure 2 It can be seen that the pore distribution of the graphite sheet after pretreatment is more uniform, allowing the nickel-based metal skeleton to grow better on the graphite sheet substrate. At the same time, the in-situ grown nickel-based metal skeleton has a flaky structure and grows vertically on the graphite sheet. Figure 2 The SEM image in further illustrates that the nickel-based metal skeleton grows uniformly on the surface of the graphite sheet on a large scale, which increases the specific surface area of the composite electrode and improves the catalytic performance of the composite electrode. At the same time, it makes the nickel-based metal skeleton firmly bonded to the graphite sheet substrate, thereby extending the life of the electrode.
[0050] Example 2
[0051] A 30 mm × 15 mm × 1 mm graphite sheet was selected, and the graphite sheet was first ultrasonically treated with acetone, ethanol, and water in sequence for 15 min, then soaked in concentrated nitric acid at room temperature for 24 h, and then washed with ultrapure water. The washed graphite sheet was vacuum dried at 80 ° C for 12 h to obtain a pretreated graphite sheet.
[0052] Weigh 0.1185 g of nickel chloride hexahydrate (NiCl2·6H2O) and 0.0830 g of terephthalic acid, mix in 35 mL of N,N-dimethylformamide (DMF), and stir for 3 min to form a uniform solution. Slowly add 2.5 mL of water and 2.5 mL of ethanol to the above solution and stir for 30 min to obtain the desired solution.
[0053] The pretreated graphite sheet and the prepared solution were transferred to a 50 mL reactor and sealed. After being placed in a 120°C oven for solvothermal reaction for 12 hours, the obtained green electrode was washed several times with ultrapure water and ethanol, and then vacuum dried at 60°C for 12 hours to obtain the nickel-based metal skeleton-graphite sheet electrode material (Ni-MOF / GPH-50%).
[0054] Example 3
[0055] A 30 mm × 15 mm × 1 mm graphite sheet was selected, and the graphite sheet was first ultrasonically treated with acetone, ethanol, and water in sequence for 15 min, then soaked in concentrated nitric acid at room temperature for 24 h, and then washed with ultrapure water. The washed graphite sheet was vacuum dried at 80 ° C for 12 h to obtain a pretreated graphite sheet.
[0056] Weigh 0.4740 g of nickel chloride hexahydrate (NiCl2·6H2O) and 0.3320 g of terephthalic acid, mix in 35 mL of N,N-dimethylformamide (DMF), and stir for 3 min to form a uniform solution. Slowly add 2.5 mL of water and 2.5 mL of ethanol to the above solution and stir for 30 min to obtain the desired solution.
[0057] The pretreated graphite sheet and the prepared solution were transferred to a 50 mL reactor and sealed. After being placed in a 120°C oven for solvothermal reaction for 12 hours, the obtained green electrode was washed several times with ultrapure water and ethanol, and then vacuum dried at 60°C for 12 hours to obtain the nickel-based metal skeleton-graphite sheet electrode material (Ni-MOF / GPH-200%).
[0058] Example 4
[0059] This example is a nickel-based metal skeleton-graphite sheet electrode material used for the preparation of acidic oxidizing potential water
[0060] Use ultrapure water to prepare 1000mL of sodium chloride solution with a concentration of 0.5g / L, and place it in an intermittent diaphragm electrolyzer with a volume of 500mL. After 20 minutes of electrolysis, the effective chlorine concentration (ACC) of the acidic oxidizing potential water produced is 14.18mg / L, and the pH value is 3.15. Among them, the counter electrode is a 30mm×30mm×1mm graphite sheet electrode, and the working electrode is the nickel-based metal skeleton-graphite sheet electrode prepared in Example 1, which is fixed with an electrode clamp. The distance between the reference electrode and the counter electrode is 2cm. A constant potential voltage is applied using a DC regulated power supply (Chuanshutai Industrial Technology Co., Ltd., ST-1530), the voltage is set to 16V, and the electrolysis is continued. The effective chlorine concentration is determined by iodine titration. At the same time, the working electrode is replaced with Comparative Example 1 and Comparative Example 2 for experimental comparison. The results are shown in Table 1, Figure 3 and 4 shown.
[0061] Example 5
[0062] This example is a variation of Example 4. The technical solution is the same as that of Example 4, except that the concentration of the sodium chloride solution prepared in Example 4 is changed to 1.0 g / L, and the other steps are the same. The effective chlorine concentration (ACC) of the acidic oxidizing electrolyzed water produced by the prepared electrode is 14.18 mg / L, and the pH value is 3.15. At the same time, the working electrode is replaced with Comparative Example 1 and Comparative Example 2 for experimental comparison. The results are shown in Table 1, Figure 3 and 4 shown.
[0063] Example 6
[0064] This example is a variation of Example 4. The technical solution is the same as that of Example 4, except that the concentration of the sodium chloride solution prepared in Example 4 is changed to 1.5 g / L, and the other steps are the same. The effective chlorine concentration (ACC) of the acidic oxidizing electrolyzed water produced by the prepared electrode is 20.56 mg / L, and the pH value is 2.81. At the same time, the working electrode is replaced with Comparative Example 1 and Comparative Example 2 for experimental comparison. The results are shown in Table 1, Figure 3 and4 shown.
[0065] Example 7
[0066] This example is a variation of Example 4. The technical solution is the same as that of Example 4, except that the concentration of the sodium chloride solution prepared in Example 4 is changed to 2.0 g / L, and the other steps are the same. The effective chlorine concentration (ACC) of the acidic oxidative electrolyzed water produced by the prepared electrode is 24.82 mg / L, and the pH value is 2.79. At the same time, the working electrode is replaced with Comparative Example 1 and Comparative Example 2 for experimental comparison. The results are shown in Table 1, Figure 3 and 4 shown.
[0067] Example 8
[0068] This example is a variation of Example 4. The technical solution is the same as that of Example 4, except that the concentration of the sodium chloride solution prepared in Example 4 is changed to 3.0 g / L, and the other steps are the same. The effective chlorine concentration (ACC) of the acidic oxidizing electrolyzed water produced by the prepared electrode is 51.41 mg / L, and the pH value is 2.48. At the same time, the working electrode is replaced with Comparative Example 1 and Comparative Example 2 for experimental comparison. The results are shown in Table 1, Figure 3 and 4 shown.
[0069] Example 9
[0070] This example is a variation of Example 4. The technical solution is the same as that of Example 4, except that the concentration of the sodium chloride solution prepared in Example 4 is changed to 5.0 g / L, and the other steps are the same. The effective chlorine concentration (ACC) of the acidic oxidative electrolyzed water produced by the prepared electrode is 115.23 mg / L, and the pH value is 2.33. At the same time, the working electrode is replaced with Comparative Example 1 and Comparative Example 2 for experimental comparison. The results are shown in Table 1, Figure 3 and 4 shown.
[0071] Table 1. Effective chlorine concentration and pH value of acidic oxidizing potential water produced by electrolysis of nickel-based metal skeleton-graphite sheet electrode, nickel-based metal skeleton-carbon cloth electrode, and nickel-based metal skeleton-carbon nanofilm electrode at different electrolyte concentrations
[0072]
[0073]
[0074] It can be seen from Table 1 that the nickel-based metal skeleton-graphite sheet electrode has a good ability to produce acidic oxidizing potential water and an effective chlorine concentration of acidic oxidizing potential water under the condition of an electrolyte concentration of 3g / L to 5g / L. The nickel-based metal skeleton-graphite sheet electrode obtained in Example 1 of the present invention maintains very high activity and stability during the electrolysis process compared with the nickel-based metal skeleton-carbon cloth electrode and the nickel-based metal skeleton-carbon nanotube film electrode. This proves that the nickel-based metal skeleton-graphite sheet electrode can be stably produced in the preparation of acidic oxidizing potential water.
[0075] Comparative Example 1
[0076] In order to demonstrate the electrolytic performance of the nickel-based metal skeleton-graphite sheet electrode material, this embodiment prepared a nickel-based metal skeleton-carbon cloth electrode material with carbon cloth as the substrate: a 30mm×15mm×1mm carbon cloth material was selected, and the carbon cloth was first ultrasonically treated with acetone, ethanol, and water in sequence for 15 minutes, then soaked in concentrated nitric acid at room temperature for 24 hours, and then washed with ultrapure water. The washed carbon cloth was vacuum dried at 80°C for 12 hours to obtain a pretreated carbon cloth.
[0077] Weigh 0.2370g of nickel chloride hexahydrate (NiCl2·6H2O) and 0.1660g of terephthalic acid, mix in 35mL of N,N-dimethylformamide (DMF), and stir for 3min to form a uniform solution. Slowly add 2.5mL of water and 2.5mL of ethanol to the above solution and stir for 30min to obtain the desired solution. Transfer the pretreated carbon cloth and the prepared solution to a 50mL reactor and seal it. After solvothermal reaction in a 120℃ oven for 12h, the obtained green electrode was washed several times with ultrapure water and ethanol, respectively, and then vacuum dried at 60℃ for 12h to obtain the nickel-based metal skeleton-carbon cloth electrode material (Ni-MOF / CC).
[0078] The electrode material and the nickel-based metal skeleton-graphite sheet electrode material described in Example 1 were respectively used in the same intermittent diaphragm electrolyzer to electrolyze and produce acidic oxidizing potential water. The results are shown in Tables 1 and Figure 3 , Figure 4 As shown, it can be seen that when the electrolyte concentration is 3g / L~5g / L, the effective concentration of acidic oxidizing potential water produced by the electrolysis of nickel-based metal skeleton-graphite sheet electrode material is greater than that produced by the electrolysis of nickel-based metal organic framework-carbon cloth electrode material, indicating that the nickel-based metal skeleton-graphite sheet electrode material has better electrolysis efficiency.
[0079] Comparative Example 2
[0080] In order to demonstrate the electrolytic performance of the nickel-based metal skeleton-graphite sheet electrode material, this embodiment prepared a nickel-based metal skeleton-carbon cloth electrode material with a carbon nanotube film as the substrate: a 30mm×15mm×1mm carbon nanotube film material was selected, and the carbon nanotube film was first ultrasonically treated with acetone, ethanol, and water in sequence for 15 minutes, then soaked in concentrated nitric acid at room temperature for 24 hours, and then washed with ultrapure water. The washed carbon nanotube film was vacuum dried at 80°C for 12 hours to obtain a pretreated carbon nanotube film.
[0081] Weigh 0.2370g of nickel chloride hexahydrate (NiCl2·6H2O) and 0.1660g of terephthalic acid, mix in 35mL of N,N-dimethylformamide (DMF), and stir for 3min to form a uniform solution. Slowly add 2.5mL of water and 2.5mL of ethanol to the above solution and stir for 30min to obtain the desired solution. Transfer the pretreated carbon nanotube film and the prepared solution to a 50mL reactor and seal it. After being placed in a 120℃ oven for solvothermal reaction for 12h, the obtained green electrode was washed several times with ultrapure water and ethanol, respectively, and then vacuum dried at 60℃ for 12h to obtain the nickel-based metal skeleton-carbon nanotube film electrode material (Ni-MOF / CNF).
[0082] The electrode material and the nickel-based metal skeleton-graphite sheet electrode material described in Example 1 were respectively used in the same intermittent diaphragm electrolyzer to electrolyze and produce acidic oxidizing potential water. The results are shown in Tables 1 and Figure 3 , Figure 4 As shown, it can be seen that when the electrolyte concentration is 3g / L~5g / L, the effective concentration of acidic oxidizing potential water produced by the electrolysis of nickel-based metal skeleton-graphite sheet electrode material is greater than that produced by the electrolysis of nickel-based metal skeleton-carbon nanotube film electrode material, indicating that the nickel-based metal skeleton-graphite sheet electrode material has better electrolysis efficiency.
[0083] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.
[0084] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0085] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a nickel-based metal skeleton-graphite sheet electrode material, characterized in that: The specific steps include: S1. Graphite sheet pretreatment: firstly, ultrasonically treat the graphite sheet with acetone, ethanol and water in sequence for 15 minutes, then soak the graphite sheet with nitric acid for 24 hours, then wash the graphite sheet with ultrapure water, and dry the washed graphite sheet in a vacuum drying oven at 80° C. for 12 hours to obtain a pretreated graphite sheet substrate; S2. Prepare solution: Weigh a certain mass of nickel chloride hexahydrate NiCl2·6H2O and terephthalic acid, mix them in 35 mL of N,N-dimethylformamide, stir for 3 min to form a uniform solution, slowly add 2.5 mL of water and 2.5 mL of ethanol to the above solution and stir for 30 min to obtain the solution required for the reaction; S3. Preparation of composite electrode materials: The pretreated graphite sheet and the prepared solution were transferred to a 50 mL reactor and sealed. After being placed in an oven for solvothermal reaction, the obtained green electrode was washed several times with ultrapure water and ethanol respectively, and then dried in a vacuum drying oven at 60°C for 12 hours to obtain a nickel-based metal skeleton-graphite sheet electrode material.
2. The method for preparing a nickel-based metal skeleton-graphite sheet electrode material according to claim 1, characterized in that: In step S1, the nitric acid is concentrated nitric acid, and the size of the graphite sheet is 30 mm×15 mm×1 mm.
3. The method for preparing a nickel-based metal skeleton-graphite sheet electrode material according to claim 1, characterized in that: The mass of nickel chloride hexahydrate NiCl2·6H2O weighed in step S2 is 0.2370 g, and the mass of terephthalic acid is 0.1660 g.
4. The method for preparing a nickel-based metal skeleton-graphite sheet electrode material according to claim 1, characterized in that: In step S3, the temperature of the oven is 120° C., the reaction time is 12 h, and the temperature of the vacuum drying oven is 60° C., and the drying time is 12 h.
5. An application of a nickel-based metal skeleton-graphite sheet electrode material prepared by the method for preparing a nickel-based metal skeleton-graphite sheet electrode material according to any one of claims 1 to 4 in the preparation of oxidizing potential water, characterized in that: The specific steps include: T1. In a self-made electrolytic cell, a sodium chloride solution is used as an electrolyte, a nickel-based metal skeleton-graphite sheet electrode material is used as a working electrode, and a graphite sheet electrode is used as a counter electrode, and then electrolysis is performed to produce acidic oxidizing potential water; T2. Use the iodine titration method to detect the content of available chlorine, i.e. ACC, in water.
6. The use of a nickel-based metal skeleton-graphite sheet electrode material in the preparation of oxidizing potential water according to claim 5, characterized in that: In step T1, the concentration of the electrolyzed sodium chloride solution is 0.5-5.0 g / L, the time is 20 min, and the electrolysis voltage is 16 V.
7. The use of a nickel-based metal skeleton-graphite sheet electrode material in the preparation of oxidizing potential water according to claim 5, characterized in that: The volume of the electrolytic cell in step T1 is 500 mL.
8. The use of a nickel-based metal skeleton-graphite sheet electrode material in the preparation of oxidizing potential water according to claim 5, characterized in that: The iodine titration method in step T2 specifically comprises the following steps: E1. Take acidic electrolyzed water, add potassium iodide solution and sulfuric acid solution and place in the dark for reaction; E2. Add distilled water and titrate with sodium thiosulfate standard solution until it is close to the end point and turns light yellow. Add starch indicator and the blue-purple solution turns into a colorless solution, which is the titration end point. E3. Record the volume of sodium thiosulfate consumed and calculate the data according to the following formula: Where: C—concentration of total oxidizing substances, measured in Cl2; C 标 —Concentration of sodium thiosulfate standard solution; V2—the volume of sodium thiosulfate standard solution consumed by the water sample; V1—the volume of sodium thiosulfate standard solution consumed in the blank; V 水 —Volume of acidic oxidizing potential water; M—molar mass of chlorine.
9. The use of a nickel-based metal skeleton-graphite sheet electrode material in the preparation of oxidizing potential water according to claim 8, characterized in that: In step E1, the concentration of the potassium iodide solution is 10%, the concentration of the sulfuric acid solution is 20%, and the dark reaction time is 10 minutes.
10. The use of a nickel-based metal skeleton-graphite sheet electrode material in the preparation of oxidizing potential water according to claim 8, characterized in that: In step E2, the starch indicator is 10 g / L, the sodium thiosulfate standard solution is 0.01 mol / L, the water sample is 10 ml, the potassium iodide solution is 10 ml, the sulfuric acid solution is 10 ml, and the distilled water is 20 ml.