Quasi-solid polymer electrolyte and preparation method and application thereof
Patent Information
- Application Number
- CN202410929855.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-11
Smart Images

Figure CN118899525A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid-state sodium metal batteries, and in particular to a quasi-solid polymer electrolyte and a preparation method and application thereof. Background Art
[0002] Energy storage and conversion technologies play a key role in the energy transition process under the dual-carbon background, and their applications include electronic products, electric vehicles, and renewable energy storage. Currently, lithium-ion batteries dominate the rechargeable battery market. However, lithium ore reserves are limited and unevenly distributed in the earth's crust, making it economically unfeasible for lithium-ion batteries to be used at the gigawatt level (such as grid-connected fixed energy storage). From the perspective of physicochemical properties, sodium and lithium belong to the first main group elements and have similar properties. From the perspective of industrial demand, metallic sodium has abundant reserves, simple extraction technology, and low production costs. Therefore, sodium metal batteries with metallic sodium as the negative electrode are very likely to become a low-cost alternative to lithium metal batteries. Among them, sodium metal has a low electrochemical potential (-2.714V (relative to standard hydrogen electrode)) and a high theoretical specific energy (1,165mAh g -1 ), using sodium metal as the negative electrode can further increase the overall capacity of the battery.
[0003] However, due to the high reactivity of sodium metal, the rapid failure of the sodium metal anode is caused by severe dendrite growth, thick and fragile SE I layer formed by the reaction of electrolyte and sodium metal, and uncontrollable volume change. In addition, the use of highly active sodium metal and the formation of sodium dendrites during battery operation have caused safety issues, especially when using highly flammable liquid electrolytes. Summary of the invention
[0004] The purpose of the present invention is to provide a quasi-solid polymer electrolyte and a preparation method and application thereof in view of the defects existing in the prior art. The cross-linked network of the polymer in the quasi-solid polymer electrolyte can anchor the highly reactive solvent, preventing it from continuously reducing and decomposing on the surface of the metal negative electrode to form a thick and uneven SE I layer, which is beneficial to improve the reversibility of Na+ deposition / stripping, delay the rapid depletion of sodium ions at the negative electrode interface, and limit the development of the sodium deposition morphology towards the dendrite morphology, thereby achieving the stability of sodium metal in long-term circulation.
[0005] To achieve the above object, the present invention provides a quasi-solid polymer electrolyte, comprising: an electrolyte salt, an organic carbonate solvent, and a solid polymer electrolyte matrix;
[0006] Wherein, the solid polymer electrolyte matrix is formed by polymerization of polymer monomers and a cross-linking agent under the action of an initiator, and has a cross-linked network structure;
[0007] The organic carbonate solvent comprises a main solvent and a fluorine-based organic solvent; the organic carbonate solvent is in-situ encapsulated in the cross-linked network structure of the solid polymer electrolyte matrix.
[0008] Preferably, the electrolyte salt is a sodium salt, including one or more of NaPF6, NaClO4, NaFS I, NaTFS I, and sodium bis(oxalato)borate NaBOB;
[0009] The polymer monomers include: one or more of butyl acrylate, 2,2,3,4,4,4-hexafluorobutyl acrylate, and butyl methacrylate;
[0010] The cross-linking agent includes: one or more of polyethylene glycol diacrylate, triethylene glycol diacrylate, and ethylene glycol methyl ether acetate;
[0011] The initiator includes azobisisobutyronitrile.
[0012] Preferably, the organic carbonate solvent and the electrolyte salt are complexed together on the surface and / or inside of the solid polymer electrolyte matrix.
[0013] Preferably, the mass ratio of the electrolyte salt to the organic carbonate solvent is 13:100-4:25;
[0014] The volume percentage of the polymer monomer in the organic carbonate solvent is greater than 0 vol. % and less than or equal to 35 vol. %;
[0015] The volume percentage of the cross-linking agent in the polymer monomer is greater than 0 vol.% and less than or equal to 5 vol.%;
[0016] The mass ratio of the initiator to the polymer monomer is 0.1:100-1:20.
[0017] Preferably, the main solvent comprises: at least one of propylene carbonate, dimethyl carbonate, ethylene carbonate, and diethylene glycol dimethyl ether;
[0018] The fluorine-based organic solvent includes: fluoroethylene carbonate;
[0019] The volume ratio of the main solvent to the fluorine-based organic solvent is 8:1-10:1.
[0020] Preferably, the voltage window of the quasi-solid polymer-based electrolyte is 0-4.5V;
[0021] The sodium ion transference number of the quasi-solid polymer electrolyte is 0.3-0.9.
[0022] In a second aspect, an embodiment of the present invention provides a method for preparing the quasi-solid polymer electrolyte described in the first aspect, characterized in that the preparation method comprises:
[0023] The electrolyte salt and the organic carbonate solvent are mixed in proportion and stirred evenly to form an electrolyte salt solution; wherein the organic carbonate solvent comprises a main solvent and a fluorine-based organic solvent;
[0024] Adding a polymer monomer and a cross-linking agent to the electrolyte salt solution and stirring evenly, and then adding an initiator and stirring evenly to obtain an electrolyte precursor;
[0025] The electrolyte precursor is injected into the battery, packaged, and then solidified at a set temperature.
[0026] Preferably, the electrolyte salt is a sodium salt, including one or more of NaPF6, NaClO4, NaFS I, NaTFS I, and sodium bis(oxalato)borate NaBOB;
[0027] The polymer monomers include: one or more of butyl acrylate, 2,2,3,4,4,4-hexafluorobutyl acrylate, and butyl methacrylate;
[0028] The cross-linking agent includes: one or more of polyethylene glycol diacrylate, triethylene glycol diacrylate, and ethylene glycol methyl ether acetate;
[0029] The initiator includes azobisisobutyronitrile;
[0030] The main solvent includes: at least one of propylene carbonate, dimethyl carbonate, ethylene carbonate, and diethylene glycol dimethyl ether;
[0031] The fluorine-based organic solvent includes: fluoroethylene carbonate;
[0032] The volume ratio of the main solvent to the fluorine-based organic solvent is 8:1-10:1;
[0033] The mass ratio of the electrolyte salt to the organic carbonate solvent is 13:100-4:25;
[0034] The volume percentage of the polymer monomer in the organic carbonate solvent is greater than 0 vol. % and less than or equal to 35 vol. %;
[0035] The volume percentage of the cross-linking agent in the polymer monomer is greater than 0 vol.% and less than or equal to 5 vol.%;
[0036] The mass ratio of the initiator to the polymer monomer is 0.1:100-1:20;
[0037] The set temperature is 60°C-80°C.
[0038] In a third aspect, an embodiment of the present invention provides a sodium battery, comprising the quasi-solid polymer electrolyte described in the first aspect.
[0039] Preferably, the sodium battery further comprises a positive electrode and a negative electrode;
[0040] The positive electrode active material of the positive electrode includes: Na x A1[A2(CN)6] y ·H2O、Na n At least one of MO2, NaFePO4, Na2MP2O7, Na3V2(PO4)3, Na2M2(SO4)3, V2O5; the negative electrode is a metallic sodium negative electrode;
[0041] Among them, A1 and A2 are at least two of Mn, Fe, Co, Ni, Cu, and Zn, x=1-4, y=1-4, z=0-10; M is at least one of Co, Fe, Mn, and Ni, and n=1-2.
[0042] The quasi-solid polymer electrolyte provided by the embodiment of the present invention can anchor the highly reactive solvent through the cross-linked network of the polymer in the quasi-solid polymer electrolyte, thereby preventing the solvent from continuously reducing and decomposing on the surface of the metal negative electrode to form a thick and uneven SE I layer, which is beneficial to improving the Na + The reversibility of deposition / stripping delays the rapid depletion of sodium ions at the negative electrode interface, limits the development of the sodium deposition morphology towards the dendrite morphology, and thus achieves the stability of sodium metal in long-term circulation. In addition, the quasi-solid polymer electrolyte matrix formed by the added polymer monomer after polymerization can change the electrolyte / electrode double layer structure, derive a more stable solid electrolyte interface, effectively reduce the negative electrode corrosion phenomenon inside the metal battery, and further improve the electrochemical performance and cycle stability of the battery. In the quasi-solid polymer electrolyte of the present invention, the organic carbonate solvent is encapsulated in the cross-linked network structure of the polymer, thereby improving the safety performance of the battery assembled with the quasi-solid polymer electrolyte. By introducing an organic carbonate solvent containing a fluorinated group, the interfacial compatibility, rate, coulomb efficiency and cyclic charge and discharge performance of the battery are effectively improved. Therefore, the quasi-solid polymer electrolyte proposed in the present invention has high interfacial compatibility, can suppress the increase of impedance during the long cycle of the battery, can improve the voltage window and ion migration number of the battery, thereby improving the service life and safety performance of the battery assembled with the quasi-solid polymer electrolyte (such as a sodium metal battery) in the energy storage power station. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 are electrochemical impedance spectroscopy (EIS) curves of the quasi-solid polymer electrolyte of the present invention at different temperatures;
[0044] Figure 2 1 is a DC polarization curve of a Na||Na symmetric battery in Example 1, wherein the blue and purple curves in the figure correspond to the EIS curves before and after polarization, respectively;
[0045] Figure 3 This is a comparative example, the DC polarization curve of the Na||Na symmetric battery. The blue and purple curves in the figure correspond to the EIS curves before and after polarization, respectively.
[0046] Figure 4 The voltammetric curves of the electrochemical oxidation stability of Example 1 and the comparative example were tested by linear cyclic voltammetry.
[0047] Figure 5 The rate performance of Example 1 and the comparative example was tested using a fresh Na metal negative electrode;
[0048] Figure 6 A long-term cycling stability test was performed on Example 1 and the comparative example at a current density of 5C using a fresh Na metal anode.
[0049] Figure 7 In Example 1 and the comparative example, Na metal was -2 Long-term cycling performance of the Na||Na symmetric battery structure.
[0050] Figure 8 In Example 2 and Example 3, Na metal is at 0.1 mA cm -2 Long-term cycling performance of the Na||Na symmetric battery structure. DETAILED DESCRIPTION
[0051] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0052] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments.
[0053] The embodiment of the present invention provides a quasi-solid polymer electrolyte, which comprises: an electrolyte salt, an organic carbonate solvent, and a solid polymer electrolyte matrix;
[0054] Wherein, the solid polymer electrolyte matrix is formed by polymerization of polymer monomers and cross-linking agents under the action of an initiator, and has a cross-linked network structure;
[0055] The organic carbonate solvent and the electrolyte salt are complexed together on the surface and / or inside of the solid polymer electrolyte matrix.
[0056] The complexed electrolyte salt provides the ions required for conductivity to the quasi-solid polymer electrolyte, thereby further improving the ionic conductivity of the quasi-solid polymer electrolyte and reducing the battery interface resistance.
[0057] The organic carbonate solvent includes a main solvent and a fluorine-based organic solvent; the organic carbonate solvent is in situ encapsulated in a cross-linked network structure of a solid polymer electrolyte matrix. The present invention can effectively improve the interfacial compatibility, rate, coulombic efficiency and cycle charge and discharge performance of the battery by adding a fluorine-based organic solvent, such as fluoroethylene carbonate.
[0058] The quasi-solid polymer electrolyte can be prepared by the preparation method shown in the following step flow chart. The specific selection of various materials is described in the preparation method.
[0059] The preparation method of the quasi-solid polymer electrolyte proposed by the present invention comprises:
[0060] Step 110, mixing the electrolyte salt and the organic carbonate solvent in proportion and stirring them evenly to form an electrolyte salt solution;
[0061] The mass ratio of the electrolyte salt to the organic carbonate solvent is 13:100-4:25.
[0062] The electrolyte salt is a sodium salt, including one or more of NaPF6, NaClO4, NaFS I, NaTFS I, and sodium bis(oxalato)borate (NaBOB).
[0063] The organic carbonate solvent includes a main solvent and a fluorine-based organic solvent; the volume ratio of the main solvent to the fluorine-based organic solvent is 8:1-10:1, preferably 9:1. The main solvent includes at least one of propylene carbonate, dimethyl carbonate, ethylene carbonate, and diethylene glycol dimethyl ether; the fluorine-based organic solvent includes fluoroethylene carbonate.
[0064] Step 120, adding a polymer monomer and a cross-linking agent to an electrolyte salt solution and stirring the mixture evenly, and then adding an initiator and stirring the mixture evenly to obtain an electrolyte precursor;
[0065] The volume percentage of the added polymer monomer in the organic carbonate solvent is greater than 0 vol % and less than or equal to 35 vol %; the volume percentage of the added crosslinking agent in the polymer monomer is greater than 0 vol % and less than or equal to 5 vol %; and the mass ratio of the added initiator to the polymer monomer is 0.1:100-1:20.
[0066] The polymer monomers include: one or more of butyl acrylate, 2,2,3,4,4,4-hexafluorobutyl acrylate, and butyl methacrylate; the crosslinking agent includes: one or more of polyethylene glycol diacrylate, triethylene glycol diacrylate, and ethylene glycol methyl ether acetate; and the initiator includes azobisisobutyronitrile.
[0067] Step 130, injecting the electrolyte precursor into the battery, packaging it, and curing it at a set temperature.
[0068] Specifically, the electrolyte precursor is directly injected into the battery to wet the electrode and the separator well, and then the battery is packaged and then the polymerization is initiated by heating. The set temperature is a temperature that can initiate polymerization, preferably 60°C-80°C. The curing time is preferably 2 hours.
[0069] The pre-electrolyte precursor with good flowability before curing through thermally induced polymerization can achieve good contact with the electrode. After the electrolyte is cured, conformal interface contact is achieved, which can ensure uniform transmission of ions between the electrode and the electrolyte.
[0070] In the present invention, the quasi-solid polymer electrolyte matrix polymerized by the above-mentioned polymer monomers has high mechanical strength, and thus can effectively inhibit sodium dendrites from piercing the electrolyte. In the quasi-solid polymer electrolyte, the solid polymer electrolyte matrix acts as a skeleton, providing active sites for the electrolyte salt, thereby ensuring both mechanical strength and ion migration number.
[0071] The quasi-solid polymer electrolyte of the present invention can improve the low ionic conductivity and poor interface compatibility of solid polymer electrolytes; at the same time, the quasi-solid polymer electrolyte can also have good processability and electrochemical properties; more importantly, since the energy storage power station has a wide operating temperature range, the battery assembled with the quasi-solid polymer electrolyte of the present invention can be more safely applied to a wider temperature range than the battery assembled with the electrolyte.
[0072] The quasi-solid polymer electrolyte proposed in the present invention can be used in sodium batteries, such as sodium metal batteries. The sodium metal battery also includes a positive electrode and a negative electrode. The positive electrode active material of the positive electrode includes: Na x A1[A2(CN)6] y ·H2O、Na n At least one of MO2, NaFePO4, Na2MP2O7, Na3V2(PO4)3, Na2M2(SO4)3, V2O5; wherein A1 and A2 are at least two of Mn, Fe, Co, Ni, Cu, Zn, x=1-4, y=1-4, z=0-10; M is at least one of Co, Fe, Mn and Ni, n=1-2. The negative electrode is a metallic sodium negative electrode.
[0073] Since sodium ions have Lewis acidity and a large ionic radius, they exhibit weaker interactions with polar solvent molecules in liquid electrolytes and are easily affected by other polar dipoles. The introduction of polymer polar groups in the present invention can change the coordination environment of sodium ions, and the orderly ion migration on the surface of the sodium metal negative electrode leads to uniform sodium deposition / stripping. In addition, the cross-linked network of the polymer in the solid polymer electrolyte can anchor the highly reactive solvent, preventing it from continuously reducing and decomposing on the surface of the metal negative electrode to form a thick and uneven SE I layer, which is beneficial to improving the Na + The reversibility of deposition / stripping delays the rapid depletion of sodium ions at the negative electrode interface, limits the development of the sodium deposition morphology towards the dendrite morphology, and thus achieves the stability of sodium metal in long-term circulation. In addition, the quasi-solid polymer electrolyte matrix formed by the added polymer monomer after polymerization can change the electrolyte / electrode double electric layer structure, derive a more stable solid electrolyte interface, effectively reduce the negative electrode corrosion phenomenon inside the metal battery, and further improve the electrochemical performance and cycle stability of the battery. In the quasi-solid polymer electrolyte of the present invention, the organic carbonate solvent is encapsulated in the cross-linked network structure of the polymer, thereby improving the safety performance of the battery assembled with the quasi-solid polymer electrolyte. By introducing an organic carbonate solvent containing a fluorinated group, the interfacial compatibility, rate, coulomb efficiency and cyclic charge and discharge performance of the battery are effectively improved. The quasi-solid polymer electrolyte prepared by the in-situ curing method of the present invention can achieve perfect conformal contact with the electrode, effectively improve the interfacial compatibility, suppress the increase of impedance during the long cycle of the battery, and improve the voltage window and ion migration number of the battery, thereby improving the service life and safety performance of the battery assembled with the quasi-solid polymer electrolyte (such as a sodium metal battery) in the energy storage power station.
[0074] The voltage window of the quasi-solid polymer-based electrolyte of the present invention is 0-4.5V, and the sodium ion migration number of the quasi-solid polymer electrolyte is 0.3-0.9. In a specific example of the present invention, the conductivity of the quasi-solid polymer electrolyte is 3.06mS / cm, and the discharge specific capacity of the sodium metal battery using the quasi-solid polymer-based electrolyte of the present invention is 114mAh / g.
[0075] The technical solution of the present invention is further described in detail with several specific examples below. It should be understood that the embodiments of the present invention are only examples, and the scope of the present invention is not limited to the processes, values or components defined in the embodiments, because these embodiments are only for schematically illustrating the technical solution of the present invention. In fact, various changes that can be made to the embodiments of the present invention by those skilled in the art or related fields without paying creative work are all within the scope of the present invention.
[0076] Unless otherwise specified, the raw material components involved in the following examples are all commercially available products well known to those skilled in the art. The weight average molecular weight of butyl acrylate used in the following examples is 128.17.
[0077] Example 1
[0078] 1) Preparation of electrolyte precursor:
[0079] ① At room temperature, mix propylene carbonate and fluoroethylene carbonate in a volume ratio of 9:1 and take 300 μL;
[0080] ② Add 60.9 mg of sodium bis(fluorosulfonyl)imide (NaFS I) and stir at room temperature for 1 hour to prepare a sodium salt solution of bis(fluorosulfonyl)imide with a concentration of 1 mol / L;
[0081] ③ Add 100 μL of butyl acrylate monomer and 5 μL of polyethylene glycol diacrylate and stir at room temperature for 1 hour to prepare a uniform precursor solution;
[0082] ④ Add 3 mg of azobisisobutyronitrile and stir for 10 minutes to obtain the electrolyte precursor.
[0083] 2) Preparation of positive electrode sheet:
[0084] The positive electrode active material sodium vanadium phosphate (NVP), conductive carbon black and binder polyvinylidene fluoride (PVDF) are dispersed in N-methylpyrrolidone and stirred to obtain a uniform positive electrode slurry; wherein the solid component contains 80wt.% NVP, 1wt.% conductive carbon black, 1wt.% PVDF, and the viscosity is 9000mPa·S. The positive electrode slurry is evenly coated on the surface of the carbon-coated aluminum foil and baked in an oven at 80°C for 12h to obtain a positive electrode sheet.
[0085] 3) Preparation of negative electrode sheet:
[0086] The sodium metal block is taken out from the kerosene and wiped dry; the oxidized part of the sodium metal surface is cut off and then rolled; the sodium metal is rolled thin and then cut to obtain a negative electrode sheet with a diameter of 10 mm.
[0087] 4) Assembling the sodium metal battery:
[0088] Assemble button cells in the order of positive electrode sheet, glass fiber, and negative electrode sheet, and inject the electrolyte precursor into the battery; place the assembled battery in a 60°C oven for curing for 2 hours, so that the electrolyte precursor forms a quasi-solid polymer electrolyte after heating and curing, thereby obtaining a quasi-solid polymer-based electrolyte sodium metal battery.
[0089] Example 2
[0090] 1) Preparation of electrolyte precursor:
[0091] ① At room temperature, mix propylene carbonate and fluoroethylene carbonate in a volume ratio of 9:1 and take 300 μL;
[0092] ② Add 60.9 mg of sodium bis(fluorosulfonyl)imide and stir at room temperature for 1 hour to prepare a sodium salt solution of bis(fluorosulfonyl)imide with a concentration of 1 mol / L;
[0093] ③ Add 100 μL of 2,2,3,4,4,4-hexafluorobutyl acrylate monomer and 5 μL of polyethylene glycol diacrylate and stir at room temperature for 1 hour to prepare a uniform precursor solution;
[0094] ④ Add 3 mg of azobisisobutyronitrile and stir for 10 minutes to obtain the electrolyte precursor.
[0095] 2) Preparation of positive electrode sheet:
[0096] The positive electrode active material sodium vanadium phosphate (NVP), conductive carbon black and binder polyvinylidene fluoride (PVDF) are dispersed in N-methylpyrrolidone and stirred to obtain a uniform positive electrode slurry; wherein the solid component contains 80wt.% NVP, 1wt.% conductive carbon black, 1wt.% PVDF, and the viscosity is 9000mPa·S. The positive electrode slurry is evenly coated on the surface of the carbon-coated aluminum foil and baked in an oven at 80°C for 12h to obtain a positive electrode sheet.
[0097] 3) Preparation of negative electrode sheet:
[0098] The sodium metal block is taken out from the kerosene and wiped dry; the oxidized part of the sodium metal surface is cut off and then rolled; the sodium metal is rolled thin and then cut to obtain a negative electrode sheet with a diameter of 10 mm.
[0099] 4) Assembling the sodium metal battery:
[0100] Assemble button cells in the order of positive electrode sheet, glass fiber, and negative electrode sheet, and inject the electrolyte precursor into the battery; place the assembled battery in a 60°C oven for curing for 2 hours, so that the electrolyte precursor forms a quasi-solid polymer electrolyte after heating and curing, thereby obtaining a quasi-solid polymer-based electrolyte sodium metal battery.
[0101] Example 3
[0102] 1) Preparation of electrolyte precursor:
[0103] ① At room temperature, mix propylene carbonate and fluoroethylene carbonate in a volume ratio of 9:1 and take 300 μL;
[0104] ② Add 60.9 mg of sodium bis(fluorosulfonyl)imide and stir at room temperature for 1 hour to prepare a sodium salt solution of bis(fluorosulfonyl)imide with a concentration of 1 mol / L;
[0105] ③ Add 100 μL of butyl methacrylate monomer and 5 μL of polyethylene glycol diacrylate and stir at room temperature for 1 hour to prepare a uniform precursor solution;
[0106] ④ Add 3 mg of azobisisobutyronitrile and stir for 10 minutes to obtain the electrolyte precursor.
[0107] 2) Preparation of positive electrode sheet:
[0108] The positive electrode active material sodium vanadium phosphate (NVP), conductive carbon black and binder polyvinylidene fluoride (PVDF) are dispersed in N-methylpyrrolidone and stirred to obtain a uniform positive electrode slurry; wherein the solid component contains 80wt.% NVP, 1wt.% conductive carbon black, 1wt.% PVDF, and the viscosity is 9000mPa·S. The positive electrode slurry is evenly coated on the surface of the carbon-coated aluminum foil and baked in an oven at 80°C for 12h to obtain a positive electrode sheet.
[0109] 3) Preparation of negative electrode sheet:
[0110] The sodium metal block is taken out from the kerosene and wiped dry; the oxidized part of the sodium metal surface is cut off and then rolled; the sodium metal is rolled thin and then cut to obtain a negative electrode sheet with a diameter of 10 mm.
[0111] 4) Assembling the sodium metal battery:
[0112] Assemble button cells in the order of positive electrode sheet, glass fiber, and negative electrode sheet, and inject the electrolyte precursor into the battery; place the assembled battery in a 60°C oven for curing for 2 hours, so that the electrolyte precursor forms a quasi-solid polymer electrolyte after heating and curing, thereby obtaining a quasi-solid polymer-based electrolyte sodium metal battery.
[0113] Example 4
[0114] 1) Preparation of electrolyte precursor:
[0115] ① At room temperature, mix propylene carbonate and fluoroethylene carbonate in a volume ratio of 9:1 and take 300 μL;
[0116] ② Add 91.2 mg of sodium bis(trifluoromethylsulfonyl)imide (NaTFS I) and stir at room temperature for 1 hour to prepare a sodium salt solution of bis(trifluoromethylsulfonyl)imide with a concentration of 1 mol / L;
[0117] ③ Add 100 μL of butyl acrylate monomer and 5 μL of polyethylene glycol diacrylate and stir at room temperature for 1 hour to prepare a uniform precursor solution;
[0118] ④ Add 3 mg of azobisisobutyronitrile and stir for 10 minutes to obtain the electrolyte precursor.
[0119] 2) Preparation of positive electrode sheet:
[0120] The positive electrode active material sodium vanadium phosphate (NVP), conductive carbon black and binder polyvinylidene fluoride (PVDF) are dispersed in N-methylpyrrolidone and stirred to obtain a uniform positive electrode slurry; wherein the solid component contains 80wt.% NVP, 1wt.% conductive carbon black, 1wt.% PVDF, and the viscosity is 9000mPa·S. The positive electrode slurry is evenly coated on the surface of the carbon-coated aluminum foil and baked in an oven at 80°C for 12h to obtain a positive electrode sheet.
[0121] 3) Preparation of negative electrode sheet:
[0122] The sodium metal block is taken out from the kerosene and wiped dry; the oxidized part of the sodium metal surface is cut off and then rolled; the sodium metal is rolled thin and then cut to obtain a negative electrode sheet with a diameter of 10 mm.
[0123] 4) Assembling the sodium metal battery:
[0124] Assemble button cells in the order of positive electrode sheet, glass fiber, and negative electrode sheet, and inject the electrolyte precursor into the battery; place the assembled battery in a 60°C oven for curing for 2 hours, so that the electrolyte precursor forms a quasi-solid polymer electrolyte after heating and curing, thereby obtaining a quasi-solid polymer-based electrolyte sodium metal battery.
[0125] Example 5
[0126] 1) Preparation of electrolyte precursor:
[0127] ① At room temperature, mix propylene carbonate and fluoroethylene carbonate in a volume ratio of 9:1 and take 300 μL;
[0128] ② Add 50.4 mg of sodium hexafluorophosphate (NaPF6) and stir at room temperature for 1 hour to prepare a sodium hexafluorophosphate solution with a concentration of 1 mol / L;
[0129] ③ Add 100 μL of butyl acrylate monomer and 5 μL of polyethylene glycol diacrylate and stir at room temperature for 1 hour to prepare a uniform precursor solution;
[0130] ④ Add 3 mg of azobisisobutyronitrile and stir for 10 minutes to obtain the electrolyte precursor.
[0131] 2) Preparation of positive electrode sheet:
[0132] The positive electrode active material sodium vanadium phosphate (NVP), conductive carbon black and binder polyvinylidene fluoride (PVDF) are dispersed in N-methylpyrrolidone and stirred to obtain a uniform positive electrode slurry; wherein the solid component contains 80wt.% NVP, 1wt.% conductive carbon black, 1wt.% PVDF, and the viscosity is 9000mPa·S. The positive electrode slurry is evenly coated on the surface of the carbon-coated aluminum foil and baked in an oven at 80°C for 12h to obtain a positive electrode sheet.
[0133] 3) Preparation of negative electrode sheet:
[0134] The sodium metal block is taken out from the kerosene and wiped dry; the oxidized part of the sodium metal surface is cut off and then rolled; the sodium metal is rolled thin and then cut to obtain a negative electrode sheet with a diameter of 10 mm.
[0135] 4) Assembling the sodium metal battery:
[0136] Assemble button cells in the order of positive electrode sheet, glass fiber, and negative electrode sheet, and inject the electrolyte precursor into the battery; place the assembled battery in a 60°C oven for curing for 2 hours, so that the electrolyte precursor forms a quasi-solid polymer electrolyte after heating and curing, thereby obtaining a quasi-solid polymer-based electrolyte sodium metal battery.
[0137] Comparative Example
[0138] 1) Preparation of electrolyte:
[0139] ① At room temperature, mix propylene carbonate and fluoroethylene carbonate in a volume ratio of 9:1 and take 300 μL;
[0140] ② Add 60.9 mg of sodium bis(fluorosulfonyl)imide and stir at room temperature for 1 hour to prepare a sodium bis(fluorosulfonyl)imide salt solution with a concentration of 1 mol / L as an electrolyte precursor.
[0141] 2) Preparation of positive electrode sheet:
[0142] The positive electrode active material sodium vanadium phosphate (NVP), conductive carbon black and binder polyvinylidene fluoride (PVDF) are dispersed in N-methylpyrrolidone and stirred to obtain a uniform positive electrode slurry; wherein the solid component contains 80wt.% NVP, 1wt.% conductive carbon black, 1wt.% PVDF, and the viscosity is 9000mPa·S. The positive electrode slurry is evenly coated on the surface of the carbon-coated aluminum foil and baked in an oven at 80°C for 12h to obtain a positive electrode sheet.
[0143] 3) Preparation of negative electrode sheet:
[0144] The sodium metal block is taken out from the kerosene and wiped dry; the oxidized part of the sodium metal surface is cut off and then rolled; the sodium metal is rolled thin and then cut to obtain a negative electrode sheet with a diameter of 10 mm.
[0145] 4) Assembling the sodium metal battery:
[0146] Assemble the button battery in the order of positive electrode sheet, glass fiber, and negative electrode sheet, and inject the electrolyte into the battery to obtain a sodium metal battery.
[0147] The above-mentioned embodiments and comparative examples were tested and analyzed.
[0148] 1. Electrochemical impedance spectroscopy test and ionic conductivity test:
[0149] Electrochemical Impedance Spectroscopy (EIS) tests apply a small amplitude AC potential wave with different frequencies to the electrochemical system. As the frequency of the sine wave changes, the impedance ratio of the measured AC potential to the current signal also changes. The test was performed using a Gamry electrochemical workstation with a test frequency range of 10 -2 Hz to 10 5 Hz, the test temperature is between 0℃ and 60℃, and the EIS curves at different temperatures are obtained, such as Figure 1 .
[0150] Ionic conductivity test Example 1 was tested by a blocking cell with both electrodes made of stainless steel (SS). The ionic conductivity (σ) was calculated according to the following formula: σ = L / R ь A; where σ(S cm -1 ) is the ionic conductivity, L (cm) is the thickness of the electrolyte between the two electrodes, A (cm -2 ) is the effective contact area between the electrolyte and the electrode, R b (Ω) is the bulk resistance, and the conductivity of the quasi-solid polymer electrolyte of Example 1 is 3.06 mS / cm.
[0151] 2. Ion migration number test:
[0152] Chronoamperometry is to apply a single potential step or a double potential step to the working electrode of the electrochemical system and measure the functional relationship between the current response and time. The present invention uses the Bruce & Vincent method to measure the electrochemical impedance spectroscopy and combines it with the chronoamperometry to measure the sodium ion migration number (t Na+ ). In order to calculate the t Na+ A Na / quasi-solid polymer electrolyte / Na battery was assembled using two sodium metal electrodes (Na) and the quasi-solid polymer electrolyte prepared in Example 1. Na+ The value of is calculated by the following formula:
[0153] t Na+ =I s *R b s (ΔV-I o *R i o ) / I o *R b 0 (ΔV-I s *R i s )
[0154] Where ΔV (mV) is the applied polarization voltage, I o ,I s (mA) are the initial current and steady-state current in the polarization process, R b 0 ,R b s (Ω) are the initial and steady-state bulk resistances, R i o ,R i s (Ω) are the initial and steady-state interfacial resistances, respectively.
[0155] Figure 2 This is the DC polarization curve of the Na||Na symmetric battery in Example 1. The blue and purple curves in the figure correspond to the EIS curves before and after polarization, respectively.
[0156] Figure 3 This is a comparative example, the DC polarization curve of the Na||Na symmetric battery. The blue and purple curves in the figure correspond to the EIS curves before and after polarization, respectively.
[0157] It can be seen that the butyl acrylate polymer-based electrolyte has a higher ion migration number while ensuring the interfacial compatibility between the solid polymer electrolyte and the positive and negative electrodes.
[0158] 3. Electrochemical stability window:
[0159] The electrochemical stability window of the quasi-solid polymer electrolyte was determined by linear sweep voltammetry. The electrochemical stability window of the quasi-solid polymer electrolyte adopts a three-electrode system (Na / quasi-solid polymer electrolyte / SS), with SS as the working electrode and Na as both the counter electrode and the reference electrode. The measurement range is 2.5~8V (vs.Na + / Na), the scan rate is 1mVs -1 The Example 1 and the comparative example were tested respectively, and the test results are as follows: Figure 4As shown, it can be seen that the discharge voltage window of the quasi-solid polymer electrolyte of Example 1 can reach 4.5 V. This indicates that the voltage window of the quasi-solid polymer electrolyte is widened by adding butyl acrylate. A high discharge voltage window is beneficial to improving the energy density of the battery cell and also means smaller polarization.
[0160] 4. Constant current charge and discharge test:
[0161] The charge and discharge tests of the battery assembled with the quasi-solid polymer electrolyte of Example 1 and the comparative example were carried out in a constant temperature box with the temperature set at 30°C. Five cycles were performed at current densities of 0.1C, 0.2C, 1C, 5C, 10C, 15C and 20C. For each cycle, charging was performed for 2h and then discharging for 2h. The test results are shown in FIG. Figure 5 As shown, it can be seen that the cycle stability of Example 1 is better than that of the comparative example.
[0162] The long-term cycle stability test of the batteries of Example 1 and the comparative example was carried out at a current density of 5C using Wuhan Blue Electric Battery Test System (CT3001A / 2001A). The charge and discharge tests were carried out in a constant temperature box with the temperature set at 30°C and a constant current density (0.1 mA cm -2 ) is charged for 2 hours, then discharged for 2 hours, and the cycle is repeated. The test results are as follows Figure 6 According to the change of the voltage curve during the cycle, it can be judged that the stability and cycle life of the battery of Example 1 of the present invention are significantly better than those of the comparative example.
[0163] Figure 7 The quasi-solid polymer electrolyte of Example 1 and the comparative example is -2 The long-term cycle performance of the Na||Na symmetric battery structure. It can be seen that the long-term cycle performance of Example 1 is significantly better than that of the comparative example.
[0164] Figure 8 The quasi-solid polymer electrolytes of Examples 2 and 3 are -2 The long-term cycle performance of the Na||Na symmetric battery structure. It can be seen that the polymers obtained using 2,2,3,4,4,4-hexafluorobutyl acrylate monomers and butyl methacrylate monomers can have relatively good long-term cycle performance.
[0165] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A quasi-solid polymer electrolyte, characterized in that: The quasi-solid polymer electrolyte comprises: an electrolyte salt, an organic carbonate solvent, and a solid polymer electrolyte matrix; Wherein, the solid polymer electrolyte matrix is formed by polymerization of polymer monomers and a cross-linking agent under the action of an initiator, and has a cross-linked network structure; The organic carbonate solvent comprises a main solvent and a fluorine-based organic solvent; the organic carbonate solvent is in-situ encapsulated in the cross-linked network structure of the solid polymer electrolyte matrix.
2. The quasi-solid polymer electrolyte according to claim 1, characterized in that The electrolyte salt is a sodium salt, including one or more of NaPF6, NaClO4, NaFSI, NaTFSI, and sodium bis(oxalate)borate NaBOB; The polymer monomers include: one or more of butyl acrylate, 2,2,3,4,4,4-hexafluorobutyl acrylate, and butyl methacrylate; The cross-linking agent includes: one or more of polyethylene glycol diacrylate, triethylene glycol diacrylate, and ethylene glycol methyl ether acetate; The initiator includes azobisisobutyronitrile.
3. The quasi-solid polymer electrolyte according to claim 1, characterized in that The organic carbonate solvent and the electrolyte salt are complexed together on the surface and / or inside of the solid polymer electrolyte matrix.
4. The quasi-solid polymer electrolyte according to claim 1, characterized in that The mass ratio of the electrolyte salt to the organic carbonate solvent is 13:100-4:25; The volume percentage of the polymer monomer in the organic carbonate solvent is greater than 0 vol.% and less than or equal to 35 vol.%; The volume percentage of the cross-linking agent in the polymer monomer is greater than 0 vol.% and less than or equal to 5 vol.%; The mass ratio of the initiator to the polymer monomer is 0.1:100-1:
20.
5. The quasi-solid polymer electrolyte according to claim 1, characterized in that The main solvent includes: at least one of propylene carbonate, dimethyl carbonate, ethylene carbonate, and diethylene glycol dimethyl ether; The fluorine-based organic solvent includes: fluoroethylene carbonate; The volume ratio of the main solvent to the fluorine-based organic solvent is 8:1-10:
1.
6. The quasi-solid polymer electrolyte according to claim 1, characterized in that The voltage window of the quasi-solid polymer-based electrolyte is 0-4.5V; The sodium ion transference number of the quasi-solid polymer electrolyte is 0.3-0.
9.
7. A method for preparing the quasi-solid polymer electrolyte according to any one of claims 1 to 6, characterized in that: The preparation method comprises: The electrolyte salt and the organic carbonate solvent are mixed in proportion and stirred evenly to form an electrolyte salt solution; wherein the organic carbonate solvent comprises a main solvent and a fluorine-based organic solvent; Adding a polymer monomer and a cross-linking agent to the electrolyte salt solution and stirring evenly, and then adding an initiator and stirring evenly to obtain an electrolyte precursor; The electrolyte precursor is injected into the battery, packaged, and then solidified at a set temperature.
8. The preparation method according to claim 7, characterized in that: The electrolyte salt is a sodium salt, including one or more of NaPF6, NaClO4, NaFS I, NaTFS I, and sodium bis(oxalate)borate NaBOB; The polymer monomers include: one or more of butyl acrylate, 2,2,3,4,4,4-hexafluorobutyl acrylate, and butyl methacrylate; The cross-linking agent includes: one or more of polyethylene glycol diacrylate, triethylene glycol diacrylate, and ethylene glycol methyl ether acetate; The initiator includes azobisisobutyronitrile; The main solvent includes: at least one of propylene carbonate, dimethyl carbonate, ethylene carbonate, and diethylene glycol dimethyl ether; The fluorine-based organic solvent includes: fluoroethylene carbonate; The volume ratio of the main solvent to the fluorine-based organic solvent is 8:1-10:1; The mass ratio of the electrolyte salt to the organic carbonate solvent is 13:100-4:25; The volume percentage of the polymer monomer in the organic carbonate solvent is greater than 0 vol.% and less than or equal to 35 vol.%; The volume percentage of the cross-linking agent in the polymer monomer is greater than 0 vol.% and less than or equal to 5 vol.%; The mass ratio of the initiator to the polymer monomer is 0.1:100-1:20; The set temperature is 60°C-80°C.
9. A sodium battery, characterized in that: The sodium battery comprises the quasi-solid polymer electrolyte described in any one of claims 1 to 6 above.
10. The sodium battery according to claim 9, characterized in that: The sodium battery also includes: a positive electrode and a negative electrode; The positive electrode active material of the positive electrode includes: Na x A1[A2(CN)6] y ·H2O、Na n At least one of MO2, NaFePO4, Na2MP2O7, Na3V2(PO4)3, Na2M2(SO4)3, V2O5; the negative electrode is a metallic sodium negative electrode; Among them, A1 and A2 are at least two of Mn, Fe, Co, Ni, Cu, and Zn, x=1-4, y=1-4, z=0-10; M is at least one of Co, Fe, Mn, and Ni, and n=1-2.
Citation Information
Patent Citations
Application of multifunctional organogel to lithium ion battery
CN110071324A
Multifunctional organogel, and preparation method thereof
CN110105502A
Application of multifunctional organogel in sensor
CN110108392A
Application of multifunctional organic gel as conductive medium
CN110111922A
Preparation method and application of sodium-based PEG / PMA composite polymer electrolyte
CN110137569A
Cited By
Full-temperature-range polymer-based solid electrolyte, solid-state battery and preparation method
CN119490607A
Full-temperature-range polymer-based solid electrolyte, solid-state battery and preparation method
WO2026102880A1